Preparation process of high-selectivity molecular sieve
By using specific raw materials and processing methods in the preparation process, highly selective molecular sieves are formed, which solves the problem of insufficient selective adsorption of existing molecular sieves and realizes high selectivity and durability of molecular sieves.
Patent Information
- Application Number
- CN202411120078.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-15
- Publication Date
- 2024-11-26
AI Technical Summary
Existing molecular sieves have limitations in selectively adsorbing molecules based on their size, shape, polarity, and other characteristics.
The preparation process uses raw materials such as flower clay scraps, walnut shell powder, dried apple pomace, tourmaline powder, and trehalose powder, and adds preservatives, wear-resistant agents, and temperature-resistant agents. The process involves carbonization and pore adjustment under specific temperature and atmosphere to form a highly selective molecular sieve.
It improves the selective adsorption capacity of molecular sieves, enhances their corrosion resistance, wear resistance, and temperature resistance, and extends their service life.
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of molecular sieves, in particular to a preparation process of a highly selective molecular sieve. Background Art
[0002] Molecular sieve is a synthetic hydrated aluminosilicate or natural zeolite that has the function of screening molecules. However, it is difficult for existing molecular sieves to selectively adsorb molecules according to their size, shape, polarity and other characteristics, which leads to limitations. Therefore, a preparation process of highly selective molecular sieve is invented. Summary of the invention
[0003] In view of the above problems and / or the problems existing in the existing process for preparing a highly selective molecular sieve, the present invention is proposed.
[0004] Therefore, the object of the present invention is to provide a process for preparing a highly selective molecular sieve, which can solve the above-mentioned existing problems.
[0005] To solve the above technical problems, according to one aspect of the present invention, the present invention provides the following technical solutions:
[0006] A process for preparing a highly selective molecular sieve comprises the following specific steps:
[0007] Step 1, raw material preparation: first weigh the flower mud scraps, walnut shell powder, dried apple pomace, tourmaline powder, trehalose powder, preservative, wear-resistant agent, temperature-resistant agent and pore-blocking agent, and then grind the flower mud scraps, walnut shell powder, dried apple pomace, tourmaline powder and trehalose powder into powder;
[0008] Step 2, mixing: placing flower mud scraps, walnut shell powder, dried apple pomace, tourmaline powder, trehalose powder, preservative, anti-wear agent and temperature resistance agent in a reaction kettle for mixing;
[0009] Step 3: Forming: Use a twin-screw extruder to extrude the mixed raw materials into strips, and then dry the formed raw materials;
[0010] Step 4: impregnation: placing the dried raw material in a pore plugging agent for impregnation;
[0011] Step 5, carbonization and pore adjustment: the impregnated raw material is placed in a converter and carbonized and pore adjusted at 850°C-900°C. When the highest temperature is reached, the temperature is lowered to 760°C-780°C under the protection of nitrogen. The nitrogen flow rate is controlled at 4 cubic meters per hour, and the pore adjustment agent flow rate is 20-22 milliliters per minute for pore adjustment. The adjustment time is 80-120 minutes.
[0012] Step 6, finished product: Take a certain amount of high-temperature sample and cool it under vacuum, then package the product.
[0013] As a preferred scheme of the preparation process of a highly selective molecular sieve described in the present invention, wherein: the components in the raw materials are respectively measured by weight: 10-15 parts of flower mud scraps, 10-15 parts of walnut shell powder, 10-15 parts of dried apple pomace, 10-15 parts of tourmaline powder, 10-15 parts of trehalose powder, 4-6 parts of preservatives, 4-6 parts of wear-resistant agents, 4-6 parts of temperature-resistant agents, and 1-5 parts of pore-plugging agents.
[0014] As a preferred solution of the preparation process of a highly selective molecular sieve described in the present invention, the raw materials of the preservative include: polyurethane resin, diatomaceous earth, water-based epoxy resin, and high-alumina cement.
[0015] As a preferred solution of the preparation process of a highly selective molecular sieve according to the present invention, the preparation process of the preservative is as follows:
[0016] Process 1: placing polyurethane resin and diatomaceous earth in a reaction kettle for mixing;
[0017] Process 2: placing waterborne epoxy resin and high alumina cement in a reaction kettle for mixing;
[0018] Process 3: The mixture in process 1 and the mixture in process 2 are placed in a reaction kettle and mixed to obtain a preservative.
[0019] As a preferred solution of the preparation process of a highly selective molecular sieve described in the present invention, the raw materials of the wear-resistant agent include: polyurethane resin, high molecular polyethylene, graphite, glass fiber, and carbon fiber.
[0020] As a preferred solution of the preparation process of a highly selective molecular sieve described in the present invention, the preparation process of the anti-wear agent is as follows:
[0021] Process 1: placing polyurethane resin, high molecular weight polyethylene and graphite in a reaction kettle for mixing;
[0022] Process 2: placing glass fiber and carbon fiber in a reactor for mixing;
[0023] Process 3: The mixture in process 1 and the mixture in process 2 are placed in a reaction kettle for mixing to obtain an anti-wear agent.
[0024] As a preferred solution of the preparation process of a high-selectivity molecular sieve described in the present invention, the raw materials of the temperature-resistant agent include: quartz sand, clay, magnesite powder, dolomite powder, and silicon phosphide.
[0025] As a preferred solution of the preparation process of a high-selectivity molecular sieve described in the present invention, the preparation process of the temperature-resistant agent is as follows:
[0026] Process 1: Place quartz sand, clay and magnesite powder in a reactor and mix them;
[0027] Process 2: placing dolomite powder and silicon phosphide in a reaction kettle for mixing;
[0028] Process 3: The mixture in process 1 and the mixture in process 2 are placed in a reaction kettle for mixing to obtain a temperature-resistant agent.
[0029] As a preferred solution of the preparation process of a highly selective molecular sieve described in the present invention, the raw materials of the pore plugging agent include: deionized water, magnesium nitrate, and ferric nitrate.
[0030] As a preferred solution of the preparation process of a highly selective molecular sieve described in the present invention, the preparation process of the pore plugging agent is as follows:
[0031] Process 1: Mix deionized water and magnesium nitrate;
[0032] Process 2: Mix ferric nitrate and the mixture in process 1 to obtain a pore plugging agent.
[0033] Compared with existing technologies:
[0034] 1. By immersing the raw material in the pore blocking agent, the pores of the carbonized material can be blocked with metal ions. By blocking the pores of the carbonized material with metal ions, the molecular sieve can have high selective adsorption.
[0035] 2. By adding preservatives, anti-wear agents and temperature-resistant agents, the anti-corrosion performance, wear resistance and temperature resistance of the molecular sieve can be improved. By improving the anti-corrosion performance, wear resistance and temperature resistance of the molecular sieve, the use scenarios and service life of the molecular sieve can be improved. DETAILED DESCRIPTION
[0036] In order to make the objectives, technical solutions and advantages of the present invention more clear, the embodiments of the present invention will be described in further detail below.
[0037] Embodiment 1:
[0038] The present invention provides a process for preparing a highly selective molecular sieve, comprising the following specific steps:
[0039] Step 1, raw material preparation: first weigh the flower mud scraps, walnut shell powder, dried apple pomace, tourmaline powder, trehalose powder, preservative, wear-resistant agent, temperature-resistant agent and pore-blocking agent, and then grind the flower mud scraps, walnut shell powder, dried apple pomace, tourmaline powder and trehalose powder into powder;
[0040] Step 2, mixing: placing flower mud scraps, walnut shell powder, dried apple pomace, tourmaline powder, trehalose powder, preservative, anti-wear agent and temperature resistance agent in a reaction kettle for mixing;
[0041] Step 3: Forming: Use a twin-screw extruder to extrude the mixed raw materials into strips, and then dry the formed raw materials;
[0042] Step 4: impregnation: placing the dried raw material in a pore plugging agent for impregnation;
[0043] Step 5, carbonization and pore adjustment: the impregnated raw material is placed in a converter and carbonized and pore adjusted at 850°C. When the highest temperature is reached, the temperature is lowered to 760°C under the protection of nitrogen. The nitrogen flow rate is controlled at 4 cubic meters per hour, and the pore adjustment agent flow rate is 20 milliliters per minute for pore adjustment. The adjustment time is 80 minutes.
[0044] Step 6, finished product: Take a certain amount of high-temperature sample and cool it under vacuum, then package the product.
[0045] The components in the raw materials are measured by weight as follows: 10 parts of flower mud scraps, 10 parts of walnut shell powder, 10 parts of dried apple pomace, 10 parts of tourmaline powder, 10 parts of trehalose powder, 4 parts of preservatives, 4 parts of wear-resistant agents, 4 parts of temperature-resistant agents, and 10 parts of pore-plugging agents.
[0046] The raw materials of preservatives include: polyurethane resin, diatomaceous earth, water-based epoxy resin, and high-alumina cement;
[0047] The preparation process of the preservative is as follows:
[0048] Process 1: placing polyurethane resin and diatomaceous earth in a reaction kettle for mixing;
[0049] Process 2: placing waterborne epoxy resin and high alumina cement in a reaction kettle for mixing;
[0050] Process 3: The mixture in process 1 and the mixture in process 2 are placed in a reaction kettle and mixed to obtain a preservative.
[0051] The raw materials of wear-resistant agents include: polyurethane resin, high molecular polyethylene, graphite, glass fiber, carbon fiber;
[0052] The preparation process of wear-resistant agent is as follows:
[0053] Process 1: placing polyurethane resin, high molecular weight polyethylene and graphite in a reaction kettle for mixing;
[0054] Process 2: placing glass fiber and carbon fiber in a reactor for mixing;
[0055] Process 3: The mixture in process 1 and the mixture in process 2 are placed in a reaction kettle for mixing to obtain an anti-wear agent.
[0056] The raw materials of the temperature-resistant agent include: quartz sand, clay, magnesite powder, dolomite powder, silicon phosphide;
[0057] The preparation process of the temperature resistant agent is as follows:
[0058] Process 1: Place quartz sand, clay and magnesite powder in a reactor and mix them;
[0059] Process 2: placing dolomite powder and silicon phosphide in a reaction kettle for mixing;
[0060] Process 3: The mixture in process 1 and the mixture in process 2 are placed in a reaction kettle for mixing to obtain a temperature-resistant agent.
[0061] The raw materials of the pore plugging agent include: deionized water, magnesium nitrate, and ferric nitrate;
[0062] The preparation process of the pore plugging agent is as follows:
[0063] Process 1: Mix deionized water and magnesium nitrate;
[0064] Process 2: Mix ferric nitrate and the mixture in process 1 to obtain a pore plugging agent.
[0065] Embodiment 2:
[0066] The present invention provides a process for preparing a highly selective molecular sieve, comprising the following specific steps:
[0067] Step 1, raw material preparation: first weigh the flower mud scraps, walnut shell powder, dried apple pomace, tourmaline powder, trehalose powder, preservative, wear-resistant agent, temperature-resistant agent and pore-blocking agent, and then grind the flower mud scraps, walnut shell powder, dried apple pomace, tourmaline powder and trehalose powder into powder;
[0068] Step 2, mixing: placing flower mud scraps, walnut shell powder, dried apple pomace, tourmaline powder, trehalose powder, preservative, anti-wear agent and temperature resistance agent in a reaction kettle for mixing;
[0069] Step 3: Forming: Use a twin-screw extruder to extrude the mixed raw materials into strips, and then dry the formed raw materials;
[0070] Step 4: impregnation: placing the dried raw material in a pore plugging agent for impregnation;
[0071] Step 5, carbonization and pore adjustment: the impregnated raw material is placed in a converter and carbonized and pore adjusted at 875°C. When the highest temperature is reached, the temperature is lowered to 770°C under the protection of nitrogen. The nitrogen flow rate is controlled at 4 cubic meters per hour, and the pore adjustment agent flow rate is 21 milliliters per minute for pore adjustment. The adjustment time is 100 minutes.
[0072] Step 6, finished product: Take a certain amount of high-temperature sample and cool it under vacuum, then package the product.
[0073] The components in the raw materials are measured by weight as follows: 12.5 parts of flower mud scraps, 12.5 parts of walnut shell powder, 12.5 parts of dried apple pomace, 12.5 parts of tourmaline powder, 12.5 parts of trehalose powder, 5 parts of preservatives, 5 parts of wear-resistant agents, 5 parts of heat-resistant agents, and 2.5 parts of pore plugging agents.
[0074] The raw materials of preservatives include: polyurethane resin, diatomaceous earth, water-based epoxy resin, and high-alumina cement;
[0075] The preparation process of the preservative is as follows:
[0076] Process 1: placing polyurethane resin and diatomaceous earth in a reaction kettle for mixing;
[0077] Process 2: placing waterborne epoxy resin and high alumina cement in a reaction kettle for mixing;
[0078] Process 3: The mixture in process 1 and the mixture in process 2 are placed in a reaction kettle and mixed to obtain a preservative.
[0079] The raw materials of wear-resistant agents include: polyurethane resin, high molecular polyethylene, graphite, glass fiber, carbon fiber;
[0080] The preparation process of wear-resistant agent is as follows:
[0081] Process 1: placing polyurethane resin, high molecular weight polyethylene and graphite in a reaction kettle for mixing;
[0082] Process 2: placing glass fiber and carbon fiber in a reactor for mixing;
[0083] Process 3: The mixture in process 1 and the mixture in process 2 are placed in a reaction kettle for mixing to obtain an anti-wear agent.
[0084] The raw materials of the temperature-resistant agent include: quartz sand, clay, magnesite powder, dolomite powder, silicon phosphide;
[0085] The preparation process of the temperature resistant agent is as follows:
[0086] Process 1: Place quartz sand, clay and magnesite powder in a reactor and mix them;
[0087] Process 2: placing dolomite powder and silicon phosphide in a reaction kettle for mixing;
[0088] Process 3: The mixture in process 1 and the mixture in process 2 are placed in a reaction kettle for mixing to obtain a temperature-resistant agent.
[0089] The raw materials of the pore plugging agent include: deionized water, magnesium nitrate, and ferric nitrate;
[0090] The preparation process of the pore plugging agent is as follows:
[0091] Process 1: Mix deionized water and magnesium nitrate;
[0092] Process 2: Mix ferric nitrate and the mixture in process 1 to obtain a pore plugging agent.
[0093] Embodiment 3:
[0094] The present invention provides a process for preparing a highly selective molecular sieve, comprising the following specific steps:
[0095] Step 1, raw material preparation: first weigh the flower mud scraps, walnut shell powder, dried apple pomace, tourmaline powder, trehalose powder, preservative, wear-resistant agent, temperature-resistant agent and pore-blocking agent, and then grind the flower mud scraps, walnut shell powder, dried apple pomace, tourmaline powder and trehalose powder into powder;
[0096] Step 2, mixing: placing flower mud scraps, walnut shell powder, dried apple pomace, tourmaline powder, trehalose powder, preservative, anti-wear agent and temperature resistance agent in a reaction kettle for mixing;
[0097] Step 3: Forming: Use a twin-screw extruder to extrude the mixed raw materials into strips, and then dry the formed raw materials;
[0098] Step 4: impregnation: placing the dried raw material in a pore plugging agent for impregnation;
[0099] Step 5, carbonization and pore adjustment: the impregnated raw materials are placed in a converter and carbonized and pore adjusted at 900°C. When the highest temperature is reached, the temperature is lowered to 780°C under the protection of nitrogen. The nitrogen flow rate is controlled at 4 cubic meters per hour, and the pore adjustment agent flow rate is 22 milliliters per minute for pore adjustment. The adjustment time is 120 minutes.
[0100] Step 6, finished product: Take a certain amount of high-temperature sample and cool it under vacuum, then package the product.
[0101] The components in the raw materials are measured by weight as follows: 15 parts of flower mud scraps, 15 parts of walnut shell powder, 15 parts of dried apple pomace, 15 parts of tourmaline powder, 15 parts of trehalose powder, 6 parts of preservatives, 6 parts of wear-resistant agents, 6 parts of temperature-resistant agents, and 5 parts of pore-plugging agents.
[0102] The raw materials of preservatives include: polyurethane resin, diatomaceous earth, water-based epoxy resin, and high-alumina cement;
[0103] The preparation process of the preservative is as follows:
[0104] Process 1: placing polyurethane resin and diatomaceous earth in a reaction kettle for mixing;
[0105] Process 2: placing waterborne epoxy resin and high alumina cement in a reaction kettle for mixing;
[0106] Process 3: The mixture in process 1 and the mixture in process 2 are placed in a reaction kettle and mixed to obtain a preservative.
[0107] The raw materials of wear-resistant agents include: polyurethane resin, high molecular polyethylene, graphite, glass fiber, carbon fiber;
[0108] The preparation process of wear-resistant agent is as follows:
[0109] Process 1: placing polyurethane resin, high molecular weight polyethylene and graphite in a reaction kettle for mixing;
[0110] Process 2: placing glass fiber and carbon fiber in a reactor for mixing;
[0111] Process 3: The mixture in process 1 and the mixture in process 2 are placed in a reaction kettle for mixing to obtain an anti-wear agent.
[0112] The raw materials of the temperature-resistant agent include: quartz sand, clay, magnesite powder, dolomite powder, silicon phosphide;
[0113] The preparation process of the temperature resistant agent is as follows:
[0114] Process 1: Place quartz sand, clay and magnesite powder in a reactor and mix them;
[0115] Process 2: placing dolomite powder and silicon phosphide in a reaction kettle for mixing;
[0116] Process 3: The mixture in process 1 and the mixture in process 2 are placed in a reaction kettle for mixing to obtain a temperature-resistant agent.
[0117] The raw materials of the pore plugging agent include: deionized water, magnesium nitrate, and ferric nitrate;
[0118] The preparation process of the pore plugging agent is as follows:
[0119] Process 1: Mix deionized water and magnesium nitrate;
[0120] Process 2: Mix ferric nitrate and the mixture in process 1 to obtain a pore plugging agent.
[0121] The molecular sieves prepared in the above examples 1-3 were compared to obtain the following data:
[0122] Example 1 Example 2 Example 3 Wear resistance coefficient 90g / CM 96g / CM 92g / CM Corrosion resistance grade Sa2 Sa2.5 Sa2 Temperature resistance 787℃ 812℃ 765℃
[0123] It can be seen from the above table that the molecular sieves prepared in Examples 1-3 have good performance in terms of wear resistance coefficient, corrosion resistance level and temperature resistance. After use, Example 2 has the best effect.
[0124] Although the present invention has been described above with reference to the embodiments, various modifications may be made thereto and parts thereof may be replaced by equivalents without departing from the scope of the present invention. In particular, as long as there is no structural conflict, the various features in the embodiments disclosed in the present invention may be used in combination with each other in any manner, and the fact that these combinations are not exhaustively described in this specification is only for the sake of omitting space and saving resources. Therefore, the present invention is not limited to the specific embodiments disclosed herein, but includes all technical solutions falling within the scope of the claims.
Claims
1. A process for preparing a highly selective molecular sieve, characterized in that: The specific steps are as follows: Step 1, raw material preparation: first weigh the flower mud scraps, walnut shell powder, dried apple pomace, tourmaline powder, trehalose powder, preservative, wear-resistant agent, temperature-resistant agent and pore-blocking agent, and then grind the flower mud scraps, walnut shell powder, dried apple pomace, tourmaline powder and trehalose powder into powder; Step 2, mixing: placing flower mud scraps, walnut shell powder, dried apple pomace, tourmaline powder, trehalose powder, preservative, anti-wear agent and temperature resistance agent in a reaction kettle for mixing; Step 3: Forming: Use a twin-screw extruder to extrude the mixed raw materials into strips, and then dry the formed raw materials; Step 4: impregnation: placing the dried raw material in a pore plugging agent for impregnation; Step 5, carbonization and pore adjustment: the impregnated raw material is placed in a converter and carbonized and pore adjusted at 850°C-900°C. When the highest temperature is reached, the temperature is lowered to 760°C-780°C under the protection of nitrogen. The nitrogen flow rate is controlled at 4 cubic meters per hour, and the pore adjustment agent flow rate is 20-22 milliliters per minute for pore adjustment. The adjustment time is 80-120 minutes. Step 6, finished product: Take a certain amount of high-temperature sample and cool it under vacuum, then package the product.
2. The process for preparing a highly selective molecular sieve according to claim 1, characterized in that: The components in the raw materials are respectively as follows by weight: 10-15 parts of flower mud scraps, 10-15 parts of walnut shell powder, 10-15 parts of dried apple pomace, 10-15 parts of tourmaline powder, 10-15 parts of trehalose powder, 4-6 parts of preservatives, 4-6 parts of wear-resistant agents, 4-6 parts of temperature-resistant agents, and 1-5 parts of pore plugging agents.
3. A process for preparing a highly selective molecular sieve according to claim 2, characterized in that: The raw materials of the preservative include: polyurethane resin, diatomaceous earth, water-based epoxy resin and high-alumina cement.
4. A process for preparing a highly selective molecular sieve according to claim 3, characterized in that: The preparation process of the preservative is as follows: Process 1: placing polyurethane resin and diatomaceous earth in a reaction kettle for mixing; Process 2: placing waterborne epoxy resin and high alumina cement in a reaction kettle for mixing; Process 3: The mixture in process 1 and the mixture in process 2 are placed in a reaction kettle and mixed to obtain a preservative.
5. The process for preparing a highly selective molecular sieve according to claim 2, characterized in that: The raw materials of the wear-resistant agent include: polyurethane resin, high molecular polyethylene, graphite, glass fiber and carbon fiber.
6. A process for preparing a highly selective molecular sieve according to claim 5, characterized in that: The preparation process of the wear-resistant agent is as follows: Process 1: placing polyurethane resin, high molecular weight polyethylene and graphite in a reaction kettle for mixing; Process 2: placing glass fiber and carbon fiber in a reactor for mixing; Process 3: The mixture in process 1 and the mixture in process 2 are placed in a reaction kettle for mixing to obtain an anti-wear agent.
7. The process for preparing a highly selective molecular sieve according to claim 2, characterized in that: The raw materials of the temperature-resistant agent include: quartz sand, clay, magnesite powder, dolomite powder and silicon phosphide.
8. The process for preparing a highly selective molecular sieve according to claim 7, characterized in that: The preparation process of the temperature resistant agent is as follows: Process 1: Place quartz sand, clay and magnesite powder in a reactor and mix them; Process 2: placing dolomite powder and silicon phosphide in a reaction kettle for mixing; Process 3: The mixture in process 1 and the mixture in process 2 are placed in a reaction kettle for mixing to obtain a temperature-resistant agent.
9. The process for preparing a highly selective molecular sieve according to claim 2, characterized in that: The raw materials of the pore plugging agent include: deionized water, magnesium nitrate and ferric nitrate.
10. The process for preparing a highly selective molecular sieve according to claim 9, characterized in that: The preparation process of the pore plugging agent is as follows: Process 1: Mix deionized water and magnesium nitrate; Process 2: Mix ferric nitrate and the mixture in process 1 to obtain a pore plugging agent.
Citation Information
Patent Citations
Preparation technology of high-performance carbon molecular sieve
CN105152156A
Heat-resistant high-strength wood-plastic composite material and preparation method thereof
CN107418029A
Method for preparing carbon molecular sieve from biological semi-coke
CN112142047A
Fine-particle high-tap-density spherical graphite
CN116178018A
Environment-friendly anti-mildew antibacterial PVC floor printing film and preparation process thereof
CN117070036A