Hydrogel for oral periodontitis and preparation method thereof

The problem of insufficient antibacterial and adhesion in oral periodontitis is solved by using antibacterial wet adhesion hydrogel composed of quaternary ammonium derivative QTA, methacrylated gelatin and modified γ-polyglutamic acid, and the problem of insufficient antibacterial and adhesion in oral periodontitis is achieved. Broad-spectrum killing and chronic wound healing effects on Gramella.

CN119019474APending Publication Date: 2024-11-26HANGZHOU INST OF ADVANCED MATERIAL BEIJING UNIV OF CHEM TECH +1
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202411221105.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-02
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

Existing methods for treating oral periodontitis are difficult to alleviate inflammatory response and repair periodontal tissue damage, and hydrogel dressings are difficult to effectively antibacterial and adhere to oral environments with moist and irregular shapes.

Method used

Antibacterial wet adhesion hydrogel consisting of quaternary ammonium derivative QTA, methacrylated gelatin and N-hydroxysuccinimide modified γ-polyglutamic acid to form broad-spectrum antibacterial and Highly adhesion dressing.

Benefits of technology

This hydrogel has a killing effect on both Gram-negative and positive bacteria. It promotes chronic wound healing through antibacterial, anti-inflammatory and removal of reactive oxygen species. It has the ability to adhere wet in humid environments and is suitable for oral periodontitis and other disease.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119019474A_ABST
    Figure CN119019474A_ABST
Patent Text Reader

Abstract

The invention provides hydrogel for oral periodontitis and a preparation method of the hydrogel. The hydrogel is prepared from the following raw materials: QTA, methacrylated gelatin and N-hydroxysuccinimide modified gamma-polyglutamic acid. The structure of the compound QTA is as follows: # imgabs0 #. The invention also provides a preparation method of the antibacterial wet adhesion hydrogel. The invention also provides application of the compound QTA or the antibacterial wet adhesion hydrogel in preparation of oral periodontitis drugs or antibacterial drugs. The compound QTA and the antibacterial wet adhesion hydrogel have broad-spectrum antibacterial property and have wet adhesion capacity on a water-containing surface.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of medical dressings, and in particular to a hydrogel for oral periodontitis and a preparation method thereof. Background Art

[0002] Oral periodontitis is a chronic inflammatory disease caused by dental plaque. The bacteria in dental plaque damage the periodontal tissue, causing it to be in an inflammatory response stage for a long time. Excessive accumulation of substances such as reactive oxygen and matrix metalloproteinases leads to symptoms such as gingival redness and swelling, alveolar bone absorption, and even tooth loss. The current treatment methods are mainly surgical mechanical debridement and antibiotic treatment, but these methods are difficult to reduce excessive inflammatory responses and repair periodontal tissue damage, and cannot provide continuous treatment for wounds. In comparison, hydrogel dressings show unique advantages in antibacterial and anti-inflammatory effects and continuous effects. The internal environment of the oral cavity is different from the skin surface. It is highly humid, dynamic, weakly acidic, and has irregular wound shapes. This requires the dressing to have strong wet adhesion and mechanical properties that can adapt to irregular shapes, which puts higher requirements on the material preparation of hydrogels.

[0003] In order to deal with the harm caused by microbial infections such as bacteria and fungi to human life and health, various antimicrobial agents are widely used. The antimicrobial agents used today are mainly divided into three categories: inorganic antimicrobial agents, organic antimicrobial agents, and natural antimicrobial agents. Quaternary ammonium salt antimicrobial agents are organic antimicrobial agents and also cationic surfactants. Their positively charged quaternary ammonium ions can attract the negatively charged bacterial cell wall surface, change the permeability of the cell membrane, and cause the intracellular solution to flow out, resulting in bacterial death. This antibacterial mechanism of quaternary ammonium salts makes them broad-spectrum bactericidal, and they have obvious effects on both Gram-negative and Gram-positive bacteria.

[0004] Tannic acid, also known as tannic acid, is a polyphenol polymer extracted from plants. It is widely used in the biomedical field due to its good antibacterial, antioxidant and anti-inflammatory effects. The pyrogallol structure it contains gives tannic acid a high reactivity, which destroys the bacterial structure by reacting with proteins, polysaccharides and lipids on the surface of bacteria, affecting the activity of enzymes in bacteria and achieving antibacterial effects. In addition, as an additive to hydrogels, the dense phenolic hydroxyl groups in tannic acid can also form a large number of hydrogen bonds with human tissues to improve the adhesion of hydrogel dressings, thereby improving the performance of dressings in many ways.

[0005] γ-Polyglutamic acid is a polyamino acid with glutamic acid as a monomer, which contains abundant free carboxyl groups. N-hydroxysuccinimide, as a commonly used acylating agent, has good biocompatibility and reactivity. It combines with the carboxyl groups in polyglutamic acid to form NHS-activated ester groups, which can be used as a cross-linking agent to react with the amino groups in gelatin to form covalent cross-links. Different from traditional cross-linking agents such as glutaraldehyde, γ-PGA-NHS has excellent biocompatibility, degradability, and low toxicity. In addition to the cross-linking effect, the unreacted free carboxyl groups and NHS-activated ester groups in γ-PGA can also undergo covalent and non-covalent interactions with amino groups, thiol groups and other groups in human tissues, thereby enhancing the adhesion of the hydrogel. Summary of the invention

[0006] In order to solve at least one of the above technical problems, in a first aspect of the present application, the present application provides a compound QTA, the structure of the compound QTA is as follows: .

[0007] In a second aspect of the present application, the present application provides a method for preparing the above-mentioned compound QTA, wherein QTA is prepared from QAS and tannic acid, and the reaction formula for preparing QTA from QAS and tannic acid is as follows: .

[0008] Preferably, QAS and tannic acid are used to prepare the compound QTA, comprising the following steps: mixing QAS and tannic acid, adding a catalyst and a solvent, reacting under the protection of an inert gas, adding deionized water to generate a precipitate after the reaction is complete, standing, washing the precipitate, filtering, collecting the filter cake, and freeze-drying to obtain the compound QTA.

[0009] Preferably, the molar ratio of the QAS to tannic acid is 2:(0.1-0.2); the catalyst is potassium carbonate, and the solvent is DMF.

[0010] Preferably, the compound QAS is prepared from dimethylaminoethyl methacrylate and 1,6-dibromohexane, and the preparation of QAS from dimethylaminoethyl methacrylate and 1,6-dibromohexane includes the following steps: adding dimethylaminoethyl methacrylate to 1,6-dibromohexane, reacting, and after the reaction is complete, taking out the liquid, adding acetonitrile to the colloid, stirring to form a suspension, centrifuging to obtain a precipitate, washing, and drying to obtain the compound QAS; the molar ratio of the dimethylaminoethyl methacrylate to 1,6-dibromohexane is 1:(2~5).

[0011] In the third aspect of the present application, the present application provides a hydrogel for oral periodontitis, wherein the raw materials of the antibacterial wet adhesion hydrogel include the compound QTA according to claim 1, methacrylated gelatin, and N-hydroxysuccinimide-modified γ-polyglutamic acid.

[0012] Preferably, the mass ratio of QTA, methacryloyl gelatin, and N-hydroxysuccinimide-modified γ-polyglutamic acid is 2: (10-15): (5-10).

[0013] In a fourth aspect of the present application, the present application provides a method for preparing the hydrogel according to the third aspect of the present invention, comprising the following steps: Step 1): prepare an aqueous solution of methacryloyl gelatin, add compound QTA, and disperse evenly; Step 2): Adjust the pH to 8.5-9.5, and add N-hydroxysuccinimide modified γ-polyglutamic acid solution; Step 3): Add a photoinitiator, polymerize, and irradiate with 405nm blue light to form a gel, thereby obtaining the antibacterial wet adhesion hydrogel.

[0014] Preferably, in the step 1), the concentration of methacrylylated gelatin in the aqueous solution of methacrylylated gelatin is 10wt%~15wt%; in the step 2), the concentration of N-hydroxysuccinimide-modified γ-polyglutamic acid solution is 5wt%~10wt%.

[0015] In the fifth aspect of the present application, the present application provides a use of the compound QTA described in the first aspect of the present application or the hydrogel described in the third aspect of the present application in the preparation of periodontitis drugs or antibacterial drugs.

[0016] The bacteria is Staphylococcus aureus or Escherichia coli.

[0017] In summary, the present invention includes at least one of the following beneficial technical effects: 1. The hydrogel of the present invention has a broad-spectrum antibacterial property and has a killing effect on both Gram-negative bacteria represented by Escherichia coli and Gram-positive bacteria represented by Staphylococcus aureus.

[0018] 2. The hydrogel described in the present invention can promote the healing of chronic wounds by means of antibacterial, anti-inflammatory and active oxygen scavenging, and has the ability of wet adhesion on water-containing surfaces. It can be used for the healing of chronic wounds caused by bacterial infection and accompanied by persistent inflammatory response in a humid environment, such as oral diseases such as oral periodontitis. BRIEF DESCRIPTION OF THE DRAWINGS

[0019] Figure 1 is the reaction formula for synthesizing QTA from QAS and TA in Example 1; Figure 2The infrared spectra of TA, QAS and QTA in the synthesis process of Example 1; Figure 3 is the hydrogen nuclear magnetic resonance spectrum of QAS in Example 1; Figure 4 is the hydrogen nuclear magnetic resonance spectrum of QTA in Example 1; Figure 5 This is a photograph of the adhesion ability of the antibacterial wet adhesion hydrogel in Example 1; Figure 6 The antibacterial properties of the antibacterial wet adhesion hydrogel in Comparative Example 1 and Example 1 against Staphylococcus aureus and Escherichia coli. DETAILED DESCRIPTION

[0020] The present invention will be further described below in conjunction with specific examples and accompanying drawings, but the following examples are only used to illustrate the present invention and should not be considered to limit the scope of the present invention. In the following examples, if specific conditions are not specified, they are carried out according to normal conditions or conditions recommended by the manufacturer. The methods used are conventional methods known in the art unless otherwise specified, and the consumables and reagents used are commercially available unless otherwise specified. Unless otherwise specified, the professional and scientific terms used herein have the same meaning as those familiar to those skilled in the art. In addition, any method or material similar or equivalent to the recorded content may also be applied to the present invention. Example 1

[0021] (1) Preparation of quaternary ammonium salts (QAS) containing double bonds ① Slowly drop 2 mmol DMAEMA (dimethylaminoethyl methacrylate) into 10 mmol 1,6-dibromohexane; ② Stir the reaction at room temperature for 24 hours; ③ After the reaction is completed, discard the unreacted liquid, add acetonitrile to the remaining colloidal substance, and stir vigorously to form a suspension; ④ The suspension is centrifuged at 7000 rpm for 5 min to obtain a precipitate, and the precipitate is washed with excess acetonitrile and centrifuged, and repeated several times; ⑤ The precipitate is vacuum dried at 50°C for 24 hours to obtain QAS.

[0022] The structural formula of QAS is shown below: .

[0023] The H NMR spectrum of QAS is as follows Figure 3 The hydrogen with chemical shifts of 6.08 ppm and 5.75 ppm corresponds to the two hydrogen atoms at one end of the carbon-carbon double bond, 3.13 ppm is the hydrogen atom on the two methyl groups in the quaternary ammonium group, and 1.60-2.00 ppm of hydrogen comes from the methylene group in dibromohexane.

[0024] (2) Preparation of quaternary ammonium tannic acid (QTA) containing double bonds The reaction formula for preparing QTA is as follows Figure 1As shown, the specific steps are as follows: ① Mix 2 mmol QAS with 0.1 mmol tannic acid, add anhydrous potassium carbonate (2 mmol, 0.28 g) as a catalyst, and add 20 mL DMF as a solvent for every 1 g tannic acid; ② Fill with nitrogen protection, stir and react at 85°C for 12 hours; ③ Drop the reaction solution into excess deionized water to produce precipitation, and remove the supernatant after standing for 15 minutes; ④ Add DMF to the precipitate to dissolve, then add excess deionized water to precipitate, and repeat several times; ⑤ Filter the suspension, collect the filter cake, and freeze-dry it for 48 hours to obtain the product QTA.

[0025] The structure of a QTA is as follows: .

[0026] The infrared spectra of TA, QAS and QTA during the synthesis of Example 1 are as follows: Figure 2 As shown. QAS is at 2925cm -1 The peak at 1635 cm is the stretching vibration peak of the carbon-hydrogen bond on the methylene group. -1 The peak at 952 cm is the stretching vibration peak of the carbon-carbon double bond. -1 The above three absorption peaks prove the successful synthesis of QAS. -1 The broad peak near 573 cm is the stretching vibration peak of the hydroxyl group, which is consistent with tannic acid. -1 The characteristic peak of the carbon-bromine bond at 400 nm disappeared in QTA, indicating that the reaction between tannic acid and QAS removed the terminal bromine, proving the successful preparation of QTA.

[0027] The H NMR spectrum of QTA is as follows Figure 4 The multiple peaks near 7.0 ppm correspond to the hydrogen on the phenolic hydroxyl group in the pyrogallol structure, while 6.05 ppm, 5.71 ppm, and 3.00 ppm are consistent with the hydrogen atoms at the corresponding positions in QAS, proving that tannic acid successfully reacts with QAS to generate QTA.

[0028] (3) Preparation of γ-PGA-NHS (N-hydroxysuccinimide-modified γ-polyglutamic acid) ① Dissolve 1g γ-PGA (γ-polyglutamic acid) and 0.85g NHS (N-hydroxysuccinimide) in 20mL DMSO, and add EDC (1-ethyl-(3-dimethylaminopropyl) carbodiimide) in a molar ratio of 1:1 to NHS; ② The solution is stirred and reacted for 20 hours at room temperature under nitrogen protection; ③ After the reaction, a mixed solution of methanol and ethanol in a volume ratio of 1:3 is added to the solution to produce a precipitate; ④ After filtration, the precipitate is washed several times with ethanol and n-hexane; ⑤ The precipitate is vacuum dried at room temperature for 24 hours to obtain the product γ-PGA-NHS.

[0029] (4) Preparation of antibacterial wet adhesion hydrogel ① Prepare 10 mL of 10 wt% GelMA (methacryloyl gelatin) aqueous solution at room temperature, add 0.2 g QTA, and disperse it evenly in the solution by ultrasound; ② Adjust the pH of the solution to 9 with NaOH solution (1 mol / L), and add 0.5 g of the γ-PGA-NHS solid prepared above; ③ Add 2 mL of 1 mol / L photoinitiator LAP (phenyl-2,4,6-trimethylbenzoyl lithium phosphite), and stir at 20 ° C for prepolymerization; ④ Use 405 nm blue light to irradiate for 10 min to form a gel.

[0030] Figure 5 The following are photos of the adhesion of the antibacterial wet adhesion hydrogel prepared in Example 1 to pig skin and glass bottles in a dry environment and to pig skin in water. The adhesion performance of the hydrogel is mainly provided by the large number of phenolic hydroxyl groups in the tannic acid structure, and the unreacted free carboxyl groups and NHS activated ester groups in γ-PGA can also interact covalently and non-covalently with amino groups, sulfhydryl groups and other groups in biological tissues to enhance adhesion. In a humid environment, the hydrophobic carbon chain in the quaternary ammonium salt can push away the hydration layer between the contact surfaces, so that the antibacterial wet adhesion hydrogel has wet adhesion ability. Example 2

[0031] (1) Preparation of quaternary ammonium salts (QAS) containing double bonds ① Slowly drop 2 mmol DMAEMA into 10 mmol 1,6-dibromohexane; ② Stir the reaction at room temperature for 24 hours; ③ After the reaction is completed, discard the unreacted liquid, add acetonitrile to the remaining colloidal substance, and stir vigorously to form a suspension; ④ The suspension is centrifuged at 7000 rpm for 5 min to obtain a precipitate, and the precipitate is washed with excess acetonitrile and centrifuged, and repeated several times; ⑤ The precipitate is vacuum dried at 50°C for 24 hours to obtain QAS.

[0032] (2) Preparation of quaternary ammonium tannic acid (QTA) containing double bonds ① Mix 2 mmol QAS with 0.1 mmol tannic acid, add anhydrous potassium carbonate (2 mmol, 0.28 g) as a catalyst, and add 20 mL DMF as a solvent for every 1 g tannic acid; ② Fill with nitrogen protection, stir and react at 85°C for 12 hours; ③ Drop the reaction solution into excess deionized water to produce precipitation, and remove the supernatant after standing for 15 minutes; ④ Add DMF to the precipitate to dissolve, then add excess deionized water to precipitate, and repeat several times; ⑤ Filter the suspension, collect the filter cake, and freeze-dry it for 48 hours to obtain the product QTA.

[0033] (3) Preparation of γ-PGA-NHS ① Dissolve 1g γ-PGA and 0.85g NHS in 20mL DMSO, and add EDC in a molar ratio of 1:1 to NHS; ② The solution is stirred and reacted for 20 hours at room temperature under nitrogen protection; ③ After the reaction, a mixed solution of methanol and ethanol in a volume ratio of 1:3 is added to the solution to produce a precipitate; ④ After filtration, the precipitate is washed several times with ethanol and n-hexane; ⑤ The precipitate is vacuum dried at room temperature for 24 hours to obtain the product γ-PGA-NHS.

[0034] (4) Preparation of antibacterial wet adhesion hydrogel ① Prepare 10 mL of 10 wt% GelMA aqueous solution at room temperature, add 0.2 g QTA, and disperse it evenly in the solution by ultrasound; ② Adjust the pH of the solution to 9 with NaOH (1 mol / L), and add 1 g of the γ-PGA-NHS solid prepared above; ③ Add 2 mL of 1 mol / L photoinitiator LAP, and stir at 20 °C for prepolymerization; ④ Irradiate with 405 nm blue light for 10 min to form a gel. Example 3

[0035] (1) Preparation of quaternary ammonium salts (QAS) containing double bonds ① Slowly drop 2 mmol DMAEMA into 10 mmol 1,6-dibromohexane; ② Stir the reaction at room temperature for 24 hours; ③ After the reaction is completed, discard the unreacted liquid, add acetonitrile to the remaining colloidal substance, and stir vigorously to form a suspension; ④ The suspension is centrifuged at 7000 rpm for 5 min to obtain a precipitate, and the precipitate is washed with excess acetonitrile and centrifuged, and repeated several times; ⑤ The precipitate is vacuum dried at 50°C for 24 hours to obtain QAS.

[0036] (2) Preparation of quaternary ammonium tannic acid (QTA) containing double bonds ① Mix 2 mmol QAS with 0.1 mmol tannic acid, add anhydrous potassium carbonate (2 mmol, 0.28 g) as a catalyst, and add 20 mL DMF as a solvent for every 1 g tannic acid; ② Fill with nitrogen protection, stir and react at 85°C for 12 hours; ③ Drop the reaction solution into excess deionized water to produce precipitation, and remove the supernatant after standing for 15 minutes; ④ Add DMF to the precipitate to dissolve, then add excess deionized water to precipitate, and repeat several times; ⑤ Filter the suspension, collect the filter cake, and freeze-dry it for 48 hours to obtain the product QTA.

[0037] (3) Preparation of γ-PGA-NHS ① Dissolve 1g γ-PGA and 0.85g NHS in 20mL DMSO, and add EDC in a molar ratio of 1:1 to NHS; ② The solution is stirred and reacted for 20 hours at room temperature under nitrogen protection; ③ After the reaction, a mixed solution of methanol and ethanol in a volume ratio of 1:3 is added to the solution to produce a precipitate; ④ After filtration, the precipitate is washed several times with ethanol and n-hexane; ⑤ The precipitate is vacuum dried at room temperature for 24 hours to obtain the product γ-PGA-NHS.

[0038] (4) Preparation of antibacterial wet adhesion hydrogel ① Prepare 10 mL of 15 wt% GelMA aqueous solution at room temperature, add 0.2 g QTA, and disperse it evenly in the solution by ultrasound; ② Adjust the pH of the solution to 9 with NaOH (1 mol / L), and add 0.5 g of the γ-PGA-NHS solid prepared above; ③ Add 2 mL of 1 mol / L photoinitiator LAP, and stir at 20 °C for prepolymerization; ④ Use 405 nm blue light to irradiate for 10 min to form a gel. Example 4

[0039] (1) Preparation of quaternary ammonium salts (QAS) containing double bonds ① Slowly drop 2 mmol DMAEMA into 10 mmol 1,6-dibromohexane; ② Stir the reaction at room temperature for 24 hours; ③ After the reaction is completed, discard the unreacted liquid, add acetonitrile to the remaining colloidal substance, and stir vigorously to form a suspension; ④ The suspension is centrifuged at 7000 rpm for 5 min to obtain a precipitate, and the precipitate is washed with excess acetonitrile and centrifuged, and repeated several times; ⑤ The precipitate is vacuum dried at 50°C for 24 hours to obtain QAS.

[0040] (2) Preparation of quaternary ammonium tannic acid (QTA) containing double bonds ① Mix 2 mmol QAS with 0.1 mmol tannic acid, add anhydrous potassium carbonate (2 mmol, 0.28 g) as a catalyst, and add 20 mL DMF as a solvent for every 1 g tannic acid; ② Fill with nitrogen protection, stir and react at 85°C for 12 hours; ③ Drop the reaction solution into excess deionized water to produce precipitation, and remove the supernatant after standing for 15 minutes; ④ Add DMF to the precipitate to dissolve, then add excess deionized water to precipitate, and repeat several times; ⑤ Filter the suspension, collect the filter cake, and freeze-dry it for 48 hours to obtain the product QTA.

[0041] (3) Preparation of γ-PGA-NHS ① Dissolve 1g γ-PGA and 0.85g NHS in 20mL DMSO, and add EDC in a molar ratio of 1:1 to NHS; ② The solution is stirred and reacted for 20 hours at room temperature under nitrogen protection; ③ After the reaction, a mixed solution of methanol and ethanol in a volume ratio of 1:3 is added to the solution to produce a precipitate; ④ After filtration, the precipitate is washed several times with ethanol and n-hexane; ⑤ The precipitate is vacuum dried at room temperature for 24 hours to obtain the product γ-PGA-NHS.

[0042] (4) Preparation of antibacterial wet adhesion hydrogel ① Prepare 10 mL of 15 wt% GelMA aqueous solution at room temperature, add 0.2 g QTA, and disperse it evenly in the solution by ultrasound; ② Adjust the pH of the solution to 9 with NaOH (1 mol / L), and add 1 g of the γ-PGA-NHS solid prepared above; ③ Add 2 mL of 1 mol / L photoinitiator LAP, and stir at 20 °C for prepolymerization; ④ Irradiate with 405 nm blue light for 10 min to form a gel. Example 5

[0043] (1) Preparation of quaternary ammonium salts (QAS) containing double bonds ① Slowly drop 2 mmol DMAEMA into 10 mmol 1,6-dibromohexane; ② Stir the reaction at room temperature for 24 hours; ③ After the reaction is completed, discard the unreacted liquid, add acetonitrile to the remaining colloidal substance, and stir vigorously to form a suspension; ④ The suspension is centrifuged at 7000 rpm for 5 min to obtain a precipitate, and the precipitate is washed with excess acetonitrile and centrifuged, and repeated several times; ⑤ The precipitate is vacuum dried at 50°C for 24 hours to obtain QAS.

[0044] (2) Preparation of quaternary ammonium tannic acid (QTA) containing double bonds ① Mix 2 mmol QAS with 0.2 mmol tannic acid, add anhydrous potassium carbonate (2 mmol, 0.28 g) as a catalyst, and add 20 mL DMF as a solvent for every 1 g tannic acid; ② Fill with nitrogen protection, stir and react at 85°C for 12 hours; ③ Drop the reaction solution into excess deionized water to produce precipitation, and remove the supernatant after standing for 15 minutes; ④ Add DMF to the precipitate to dissolve, then add excess deionized water to precipitate, and repeat several times; ⑤ Filter the suspension, collect the filter cake, and freeze-dry it for 48 hours to obtain the product QTA.

[0045] (3) Preparation of γ-PGA-NHS ① Dissolve 1g γ-PGA and 0.85g NHS in 20mL DMSO, and add EDC in a molar ratio of 1:1 to NHS; ② The solution is stirred and reacted for 20 hours at room temperature under nitrogen protection; ③ After the reaction, a mixed solution of methanol and ethanol in a volume ratio of 1:3 is added to the solution to produce a precipitate; ④ After filtration, the precipitate is washed several times with ethanol and n-hexane; ⑤ The precipitate is vacuum dried at room temperature for 24 hours to obtain the product γ-PGA-NHS.

[0046] (4) Preparation of antibacterial wet adhesion hydrogel ① Prepare 10 mL of 10 wt% GelMA aqueous solution at room temperature, add 0.2 g QTA, and disperse it evenly in the solution by ultrasound; ② Adjust the pH of the solution to 9 with NaOH (1 mol / L), and add 0.5 g of the γ-PGA-NHS solid prepared above; ③ Add 2 mL of 1 mol / L photoinitiator LAP, and stir at 20 °C for prepolymerization; ④ Irradiate with 405 nm blue light for 10 min to form a gel. Example 6

[0047] (1) Preparation of quaternary ammonium salts (QAS) containing double bonds ① Slowly drop 2 mmol DMAEMA into 10 mmol 1,6-dibromohexane; ② Stir the reaction at room temperature for 24 hours; ③ After the reaction is completed, discard the unreacted liquid, add acetonitrile to the remaining colloidal substance, and stir vigorously to form a suspension; ④ The suspension is centrifuged at 7000 rpm for 5 min to obtain a precipitate, and the precipitate is washed with excess acetonitrile and centrifuged, and repeated several times; ⑤ The precipitate is vacuum dried at 50°C for 24 hours to obtain QAS.

[0048] (2) Preparation of quaternary ammonium tannic acid (QTA) containing double bonds ① Mix 2 mmol QAS with 0.2 mmol tannic acid, add anhydrous potassium carbonate (2 mmol, 0.28 g) as a catalyst, and add 20 mL DMF as a solvent for every 1 g tannic acid; ② Fill with nitrogen protection, stir and react at 85°C for 12 hours; ③ Drop the reaction solution into excess deionized water to produce precipitation, and remove the supernatant after standing for 15 minutes; ④ Add DMF to the precipitate to dissolve, then add excess deionized water to precipitate, and repeat several times; ⑤ Filter the suspension, collect the filter cake, and freeze-dry it for 48 hours to obtain the product QTA.

[0049] (3) Preparation of γ-PGA-NHS ① Dissolve 1g γ-PGA and 0.85g NHS in 20mL DMSO, and add EDC in a molar ratio of 1:1 to NHS; ② The solution is stirred and reacted for 20 hours at room temperature under nitrogen protection; ③ After the reaction, a mixed solution of methanol and ethanol in a volume ratio of 1:3 is added to the solution to produce a precipitate; ④ After filtration, the precipitate is washed several times with ethanol and n-hexane; ⑤ The precipitate is vacuum dried at room temperature for 24 hours to obtain the product γ-PGA-NHS.

[0050] (4) Preparation of antibacterial wet adhesion hydrogel ① Prepare 10 mL of 10 wt% GelMA aqueous solution at room temperature, add 0.2 g QTA, and disperse it evenly in the solution by ultrasound; ② Adjust the pH of the solution to 9 with NaOH (1 mol / L), and add 1 g of the γ-PGA-NHS solid prepared above; ③ Add 2 mL of 1 mol / L photoinitiator LAP, and stir at 20 °C for prepolymerization; ④ Irradiate with 405 nm blue light for 10 min to form a gel. Example 7

[0051] (1) Preparation of quaternary ammonium salts (QAS) containing double bonds ① Slowly drop 2 mmol DMAEMA into 10 mmol 1,6-dibromohexane; ② Stir the reaction at room temperature for 24 hours; ③ After the reaction is completed, discard the unreacted liquid, add acetonitrile to the remaining colloidal substance, and stir vigorously to form a suspension; ④ The suspension is centrifuged at 7000 rpm for 5 min to obtain a precipitate, and the precipitate is washed with excess acetonitrile and centrifuged, and repeated several times; ⑤ The precipitate is vacuum dried at 50°C for 24 hours to obtain QAS.

[0052] (2) Preparation of quaternary ammonium tannic acid (QTA) containing double bonds ① Mix 2 mmol QAS with 0.2 mmol tannic acid, add anhydrous potassium carbonate (2 mmol, 0.28 g) as a catalyst, and add 20 mL DMF as a solvent for every 1 g tannic acid; ② Fill with nitrogen protection, stir and react at 85°C for 12 hours; ③ Drop the reaction solution into excess deionized water to produce precipitation, and remove the supernatant after standing for 15 minutes; ④ Add DMF to the precipitate to dissolve, then add excess deionized water to precipitate, and repeat several times; ⑤ Filter the suspension, collect the filter cake, and freeze-dry it for 48 hours to obtain the product QTA.

[0053] (3) Preparation of γ-PGA-NHS ① Dissolve 1g γ-PGA and 0.85g NHS in 20mL DMSO, and add EDC in a molar ratio of 1:1 to NHS; ② The solution is stirred and reacted for 20 hours at room temperature under nitrogen protection; ③ After the reaction, a mixed solution of methanol and ethanol in a volume ratio of 1:3 is added to the solution to produce a precipitate; ④ After filtration, the precipitate is washed several times with ethanol and n-hexane; ⑤ The precipitate is vacuum dried at room temperature for 24 hours to obtain the product γ-PGA-NHS.

[0054] (4) Preparation of antibacterial wet adhesion hydrogel ① Prepare 10 mL of 15 wt% GelMA aqueous solution at room temperature, add 0.2 g QTA, and disperse it evenly in the solution by ultrasound; ② Adjust the pH of the solution to 9 with NaOH (1 mol / L), and add 0.5 g of the γ-PGA-NHS solid prepared above; ③ Add 2 mL of 1 mol / L photoinitiator LAP, and stir at 20 °C for prepolymerization; ④ Use 405 nm blue light to irradiate for 10 min to form a gel. Example 8

[0055] (1) Preparation of quaternary ammonium salts (QAS) containing double bonds ① Slowly drop 2 mmol DMAEMA into 10 mmol 1,6-dibromohexane; ② Stir the reaction at room temperature for 24 hours; ③ After the reaction is completed, discard the unreacted liquid, add acetonitrile to the remaining colloidal substance, and stir vigorously to form a suspension; ④ The suspension is centrifuged at 7000 rpm for 5 min to obtain a precipitate, and the precipitate is washed with excess acetonitrile and centrifuged, and repeated several times; ⑤ The precipitate is vacuum dried at 50°C for 24 hours to obtain QAS.

[0056] (2) Preparation of quaternary ammonium tannic acid (QTA) containing double bonds ① Mix 2 mmol QAS with 0.2 mmol tannic acid, add anhydrous potassium carbonate (2 mmol, 0.28 g) as a catalyst, and add 20 mL DMF as a solvent for every 1 g tannic acid; ② Fill with nitrogen protection, stir and react at 85°C for 12 hours; ③ Drop the reaction solution into excess deionized water to produce precipitation, and remove the supernatant after standing for 15 minutes; ④ Add DMF to the precipitate to dissolve, then add excess deionized water to precipitate, and repeat several times; ⑤ Filter the suspension, collect the filter cake, and freeze-dry it for 48 hours to obtain the product QTA.

[0057] (3) Preparation of γ-PGA-NHS ① Dissolve 1g γ-PGA and 0.85g NHS in 20mL DMSO, and add EDC in a molar ratio of 1:1 to NHS; ② The solution is stirred and reacted for 20 hours at room temperature under nitrogen protection; ③ After the reaction, a mixed solution of methanol and ethanol in a volume ratio of 1:3 is added to the solution to produce a precipitate; ④ After filtration, the precipitate is washed several times with ethanol and n-hexane; ⑤ The precipitate is vacuum dried at room temperature for 24 hours to obtain the product γ-PGA-NHS.

[0058] (4) Preparation of antibacterial wet adhesion hydrogel ① Prepare 10 mL of 15 wt% GelMA aqueous solution at room temperature, add 0.2 g QTA, and disperse it evenly in the solution by ultrasound; ② Adjust the pH of the solution to 9 with NaOH (1 mol / L), and add 1 g of the γ-PGA-NHS solid prepared above; ③ Add 2 mL of 1 mol / L photoinitiator LAP, and stir at 20 °C for prepolymerization; ④ Irradiate with 405 nm blue light for 10 min to form a gel. Comparative Example 1

[0059] (1) Preparation of quaternary ammonium salts (QAS) containing double bonds ① Slowly drop 2 mmol DMAEMA into 10 mmol 1,6-dibromohexane; ② Stir the reaction at room temperature for 24 hours; ③ After the reaction is completed, discard the unreacted liquid, add acetonitrile to the remaining colloidal substance, and stir vigorously to form a suspension; ④ The suspension is centrifuged at 7000 rpm for 5 min to obtain a precipitate, and the precipitate is washed with excess acetonitrile and centrifuged, and repeated several times; ⑤ The precipitate is vacuum dried at 50°C for 24 hours to obtain QAS.

[0060] (2) Preparation of γ-PGA-NHS ① Dissolve 1g γ-PGA and 0.85g NHS in 20mL DMSO, and add EDC in a molar ratio of 1:1 to NHS; ② The solution is stirred and reacted for 20 hours at room temperature under nitrogen protection; ③ After the reaction, a mixed solution of methanol and ethanol in a volume ratio of 1:3 is added to the solution to produce a precipitate; ④ After filtration, the precipitate is washed several times with ethanol and n-hexane; ⑤ The precipitate is vacuum dried at room temperature for 24 hours to obtain the product γ-PGA-NHS.

[0061] (3) Preparation of antibacterial wet adhesion hydrogel ① Prepare 10 mL of 10 wt% GelMA aqueous solution at room temperature, add 0.2 g QAS, and sonicate to fully dissolve it in the solution; ② Adjust the pH of the solution to 9 with NaOH solution (1 mol / L), and add 0.5 g of the prepared γ-PGA-NHS solid; ③ Add 2 mL of 1 mol / L photoinitiator LAP, and stir at 20 °C for prepolymerization; ④ Irradiate with 405 nm blue light for 10 min to form a gel.

[0062] Figure 6 The antibacterial properties of the two antibacterial wet adhesive hydrogels prepared in Comparative Example 1 and Example 1 against Staphylococcus aureus and Escherichia coli are shown. Gel 1 group is the bacterial growth status after co-culture of the antibacterial wet adhesive hydrogel using QAS as one of the raw materials in Comparative Example 1 with the two bacteria, in which only the quaternary ammonium salt molecular structure plays an antibacterial effect and lacks tannic acid. Compared with the blank control group (Blank), it has a certain antibacterial effect, but the effect is not ideal. Gel 2 group is the growth status after co-culture of the antibacterial wet adhesive hydrogel using QTA as one of the raw materials in Example 1 with the two bacteria, and the number of colonies is significantly reduced compared with the blank control group and Gel 1 group. Staphylococcus aureus and Escherichia coli are representative bacteria of Gram-positive bacteria and Gram-negative bacteria, respectively. The antibacterial effect on the two bacteria proves that the antibacterial wet adhesive hydrogel prepared in Example 1 has a broad-spectrum antibacterial property.

[0063] In this comparative example, QAS is used instead of QTA to prepare the hydrogel. The ratio of the amount of dimethylaminoethyl methacrylate and 1,6-dibromohexane used to prepare QAS is 1:5, and the preparation method used is consistent with Example 1. Since QAS contains a double bond structure, it can still be photopolymerized with GelMA by 405nm blue light irradiation, but compared with QTA, it lacks the pyrogallol structure in tannic acid, and the antibacterial and antioxidant effects of the prepared hydrogel are weakened. The lack of phenolic hydroxyl groups also changes the cross-linking degree of the hydrogel network, reduces the mechanical properties, and loses wet adhesion. The performance of the hydrogel prepared in Comparative Example 1 is weaker than any of the above examples, and the expected effect is not achieved.

[0064] The above are all preferred embodiments of the present application, and the protection scope of the present application is not limited thereto. Therefore, any equivalent changes made according to the structure, shape, and principle of the present application should be included in the protection scope of the present application.

Claims

1. A compound QTA, characterized in that The structure of the compound QTA is shown below: 。 2. A method for preparing the compound QTA according to claim 1, characterized in that: The QTA is prepared from QAS and tannic acid. The reaction formula for preparing QTA from QAS and tannic acid is as follows: 。 3. The method for preparing the compound QTA according to claim 2, characterized in that: The method for preparing a compound QTA from QAS and tannic acid comprises the following steps: mixing QAS and tannic acid, adding a catalyst and a solvent, reacting under the protection of an inert gas, adding deionized water to generate a precipitate after the reaction is complete, standing, washing the precipitate, filtering, collecting a filter cake, and freeze-drying to obtain the compound QTA.

4. The method for preparing the compound QTA according to claim 3, characterized in that: The molar ratio of the QAS to the tannic acid is 2:(0.1-0.2); the catalyst is potassium carbonate, and the solvent is DMF.

5. The method for preparing the compound QTA according to claim 3, characterized in that: The compound QAS is prepared from dimethylaminoethyl methacrylate and 1,6-dibromohexane. The preparation of QAS from dimethylaminoethyl methacrylate and 1,6-dibromohexane includes the following steps: adding dimethylaminoethyl methacrylate to 1,6-dibromohexane, reacting, taking out the liquid after the reaction is complete, adding acetonitrile to the colloid, stirring to form a suspension, centrifuging to obtain a precipitate, washing, and drying to obtain the compound QAS; the molar ratio of the dimethylaminoethyl methacrylate to 1,6-dibromohexane is 1:(2-5).

6. A hydrogel for oral periodontitis, characterized in that: The raw materials of the antibacterial wet adhesion hydrogel include the compound QTA described in claim 1, methacrylated gelatin, and N-hydroxysuccinimide-modified gamma-polyglutamic acid.

7. The hydrogel according to claim 6, characterized in that The mass ratio of QTA, methacryloyl gelatin, and N-hydroxysuccinimide-modified γ-polyglutamic acid is 2:(10~15):(5~10).

8. A method for preparing the hydrogel according to claim 6 or 7, characterized in that: The steps include: Step 1): prepare an aqueous solution of methacryloyl gelatin, add compound QTA, and disperse evenly; Step 2): Adjust the pH to 8.5-9.5, and add N-hydroxysuccinimide modified γ-polyglutamic acid solution; Step 3): Add a photoinitiator, polymerize, and irradiate with 405nm blue light to form a gel, thereby obtaining the antibacterial wet adhesion hydrogel.

9. The method for preparing the hydrogel according to claim 8, characterized in that: In the step 1), the concentration of methacrylylated gelatin in the aqueous solution of methacrylylated gelatin is 10wt% to 15wt%; in the step 2), the concentration of N-hydroxysuccinimide-modified γ-polyglutamic acid solution is 5wt% to 10wt%.

10. Use of the compound QTA according to claim 1 or the hydrogel according to claim 6 or 7 in the preparation of periodontitis drugs or antibacterial drugs.

Citation Information

Cited By

  • Acoustic power driven Janus hydrogel as well as preparation method and application thereof

    CN121731202A

  • An acoustically powered Janus hydrogel and methods of making and using the same

    CN121731202B