Aggregation-induced emission material as well as preparation method and application thereof
By using new aggregation-induced luminescent materials in microcavity lasers, the problems of low quantum yield and high operational difficulty of gain materials are solved, efficient and stable laser output is achieved, and its application in the fields of detection and materials has been expanded.
Patent Information
- Application Number
- CN202410918948.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-10
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2044-07-10
Smart Images

Figure CN119019432A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of micro-nano optics and material synthesis technology, and in particular to an aggregation-induced luminescence material and a preparation method and application thereof. Background Art
[0002] Whispering Gallery Mode (WGM) lasers use light to propagate on the inner surface of a high refractive index cavity and form total reflection, so that the light wave is transmitted along the inner wall of the microcavity with extremely low energy dissipation. Therefore, WGM lasers have the advantages of extremely high quality factor, small mode volume, fast dynamic response, and high sensitivity. These characteristics contribute to the application of WGM microcavities in single nanoparticle detection, biosensing, optical communications, and integrated circuits.
[0003] Like traditional lasers, microcavity lasers require gain media, pump sources, and resonant cavities (WGM microcavities). The pump source is used to provide energy to the gain medium to achieve population inversion and form lasers. The gain medium material determines the spectral, temporal, and power characteristics of the laser emission. Organic fluorescent dyes are commonly used gain media in active microcavities. However, traditional organic dyes generally have aggregation quenching (ACQ) phenomena. At high concentrations or in aggregated states, only weak emission is produced due to strong interactions between molecules, which seriously affects the gain properties of the dyes. Literature reports that fluorescein shows a trend of decreasing fluorescence intensity in an aggregated state, or even complete quenching, which is unfavorable for experimental studies that require repeated measurements and high pump power, and will seriously restrict the performance of microcavity laser devices. It can be seen that the choice of gain medium materials has a decisive influence on the performance of the laser, which determines key parameters such as the spectral characteristics, output power, and temporal characteristics of the laser. Therefore, researchers are currently actively exploring new organic gain materials in order to improve the performance and application range of lasers.
[0004] Aggregation induced emission luminogens (AIEs) are a special class of fluorescent molecules that emit almost no light or very weak light in a dissolved state, but emit strong fluorescence when aggregated. Aggregation induced emission dyes have the advantages of high luminescence efficiency and high doping concentration, and there is no self-quenching phenomenon of fluorescent dyes under high concentration or aggregation conditions. Therefore, by increasing the concentration of aggregation induced emission dyes to obtain higher fluorescence emission intensity, or by reducing the effective concentration of application through efficient luminescence in the aggregated state, the above problems of organic dyes in microcavity lasers can be effectively solved. For example, the invention patent CN111952827B discloses a bottle-shaped polymer microcavity laser based on aggregation induced emission dye gain and a preparation method thereof. The method comprises: dripping a dye solution into a polymer fluid to obtain a precursor solution; adding a precursor solution to the thinnest part of a bidirectional tapered optical fiber, self-assembling a polymer microcavity, obtaining a bottle-shaped microcavity, and curing; coupling with the equatorial plane at the maximum diameter of the bottle-shaped microcavity with another bidirectional tapered optical fiber, encapsulating, and obtaining a microcavity laser. Invention patent CN110676684B discloses a gain material self-aggregation laser and its preparation method. The laser is a polymer microsphere containing a gain material that exists stably in a solution, and a surfactant is distributed on the surface of the microsphere, and the concentration of the gain material in the polymer microsphere is higher than the concentration in the solution outside the polymer microsphere, and the gain material does not emit light in the solution, and the laser is realized in the polymer microsphere. The above method is usually synthesized in a self-assembled manner to synthesize a microsphere microcavity, and then the optical fiber is coupled to excite the laser. However, this method has great defects. On the one hand, the self-assembly method has high requirements on the manufacturing precision and the tapered optical fiber is fragile and easy to damage during the manufacturing process, which is difficult to manufacture. The formation of the whispering gallery microsphere cavity is difficult and complicated; and each time the organic dye is replaced, the microsphere needs to be re-self-assembled, which is inconvenient for the experimental operation and reduces the practicality. On the other hand, the tapered optical fiber is more susceptible to external interference, resulting in data instability. More importantly, the traditional aggregation-induced emission material is used, and the quantum yield is low, generally less than 50%. Summary of the invention
[0005] In view of the above-mentioned deficiencies in the prior art, the technical problems to be solved by the present invention are: to provide an aggregation-induced light-emitting material and a preparation method and application thereof, thereby enriching the types and selectivity of existing light-emitting materials; the present invention also provides the application of the aggregation-induced light-emitting material in a microcavity laser, thereby solving the problems existing in the existing microcavity laser, such as low quantum yield of the light-emitting material, fluorescence quenching (ACQ) of the existing gain material in the solid or aggregated state, poor stability and great difficulty in operation.
[0006] In order to solve the above technical problems, the present invention adopts the following technical solution: an aggregation-induced luminescent material, the structural formula of the luminescent material is as follows:
[0007] Another object of the present invention is to provide a method for preparing the above-mentioned aggregation-induced emission material, and the synthesis route thereof is as follows:
[0008]
[0009] The following steps are involved:
[0010] S1: Compound 1 and N-iodosuccinimide are dissolved in CH2Cl2 solvent, and then the reaction solution is stirred at room temperature until the raw material is completely consumed as monitored by TLC analysis. After the reaction is completed, it is vacuum concentrated and the obtained solid is separated by column chromatography to obtain a red intermediate compound 2.
[0011] S2: Compound 2 and 4-(1,2,2-triphenylvinyl)phenylboronic acid are placed in a tetrahydrofuran solvent, and tetrakis(triphenylphosphine)palladium and K2CO3 are added in sequence to obtain a reaction solution, and then the reaction solution is placed in an inert gas environment for reaction and stirred overnight. After the reaction is completed, the reaction solution is quenched with H2O and extracted with CH2Cl2, and then dried to remove the solvent. The obtained solid is purified by silica gel column chromatography to obtain compound 3, i.e., the aggregation-induced emission material.
[0012] Preferably, in step S1, the molar ratio of compound 1 to N-iodosuccinimide is 1:1 to 1:2.5.
[0013] Preferably, in step S2, the molar ratio of compound 2 to 4-(1,2,2-triphenylvinyl)phenylboronic acid is 1:2 to 1:4; and the molar ratio of tetrakis(triphenylphosphine)palladium to K2CO3 is 1:50 to 1:300.
[0014] Preferably, the reaction temperature in step S2 is 70-90° C., the reaction time is 24-48 h, and the inert gas is nitrogen or argon.
[0015] Preferably, the eluent in the column chromatography is cyclohexane / dichloromethane, and the volume ratio of cyclohexane to dichloromethane is 4 to 10:1.
[0016] Another object of the present invention is to provide application of the above-mentioned aggregation-induced emission material in microcavity laser detection.
[0017] Another object of the present invention is to provide a method for preparing a microcavity laser, comprising the following steps:
[0018] 1) Selecting a section of capillary quartz microtube, preparing a microbubble cavity with a nearly spherical structure on the capillary quartz microtube by melt blowing, wherein the microbubble cavity is a hollow structure with left and right ends open, thus obtaining a microbubble cavity device;
[0019] 2) dissolving the above-mentioned aggregation-induced emission material in a mixed solution of PBS and DMSO to obtain an aggregation-induced emission material solution for later use; the above-mentioned aggregation-induced emission material may also be an aggregation-induced emission material of other structures.
[0020] 3) fixing the two ends of one or more microbubble cavity devices prepared in step 1) on a glass slide, and then placing the glass slide on a three-dimensional adjustment frame, connecting one end of the microbubble cavity device to a spectrometer via an optical fiber, and connecting the other end to a syringe via a Teflon tube, and slowly injecting the aggregation-induced luminescence solution prepared in step 2) through the syringe until the solution fills the entire microbubble cavity and no air bubbles are left;
[0021] 4) The pump light source is adjusted to focus the output light of the pump light source into the microbubble cavity through a reflector and a focusing lens. The laser signal output from the microbubble cavity is collected and presented as a spectral signal by adjusting a certain angle by an optical fiber spectrometer, thereby obtaining the microcavity laser.
[0022] Preferably, the concentration of the aggregation-induced emission material solution is 1 mM to 10 mM.
[0023] Another object of the present invention is to provide a microcavity laser prepared by the above method.
[0024] Compared with the prior art, the present invention has the following beneficial effects:
[0025] 1. The present invention provides a novel aggregation-induced luminescence material, which introduces two tetraphenylethylene (TPE) structures into fluoroboron dipyrrole dye (BODIPY). Due to the aggregation-induced luminescence properties of the double TPE, the synthesized material has better aggregation-induced luminescence performance in solution, and the quantum yield reaches 86%, which has better properties than traditional aggregation-induced luminescence materials. The material of the present invention has good biocompatibility, high fluorescence quantum yield, and is a good choice for gain medium, thereby broadening the content of organic material micro-nano lasers in the field of materials and detection, which is of great significance.
[0026] 2. The present invention introduces aggregation-induced luminescence dye as the laser gain medium of the laser into the design of the laser with the properties of the whispering gallery. During the preparation process, the aggregation-induced luminescence material is directly injected into the homemade microbubble cavity, and the pump light is focused on the microbubble cavity by using a reflector and a focusing lens to obtain the laser spectrum. The system and method improve the energy utilization efficiency of the excitation laser, and at the same time greatly improve the laser stability, and realize a low-threshold organic dye microcavity laser. And there is no need to pull the tapered fiber to introduce the pump light, the laser is integrated with the pump system, and the device is more robust. The present invention can also realize parallel excitation of multiple microbubble cavities by adjusting the laser spot, and has the advantage of realizing multi-wavelength output. The present invention has a simple process, simpler operation, convenient replacement of organic dye solution, low production cost, and overcomes the defect of fluorescence quenching (ACQ) of traditional fluorescent materials in solid or aggregated state. At the same time, this method provides a new idea and a practical technical solution for microcavity laser technology in the field of high-sensitivity sensor research, broadens the application prospects of organic materials in micro-nano lasers, materials and detection fields, and then strongly promotes the application of organic micro-nano laser materials in chemical sensing and biology. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] Figure 1 It is the mass spectrum of the aggregation-induced emission material of the present invention.
[0028] Figure 2 It is the nuclear magnetic resonance hydrogen spectrum of the aggregation-induced emission material of the present invention.
[0029] Figure 3 It is the aggregation-induced emission characteristic of the aggregation-induced emission material of the present invention.
[0030] Figure 4 Schematic diagram of the device of the microcavity laser of the present invention.
[0031] Figure 5 FIG. 4 is a flow chart of the preparation of the microcavity device of the present invention.
[0032] Figure 6 This is a laser spectrum diagram of the microcavity laser of the present invention.
[0033] Figure 7 It is a schematic diagram of a device for multi-wavelength output of a microcavity laser of the present invention.
[0034] Figure 8 Graphs showing different laser emission spectra of multi-wavelength outputs of the microcavity laser of the present invention. DETAILED DESCRIPTION
[0035] The present invention is further described in detail below in conjunction with the examples. The experimental methods used in the following examples are conventional methods unless otherwise specified. The materials, reagents, etc. used in the following examples, unless otherwise specified, can all be obtained from commercial sources.
[0036] Example 1
[0037] A preparation process route of an aggregation-induced emission material is as follows:
[0038] S1: Compound 1 (300 mg, 0.93 mmol) and excess N-iodosuccinimide NIS (837 mg, 3.72 mmol) were dissolved in anhydrous CH2Cl2 (40 mL) solvent, and the mixture was stirred at room temperature for about 30 min and monitored by TLC until the starting material was completely consumed. After the reaction was completed, the reaction product was concentrated in vacuo and the crude product was purified by column chromatography with cyclohexane / dichloromethane (v / v) = 4:1 as eluent to obtain red solid compound 2 (450 mg, yield 84.0%).
[0039] S2: Compound 2 (310 mg, 0.69 mmol) and 4-(1,2,2-triphenylvinyl)phenylboronic acid (285 mg, 0.76 mmol) were placed in a tetrahydrofuran aqueous solvent (including 16 mL THF and 4 mL H2O), and tetrakis(triphenylphosphine)palladium (31 mg, 0.026 mmol) and K2CO3 (1.2 g, 8.6 mmol) were added in sequence to obtain a reaction solution, and then the reaction solution was placed in a nitrogen environment for reaction, heated to 80±1°C for reaction for 48 h, and after the reaction was completed, the mixed solution was quenched with H2O (20 mL) and extracted 3 times with CH2Cl2, and then the solvent was dried with anhydrous Na2SO4, and then the solvent was removed in vacuo, and the residue was purified by column chromatography with cyclohexane / dichloromethane (v / v) = 4:1 as an eluent to obtain the aggregation-induced emission material, i.e., compound 3 (232 mg, yield 50.6%).
[0040] 1. The aggregation-induced luminescence material prepared in this example was subjected to mass spectrometry and nuclear magnetic resonance hydrogen spectrum analysis. The results are as follows: Figure 1 and Figure 2 The specific data is as follows:
[0041] 1 HNMR (400MHz, CDCl3) 7.51 (s, 3H), 7.35-7.34 (m, 2H), 7.16-7.03 (m, 36H), 6.91-6.89 (d, 2H), 2.52 (s, 6H), 1.59 (s, 6H).
[0042] The molecular formula of the luminescent material obtained by the present invention is C71 H 57 BF2N2, the structural formula is as follows:
[0043]
[0044] 2. Compound 3 prepared in this example was added to a mixed solution of PBS and DMSO to a concentration of 10 μM, and then its aggregation-induced emission properties were detected by changing the ratio of PBS to DMSO solvents, wherein the volume ratios of PBS to DMSO were 1:9, 3:7, 4:6, 1:1, 2:1, 3:1, 4:1, 9:1 and 99:1, respectively. The results are as follows: Figure 3 shown.
[0045] As can be seen from the figure, under the action of 380nm excitation wavelength, the fluorescence intensity of compound 3 in the aqueous phase is significantly enhanced with the increase of the proportion of PBS in the solvent, showing typical AIE characteristics, indicating that the luminescent material of the present invention has good aggregation-induced emission performance in solution. Using the following formula, the quantum yield of the aggregation-induced material of the present invention is calculated to be 86%.
[0046] φ X =φ st (Grad X / Grad st )(η X 2 / η st 2 )
[0047] In the formula, "Φ" represents the fluorescence quantum yield, "Grad" represents the slope of the ratio of the integral of the fluorescence intensity area to the corresponding absorption value, and "η" represents the refractive index of the solution. The subscripts "st" and "X" represent the standard solution and the test solution, respectively.
[0048] Example 2
[0049] A microcavity laser based on aggregation-induced luminescence material includes a microbubble cavity device, an aggregation-induced luminescence gain material and an excitation light system. The schematic diagram of the device is shown in FIG. Figure 4 As shown, it includes a laser pump source 1, a reflector 2, an optical focusing objective lens 3, an imaging CCD 4, a microbubble cavity device 5 and a fiber optic spectrometer 6.
[0050] The method for preparing the microcavity laser based on the aggregation-induced emission material comprises the following steps:
[0051] 1) If Figure 5As shown, take a capillary quartz tube, connect one end of it to a syringe, burn off the coating layer on the surface of the capillary quartz tube with an alcohol lamp, and wipe the capillary quartz tube clean with alcohol dipped in clean paper, melt and seal the other end of the capillary quartz tube with the help of an optical fiber fusion splicer, adjust the position of the capillary quartz tube in the fusion splicer, ensure that both ends of the position where microbubbles are formed have appropriate lengths, then slowly push the syringe while discharging, until a symmetrical and rounded microbubble with a nearly spherical structure is formed at the position of the discharge, and a microbubble cavity is obtained. The two ends of the obtained microbubble cavity are connected to Teflon tubes using ultraviolet glue, which is convenient for injecting liquid. And it has good air tightness, after the Teflon tube at one end injects liquid, there is no leakage, that is, the liquid can flow smoothly from the water injection port to the water outlet, and a microbubble cavity device 5 is obtained.
[0052] 2) 0.01 g of the aggregation-induced emission solid material prepared in Example 1 was dissolved in 0.1 mL of a mixed solution of PBS and DMSO to obtain an aggregation-induced emission material solution.
[0053] 3) Fixing both ends of the microbubble cavity device 5 prepared in step 1) on a glass slide, placing the glass slide on a three-dimensional adjustment frame, connecting one end of the microbubble cavity device to a fiber optic spectrometer 6 via an optical fiber, and connecting the other end to a syringe via a Teflon tube, and then slowly injecting the aggregation-induced luminescence solution prepared in step 2) using a syringe until the solution enters and gradually fills the entire microbubble cavity, and using a microscope and CCD 4 to observe that there are no air bubbles in the entire whispering gallery microbubble cavity.
[0054] 4) The output light of the laser pump source 1 can be focused into the microbubble cavity of the microbubble cavity device through the reflector 2 and the optical focusing lens 3. The laser signal output by the microbubble cavity is collected and presented as a spectral signal by adjusting a certain angle by the optical fiber spectrometer, so as to obtain the microcavity laser.
[0055] When implementing it, Figure 4 As shown, the 532nm pulse excitation light source laser pump source 1 in the obtained microcavity laser is turned on, and the pump light is coupled into the optical focusing lens 3 through the reflector 2, and then the light spot is focused in the microbubble cavity of the microbubble cavity device 5, and the energy excited by the laser pump source 1 is adjusted so that the microfluidic microcavity laser can achieve stable output of the whispering gallery laser at a low threshold. The laser emitted from the microbubble cavity is directly collected by optical fiber by finding a certain laser emission angle, and then transmitted to the optical fiber spectrometer 6 to display the spectral information, and a section of the whispering gallery laser spectrum is obtained. The result is as shown in FIG. Figure 6 As shown. Figure 6 It can be seen that the central wavelength of the laser output by the microcavity laser in this embodiment is around 600nm and can be output stably. The microcavity laser of the present invention greatly improves the laser stability and the energy utilization efficiency of the excited laser, thus realizing a low-threshold organic dye microcavity laser.
[0056] Further, in the specific implementation, a plurality of capillary quartz tubes with microbubble cavities are prepared, as above, such as Figure 7 The microbubble cavity device 1 and the microbubble cavity device 2 are shown, and then the microbubble cavity device 1 and the microbubble cavity device 2 are arranged in parallel and their two ends are fixed on the same glass slide, 0.1 mg / ml of rhodamine B solution is injected into the microbubble cavity device 1, and 0.1 mg / ml of the aggregation-induced luminescence material solution prepared in the present invention is injected into the microbubble cavity device 2. The angle of the lens can be adjusted autonomously by the built reflector, that is, the position of the pump laser spot can be accurately regulated by adjusting the reflector, so that the regulated pump spot is focused in different microbubble cavities in the microbubble cavity device, and a certain laser emission angle is found to be directly collected by optical fiber, and then the spectrum information is transmitted to the optical fiber spectrometer to display the spectrum information, and the echo gallery laser spectrum is obtained. The result is as shown Figure 8 As shown, this embodiment simultaneously obtains two different laser emission spectra ( Figure 8 A is the spectrum of Rhodamine B. Figure 8 B is the spectrum of compound 3), and the laser intensity generated by the aggregation-induced luminescence material of the present invention has obvious advantages, indicating that the present invention can conveniently and quickly realize simultaneous excitation of multiple materials and simultaneous output of multiple wavelengths.
[0057] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. An aggregation-induced emission material, characterized in that: The structural formula of the luminescent material is as follows:
2. A method for preparing the aggregation-induced emission material according to claim 1, characterized in that: Its synthetic route is as follows: The following steps are involved: S1: Compound 1 and N-iodosuccinimide are dissolved in CH2Cl2 solvent, and then the reaction solution is stirred at room temperature until the raw material is completely consumed as monitored by TLC analysis. After the reaction is completed, it is vacuum concentrated, and the obtained solid is separated by column chromatography to obtain a red intermediate compound 2; S2: The intermediate compound 2 and 4-(1,2,2-triphenylvinyl)phenylboronic acid are placed in a tetrahydrofuran aqueous solvent, and tetrakis(triphenylphosphine)palladium and K2CO3 are added in sequence to obtain a reaction solution, and then the reaction solution is placed in an inert gas environment for reaction and stirred overnight. After the reaction is completed, the reaction solution is quenched with H2O and extracted with CH2Cl2, and then dried to remove the solvent. The obtained solid is purified by silica gel column chromatography to obtain the aggregation-induced emission material.
3. The method for preparing the aggregation-induced emission material according to claim 2, characterized in that: The molar ratio of compound 1 to N-iodosuccinimide in step S1 is 1:1 to 1:2.
5.
4. The method for preparing the aggregation-induced emission material according to claim 2, characterized in that: In step S2, the molar ratio of compound 2 to 4-(1,2,2-triphenylvinyl)phenylboronic acid is 1:2 to 1:4; the molar ratio of tetrakis(triphenylphosphine)palladium to K2CO3 is 1:50 to 1:
300.
5. The method for preparing the aggregation-induced emission material according to claim 2, characterized in that: The reaction temperature in step S2 is 70-90° C., and the reaction time is 24-48 hours; the inert gas is nitrogen or argon.
6. The method for preparing the aggregation-induced emission material according to claim 2, characterized in that: The eluent in the column chromatography is cyclohexane / dichloromethane, and the volume ratio of cyclohexane to dichloromethane is 4-10:
1.
7. Use of the aggregation-induced emission material according to claim 1 or the aggregation-induced emission material prepared by the method according to any one of claims 2 to 6 in microcavity laser detection.
8. A method for preparing a microcavity laser, characterized in that: The following steps are involved: 1) Selecting a section of capillary quartz microtube, preparing a microbubble cavity with a nearly spherical structure on the capillary quartz microtube by melt blowing, wherein the microbubble cavity is a hollow structure with left and right ends open, thus obtaining a microbubble cavity device; 2) dissolving the aggregation-induced emission material according to claim 1 in a mixed solution of PBS and DMSO to obtain an aggregation-induced emission material solution for later use; 3) fixing both ends of one or more microbubble cavity devices prepared in step 1) on a glass slide, then placing the glass slide on a three-dimensional adjustment frame, connecting one end of the microbubble cavity device to a syringe through a Teflon tube, and slowly injecting the aggregation-induced luminescence solution prepared in step 2) through the syringe until the solution fills the entire microbubble cavity and no air bubbles are left; 4) The pump light source is adjusted to focus the output light of the pump light source into the microbubble cavity of the microbubble cavity device through a reflector and a focusing lens. The laser signal output by the microbubble cavity is collected by a fiber spectrometer and presents a spectral signal, thus obtaining the microcavity laser.
9. The method for preparing a microcavity laser according to claim 8, characterized in that: The concentration of the aggregation-induced emission material solution is 1 mM to 10 mM.
10. A microcavity laser prepared by the method of claim 8 or 9.
Citation Information
Patent Citations
Extreme-small fabry-perot type microcavity fluid laser
CN106785849A
Micro-cavity quantum dot laser prepared by capillary force driving and preparation method thereof
CN108832473A
Fabry-Perot microcavity sensing chip, preparation method thereof and molecular detection system
CN115015170A
Immunodetection reagent based on AIE magnetic coding microspheres and AIE nanometer microspheres as well as preparation method and application of immunodetection reagent