Bio-based triphenylmethane phthalonitrile monomer as well as preparation method and application thereof

The bio-based triphenyl phthalene monomer was prepared by solid super acid catalysis and magnesium oxide catalysis, which solved the problems of environmental pollution and side reactions in the traditional preparation process, and obtained a resin with excellent high temperature resistance. Improve the efficiency of biomass resources utilization.

CN119019286APending Publication Date: 2024-11-26HARBIN ENG UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411134553.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-19
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

The preparation process of existing bio-based phthalonitrile monomers has problems such as environmental pollution, the use of toxic solvents, and side reactions. The traditional catalysts lack water absorption and cannot effectively utilize biomass resources.

Method used

Tritylmethane-type triphenol compounds were prepared by solid super acid catalyzed bio-derived aldehyde and biomonophenol reaction, and under the protection of inert gas, magnesium oxide was used to catalyze triptylmethane-type triphenol and 4-nitrophthalene phenol under the protection of inert gas. The reaction was used to produce bio-trityl phthalene monomer, avoiding side reactions caused by the use of toxic azeotropic solvents and water.

Benefits of technology

The efficient preparation of bio-based monomers is achieved, and the obtained resin has excellent high temperature resistance and good processing window, which improves the utilization efficiency of biomass resources and reduces the harm to the environment.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119019286A_ABST
    Figure CN119019286A_ABST
Patent Text Reader

Abstract

The invention discloses a bio-based triphenylmethane phthalonitrile monomer as well as a preparation method and application thereof, and belongs to the technical field of organic synthesis. The invention solves the problems of low yield, pollution and the like of the existing phthalonitrile monomer. The method comprises the following steps: firstly, catalyzing a reaction of bio-based derivative aldehyde and biological monophenol by using solid superacid to prepare a triphenylmethane type triphenol compound, then taking the triphenylmethane type triphenol compound and 4-nitrophthalonitrile as raw materials, and carrying out a catalytic reaction in polyethylene glycol by using magnesium oxide to obtain a bio-based triphenylmethane type phthalonitrile monomer; a resin prepolymer prepared from the monomer has a wide processing window, low melt viscosity and good processability, and resin obtained after further curing has a high glass transition temperature. According to the monomer preparation process provided by the invention, the utilization efficiency of biomass resources is increased, and compared with the traditional petroleum-based phthalonitrile resin, the obtained resin has excellent high temperature resistance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a bio-based triphenylmethane type phthalonitrile monomer and a preparation method and application thereof, belonging to the technical field of organic synthesis. Background Art

[0002] Phthalonitrile resin has excellent properties such as high glass transition temperature, excellent thermal oxidation stability and flame retardancy, good mechanical properties and low water absorption. It has broad application prospects in high-tech fields such as aerospace, shipbuilding, automobiles, electronics, and machinery.

[0003] In the molecular design of phthalonitrile resin monomers and polymers, the current research hotspot is to use phthalonitrile for end-capping or side-chain polyarylether, polyarylether nitrile, polyimide, etc. by introducing functional, polymerizable groups such as imide and benzoxazine. Progress has been made, but there is still little research on the design of multifunctional phthalonitrile monomers and the performance of the resin after curing.

[0004] Due to the non-renewability and adverse effects on the environment of traditional petroleum-based materials, non-petroleum-based polymer materials and bio-based materials based on renewable resources have received unprecedented attention. At present, most of the research on bio-based phthalonitrile resins directly utilizes existing bio-based phenols. However, the types of bisphenols and triphenols obtained from natural extracts are relatively small and expensive. For example, Laskoski's team used resveratrol and hydrogenated resveratrol to synthesize trifunctional bio-based phthalonitrile monomers, but the extraction process of resveratrol and hydrogenated resveratrol is cumbersome and expensive, and requires the use of a large amount of organic solvents.

[0005] Bio-derived aldehydes and bio-monophenols are widely available and are key basic monomers for the preparation of bio-phenolic compounds. They contain multiple active groups and can be used to prepare bio-derived bisphenols and triphenols through acid or base catalysis to improve the utilization efficiency of bio-derived aldehydes and bio-monophenols. However, the liquid acids or bases used for catalysis have problems such as polluting the environment, corroding equipment, and being difficult to separate from the products. In addition, DMSO and DMF are generally selected as solvents for the preparation of phthalonitrile. Such solvents are volatile organic compounds and have a huge impact on human health and production safety. At the same time, it will also cause serious harm to the environment, such as inducing smog weather, destroying the ozone layer, and causing a greenhouse effect.

[0006] In addition, the synthesis of phthalonitrile monomers relies on the nucleophilic substitution reaction between aromatic nitro or halogen-substituted nitriles and phenols, and potassium carbonate or sodium carbonate is often used as catalysts. However, both catalysts have weak water absorption and cannot absorb the water generated during the synthesis process. Therefore, toxic benzene or toluene is required as an azeotropic solvent to remove the generated water, thereby reducing the occurrence of side reactions.

[0007] Based on this, it is very necessary to provide a bio-based multifunctional phthalonitrile monomer with a simple and green preparation process and excellent high temperature resistance after curing, so as to provide new ideas for the efficient utilization of biomass resources. Summary of the invention

[0008] In view of the above technical problems existing in the existing phthalonitrile monomers, the present invention provides a bio-based triphenylmethane type phthalonitrile monomer and a preparation method and application thereof.

[0009] The technical solution of the present invention:

[0010] One of the purposes of the present invention is to provide a bio-based triphenylmethane-type phthalonitrile monomer, the chemical structure of which is as follows:

[0011]

[0012] In the formula The structure is:

[0013]

[0014] It is further defined that the monomer is prepared by using a triphenylmethane type triphenol compound and 4-nitrophthalonitrile as raw materials, in a polyethylene glycol solvent under the protection of an inert gas, and using magnesium oxide as a catalyst to react;

[0015] The triphenylmethane triphenol compound is obtained by reacting a bio-based derived aldehyde and a bio-monophenol catalyzed by a solid superacid.

[0016] In a further embodiment, the bio-derived aldehyde is syringaldehyde, vanillin or parabenaldehyde.

[0017] It is further defined that the biomonophenol is phenol, guaiacol or syringol.

[0018] The second object of the present invention is to provide a method for preparing the above-mentioned bio-based triphenylmethane-type phthalonitrile monomer, which comprises the following steps:

[0019] (1) Synthesis of triphenylmethane-type triphenol compounds;

[0020] The bio-based derived aldehyde and bio-monophenol are dissolved in anhydrous ethanol, solid superacid is added in batches at room temperature, and then the temperature is raised to 40-78°C for reaction for 5-10 hours. After the reaction is completed, the solid superacid is recovered, and the liquid phase is washed with distilled water, purified, and dried to obtain a triphenylmethane triphenol compound;

[0021] (2) Synthesize bio-based triphenylmethane-type phthalonitrile monomers;

[0022] Under the protection of inert gas, a triphenylmethane triphenol compound and magnesium oxide are reacted in polyethylene glycol at 100-150° C. for 8-12 hours, the temperature is lowered to 50-80° C., 4-nitrophthalonitrile is added, and the reaction is continued for 8-12 hours. The reaction solution is poured into dilute hydrochloric acid for precipitation, filtered, and the precipitate is washed with sodium hydroxide solution, distilled water and anhydrous ethanol in sequence, and dried to obtain a bio-based triphenylmethane phthalonitrile monomer.

[0023] It is further defined that the volume ratio of the amount of the bio-derived aldehyde substance, the amount of the bio-monophenol substance and the anhydrous ethanol in (1) is 1 mol: (2-2.1) mol: (0.3-0.4) L.

[0024] It is further defined that (1) the amount of solid superacid added is 4 wt.% of the total mass of bio-derived aldehyde and bio-monophenol.

[0025] It is further defined that the drying conditions in (1) are: drying at 45°C under vacuum for 12 to 24 hours.

[0026] Further defined, the solid superacid is SO 4 2- / ZrO 2 Solid acid, SO 4 2- / TiO 2 Solid acid, SO 4 2- / Fe 2 O 3 Solid acid or SO 4 2- / SnO 2 One of the solid acids.

[0027] It is further defined that the molar ratio of the triphenylmethane type triphenol compound, magnesium oxide and 4-nitrophthalonitrile in (2) is 1:(3 to 3.6):(3 to 3.6).

[0028] It is further defined that the ratio of the amount of the triphenylmethane type triphenol compound substance to the volume of the polyethylene glycol in (2) is 1 mol:(4-10)L.

[0029] It is further defined that the molecular weight of the polyethylene glycol in (2) is 200 to 800.

[0030] Further limited to, the molecular weight of the polyethylene glycol in (2) is 200, 300, 400, 600 or 800.

[0031] It is further defined that the concentration of the sodium hydroxide solution in (2) is 0.5 mol / L.

[0032] It is further defined that the drying conditions in (2) are: drying at 40-80° C. under vacuum conditions for 24-48 hours.

[0033] The third object of the present invention is to provide an application of the above-mentioned bio-based triphenylmethane type phthalonitrile monomer, specifically for preparing bio-based triphenylmethane type phthalonitrile resin.

[0034] It is further defined that the method for preparing bio-based triphenylmethane phthalonitrile resin using bio-based triphenylmethane phthalonitrile monomer is: mixing the bio-based triphenylmethane phthalonitrile monomer and the curing agent in a molten state to obtain a prepolymer, and placing the prepolymer into a mold for hot pressing.

[0035] It is further defined that the curing agent is 4-(4-aminophenoxy)phthalonitrile, and the amount used is 10wt.% of the bio-based triphenylmethane type phthalonitrile monomer.

[0036] It is further defined that the curing process is: keep at 210°C for 3 hours, heat to 240°C for 3 hours, heat to 270°C for 3 hours, heat to 300°C for 3 hours, heat to 330°C for 3 hours, and finally heat to 375°C for 5 hours.

[0037] Beneficial effects:

[0038] The present invention first utilizes solid superacid to catalyze the reaction of bio-based derivative aldehyde and bio-monophenol to prepare triphenylmethane type triphenol compound, then uses triphenylmethane type triphenol compound and 4-nitrophthalonitrile as raw materials, in polyethylene glycol, magnesium oxide catalytic reaction obtains bio-based triphenylmethane type phthalonitrile monomer, and the resin prepolymer prepared by using the monomer has a wide processing window and low melt viscosity, showing good processability, and the resin obtained after further curing has a higher glass transition temperature. Compared with the prior art, the monomer preparation process provided by the present invention provides a green solution for the efficient utilization of bio-based derivative aldehyde and bio-monophenol, and the obtained resin has excellent high temperature resistance compared with traditional petroleum-based phthalonitrile resin, and increases the utilization efficiency of biomass resources, and has more carbon reduction and renewable advantages. In addition, the present invention selects magnesium oxide as a catalyst, and utilizes its water absorption and the characteristics of ionizing and catalyzing substituted phenols, which can not only avoid the use of toxic azeotropic solvents, but also avoid the side reactions caused by water. BRIEF DESCRIPTION OF THE DRAWINGS

[0039] Figure 1 This is the infrared spectrum of the bio-based triphenylmethane-type phthalonitrile monomer prepared in Example 1;

[0040] Figure 2 This is the H NMR spectrum of the bio-based triphenylmethane-type phthalonitrile monomer prepared in Example 1;

[0041] Figure 3 This is the thermal decomposition curve of the bio-based triphenylmethane-type phthalonitrile resin prepared in Example 1. DETAILED DESCRIPTION

[0042] In order to make the above-mentioned objects, features and advantages of the present invention more obvious and easy to understand, the specific implementation methods of the present invention are described in detail below in conjunction with the embodiments of the specification.

[0043] In the following description, many specific details are set forth to facilitate a full understanding of the present invention, but the present invention may also be implemented in other ways different from those described herein, and those skilled in the art may make similar generalizations without violating the connotation of the present invention. Therefore, the present invention is not limited to the specific embodiments disclosed below.

[0044] Secondly, the term "one embodiment" or "embodiment" as used herein refers to a specific feature, structure, or characteristic that may be included in at least one implementation of the present invention. The term "in one embodiment" that appears in different places in this specification does not necessarily refer to the same embodiment, nor does it refer to a separate or selective embodiment that is mutually exclusive with other embodiments.

[0045] The experimental methods used in the following examples are conventional methods unless otherwise specified. The materials, reagents, methods and instruments used are conventional materials, reagents, methods and instruments in the art unless otherwise specified, and can be obtained through commercial channels by those skilled in the art, and the purity of the solid and liquid reagents used is analytically pure.

[0046] SO used in the following examples 4 2- / Fe 2 O 3 Solid acid and SO 4 2- / ZrO 2 The solid acids were purchased from Qinzhou Yamei Chemical Co., Ltd.

[0047] Example 1

[0048] Step 1: Synthesis of triphenylmethane triphenol compounds:

[0049] Vanillin (0.1 mol, 15.4 g) and guaiacol (0.2 mol, 24.8 g) were dissolved in 32 mL of anhydrous ethanol and SO 4 2- / Fe 2 O 3Solid acid (1.61 g, accounting for 4 wt.% of the total mass of vanillin and guaiacol) was slowly added in batches, and after completion, the reaction was continued at 50°C for 6 hours. After the reaction was completed, the solid acid was filtered and recovered, the liquid phase was washed with distilled water, and then purified by column chromatography, and the sample was vacuum dried at 45°C for 12 hours to obtain a triphenylmethane triphenol compound 4,4',4"-methanetriethyltris(2-methoxyphenol) (abbreviated as GVT), which was set aside.

[0050] Step 2: Synthesis of bio-based triphenylmethane-type phthalonitrile monomer:

[0051] GVT (0.01 mol, 3.8 g), magnesium oxide (0.03 mol, 1.2 g) and polyethylene glycol-200 (50 mL) were added to a three-necked flask with a magnetic rotor, and condensed and refluxed at 120°C for 10 h. After the reaction was completed, it was cooled to room temperature, and 4-nitrophthalonitrile (0.03 mol, 5.2 g) was added, and the reaction was continued at 60°C for 12 h. Then the mixture was cooled to room temperature, poured into 250 mL of dilute hydrochloric acid (0.5 mol / L), filtered, and washed with 1 mol / L NaOH, distilled water, and anhydrous ethanol for multiple times, and dried in a vacuum drying oven at 50°C for 48 h to obtain a bio-based triphenylmethane type phthalonitrile monomer (GVTP) with a yield of 85%, which was set aside.

[0052] The structure of the bio-based triphenylmethane-type phthalonitrile monomer GVTP obtained in step 2 was characterized, and the infrared spectrum was as follows: Figure 1 As shown by Figure 1 It can be seen that the GVTP curve is at 2231cm -1 There is a very obvious absorption peak at , which is the stretching vibration peak of cyano group (C≡N). Figure 2 is the H NMR spectrum of GVTP, such as Figure 2 As shown, 3.67 ppm is the proton hydrogen on the methoxy group (O-CH 3 ). The peak at 5.84ppm is the chemical shift of the proton hydrogen (CH) on the carbon connected to the three benzene rings. The peak at 6.89-8.09ppm is attributed to the chemical shift of the proton hydrogen on the benzene ring. Combined with the infrared spectrum and nuclear magnetic hydrogen spectrum, it is shown that the obtained structure is consistent with the designed structure, as shown in the following structure;

[0053]

[0054] Step 3: Preparation of bio-based triphenylmethane phthalonitrile resin:

[0055] 10 wt% of 4-(4-aminophenoxy)phthalonitrile was added to GVTP as a curing agent, and mixed evenly in a molten state to obtain a prepolymer. The prepolymer was placed in a mold and heated at 10 kg / cm 3The specific curing process temperature is set as follows: 210℃ for 3h, 240℃ for 3h, 270℃ for 3h, 300℃ for 3h, 330℃ for 3h, and finally 375℃ for 5h to obtain bio-based triphenylmethane type phthalonitrile resin.

[0056] The bio-based triphenylmethane phthalonitrile resin obtained in step 3 was subjected to TGA test under nitrogen. The thermal decomposition curve is as follows: Figure 3 As shown by Figure 3 It can be seen that the glass transition temperature of the resin is 401.8°C, T 5 (thermal decomposition temperature of 5% weight loss) = 521.0°C, T 10 (Thermal decomposition temperature at 10% weight loss) = 557.2°C, and the residual carbon rate (800°C) is 68.0%, showing excellent heat resistance.

[0057] Example 2

[0058] GVT was prepared using the method of Example 1. GVT (0.01 mol, 3.8 g), magnesium oxide (0.03 mol, 1.2 g) and polyethylene glycol-200 (40 mL) were added to a three-necked flask with a magnetic rotor, condensed and refluxed at 150° C. for 8 h, cooled to room temperature after the reaction, and then 4-nitrophthalonitrile (0.03 mol, 5.2 g) was added, and the reaction was continued at 70° C. for 10 h. The mixture was then cooled to room temperature, poured into 250 mL of dilute hydrochloric acid (0.5 mol / L), filtered, and washed with 1 mol / L NaOH, distilled water, and anhydrous ethanol for multiple times in sequence, and dried in a vacuum drying oven at 60° C. for 36 h. The yield of the obtained bio-based triphenylmethane-type phthalonitrile monomer GVTP was 84%.

[0059] Example 3

[0060] GVT was prepared using the method of Example 1. GVT (0.01 mol, 3.8 g), magnesium oxide (0.03 mol, 1.2 g) and polyethylene glycol-200 (90 mL) were added to a three-necked flask with a magnetic rotor, condensed and refluxed at 100°C for 12 h, cooled to room temperature after the reaction, and then 4-nitrophthalonitrile (0.03 mol, 5.2 g) was added, and the reaction was continued at 80°C for 8 h. The mixture was then cooled to room temperature, poured into 250 mL of dilute hydrochloric acid (0.5 mol / L), filtered, washed with 1 mol / L NaOH, distilled water, and anhydrous ethanol for multiple times, and dried in a vacuum drying oven at 70°C for 24 h. The yield of the obtained bio-based triphenylmethane-type phthalonitrile monomer GVTP was 83%.

[0061] Example 4

[0062] Step 1: Synthesis of triphenylmethane triphenol compounds:

[0063] Phenol (0.2 mol, 18.82 g) and paraben aldehyde (0.1 mol, 12.2 g) were dissolved in 30 mL of anhydrous ethanol. 4 wt.% of SO 4 2- / Fe 2 O 3 The solid acid was slowly added in batches, and after completion, the reaction was continued at 40°C for 7 hours. After the reaction was completed, the solid acid was filtered and recovered, the liquid phase was washed with distilled water, and then purified by column chromatography, and the sample was vacuum dried at 45°C for 18 hours to obtain the monomer 4,4',4"-formyltriphenol (PHT) for later use.

[0064] Step 2: Synthesis of bio-based triphenylmethane-type phthalonitrile monomer:

[0065] PHT was used to replace GVT in step 2 of Example 1, polyethylene glycol-600 was selected as the solvent, and the other parameters were set the same as in Example 1 to obtain a bio-based triphenylmethane-type phthalonitrile monomer with a structure shown below, with a yield of 85%.

[0066]

[0067] Example 5

[0068] Step 1: Synthesis of triphenylmethane triphenol compounds:

[0069] Syringol (0.2 mol, 30.8 g) and syringaldehyde (0.1 mol, 18.2 g) were dissolved in 38 mL of anhydrous ethanol and SO 4 2- / ZrO 2 Solid acid (1.96 g) was slowly added in batches, and after completion, the reaction was continued at 78°C for 6 hours. After the reaction was completed, the solid acid was recovered by filtration, the liquid phase was washed with distilled water, and then purified by column chromatography, and the sample was vacuum dried at 45°C for 24 hours to obtain the monomer 4,4',4'-formyltris(2,6-dimethoxyphenol) (SST) for use.

[0070] Step 2: Synthesis of bio-based triphenylmethane-type phthalonitrile monomer:

[0071] SST was used to replace GVT in step 2 of Example 1, polyethylene glycol-400 was selected as the solvent, and the other parameters were set the same as in Example 1 to obtain a bio-based triphenylmethane-type phthalonitrile monomer with a structure shown below, with a yield of 83%.

[0072]

[0073] Comparative Example 1

[0074] The difference between this comparative example and Example 1 is that ethylene glycol is used instead of polyethylene glycol-200 in step 2, and the other parameter settings and process steps are the same as those of Example 1. After the reaction is completed, the mixture is cooled to room temperature and poured into 250 mL of dilute hydrochloric acid. No obvious solid precipitation occurs, indicating that the bio-based triphenylmethane-type phthalonitrile monomer has not been successfully prepared.

[0075] Comparative Example 2

[0076] The difference between this comparative example and Example 1 is that polyethylene glycol-2000 is used instead of polyethylene glycol-200 in step 2, and the other parameter settings and process steps are the same as those of Example 1. The yield of the obtained bio-based triphenylmethane-type phthalonitrile monomer GVTP is 50%, which is mainly due to the high viscosity of the system during the reaction, and the yield is greatly reduced compared with Example 1.

[0077] Comparative Example 3

[0078] The difference between this comparative example and Example 1 is that K 2 CO 3 (0.03 mol, 4.2 g) was used to replace magnesium oxide, and the other parameter settings and process steps were the same as those in Example 1. The yield of the obtained bio-based triphenylmethane phthalonitrile monomer GVTP was 78%, which was due to the side reaction caused by water produced during the reaction, resulting in a slight decrease in the yield.

[0079] Although the present invention has been disclosed as above in the preferred embodiment, it is not intended to limit the present invention. Anyone familiar with this technology can make various changes and modifications without departing from the spirit and scope of the present invention. Therefore, the scope of protection of the present invention should be based on the definition of the claims.

Claims

1. A bio-based triphenylmethane-type phthalonitrile monomer, characterized in that: The chemical structure of the monomer is as follows: In the formula The structure is:

2. The monomer according to claim 1, characterized in that The monomer is prepared by using triphenylmethane triphenol compound and 4-nitrophthalonitrile as raw materials, in a polyethylene glycol solvent under the protection of an inert gas, and using magnesium oxide as a catalyst. The triphenylmethane triphenol compound is obtained by reacting a bio-based derived aldehyde and a bio-monophenol catalyzed by a solid superacid.

3. The monomer according to claim 2, characterized in that The bio-derived aldehyde is syringaldehyde, vanillin or parabenaldehyde; the bio-monophenol is phenol, guaiacol or syringol.

4. A method for preparing the bio-based triphenylmethane-type phthalonitrile monomer according to any one of claims 1 to 3, characterized in that: include: (1) Synthesis of triphenylmethane-type triphenol compounds; The bio-based derived aldehyde and bio-monophenol are dissolved in anhydrous ethanol, solid superacid is added in batches at room temperature, and then the temperature is raised to 40-78°C for reaction for 5-10 hours. After the reaction is completed, the solid superacid is recovered, and the liquid phase is washed with distilled water, purified, and dried to obtain a triphenylmethane triphenol compound; (2) Synthesize bio-based triphenylmethane-type phthalonitrile monomers; Under the protection of inert gas, a triphenylmethane triphenol compound and magnesium oxide are reacted in polyethylene glycol at 100-150° C. for 8-12 hours, the temperature is lowered to 50-80° C., 4-nitrophthalonitrile is added, and the reaction is continued for 8-12 hours. The reaction solution is poured into dilute hydrochloric acid for precipitation, filtered, and the precipitate is washed with sodium hydroxide solution, distilled water and anhydrous ethanol in sequence, and dried to obtain a bio-based triphenylmethane phthalonitrile monomer.

5. The preparation method according to claim 4, characterized in that: (1) The volume ratio of the amount of bio-derived aldehyde substance, the amount of bio-monophenol substance and anhydrous ethanol is 1 mol: (2-2.1) mol: (0.3-0.4) L; the amount of solid superacid added accounts for 4 wt.% of the total mass of bio-derived aldehyde and bio-monophenol.

6. The preparation method according to claim 4 or 5, characterized in that: Solid superacid is SO4 2- / ZrO2-based solid acid, SO4 2- / TiO2 based solid acid, SO4 2- / Fe2O3 based solid acid or SO4 2- / One of the SnO2-based solid acids.

7. The preparation method according to claim 4, characterized in that: The molar ratio of the triphenylmethane type triphenol compound, magnesium oxide and 4-nitrophthalonitrile in (2) is 1:(3 to 3.6):(3 to 3.6).

8. The preparation method according to claim 4, characterized in that: (2) The ratio of the amount of triphenylmethane triphenol compound to the volume of polyethylene glycol is 1 mol: (4-10) L.

9. The preparation method according to claim 4, characterized in that: (2) The molecular weight of polyethylene glycol is 200 to 800.

10. Use of the bio-based triphenylmethane-type phthalonitrile monomer according to any one of claims 1 to 3, characterized in that: Used to prepare bio-based triphenylmethane-type phthalonitrile resin.