Salt-resistant filtrate reducer at 220-230 DEG C and preparation method thereof
By introducing benzene ring groups on the main chain of the polymer molecule, an anti-salt reduction filter loss agent was prepared at 220°C to 230°C, which solved the problems of the prior art of drilling fluid flocculation and gelation under high temperature and high salt conditions, and achieved the Good filtration loss reduction and viscosity reduction performance in environments of 220°C to 230°C meet the needs of deep or ultra-deep well drilling.
Patent Information
- Application Number
- CN202310593211.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-24
- Publication Date
- 2024-11-26
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The existing temperature-resistant and salt-resistant filtration loss agent cannot effectively control the flocculation and gelation of drilling fluid under high temperature and high salt conditions above 200℃, resulting in the uncontrollable filtration loss and cannot meet the needs of deep drilling fluid.
By introducing benzene ring groups on the backbone of the polymer molecule, combining monomers such as acrylamide, sodium para-styrenesulfonate, 2-acrylamide-2-methylpropanesulfonic acid, anti-anti-anti-2-methylpropanesulfonic acid, 220°C to 230°C were prepared by introducing benzene ring groups on the backbone of the polymer molecule, and combining monomers such as acrylamide, sodium para-styrenesulfonate, 2-acrylamide-2-methylpropanesulfonic acid, anti-anti-anti-de-anti-de-anti-de-form-propanesulfonic acid, anti-anti-anti-form-form-propanesulfonic acid, etc., the anti-anti-anti-form-form-form-propanesulfonic acid was prepared by 220°C to 230°C. Salt filter reduction agent improves its stability and salt resistance at high temperatures.
In a saturated salt environment between 220°C and 230°C, the prepared anti-salt filtration loss reducer has good filtration loss reduction and viscosity reduction performance, which can effectively meet the needs of deep wells or ultra-deep well drilling.
Smart Images

Figure FT_1 
Figure SMS_1
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of preparing high-temperature salt-resistant fluid loss reducer, and is a 220-230°C-resistant salt-resistant fluid loss reducer and a preparation method thereof. Background Art
[0002] With the development of economy, the demand for energy is increasing, and the goal of developing oil and gas in deep formations is becoming more and more urgent. However, in developing oil and gas in deep formations, as the well depth increases, from the perspective of higher temperatures in deep formations, treatment agents with stronger temperature resistance are needed; from the perspective of the stability of the drilling fluid's own performance, the drilling fluid needs to be able to withstand higher salinity, so temperature and salt resistance treatment agents are important considerations for deep drilling fluid materials.
[0003] At present, the main temperature-resistant and salt-resistant fluid loss reducers include polymers, sulfonated methyl phenolic resins and sulfonated lignite resins. The maximum temperature resistance of sulfonated methyl phenolic resins and sulfonated lignite is 180°C. They can resist saturated NaCl pollution, but cannot resist Ca 2+ Ion contamination, and it should not be used at bottom hole temperatures exceeding 200°C.
[0004] As we move towards deeper layers of 10,000 meters, it will become more and more common for the bottom hole temperature to reach or exceed 200℃, and the temperature resistance requirement for drilling fluid treatment agents is also 200℃ or above. Fluid loss reducers are one of the most critical treatment agents among various drilling fluid treatment agents. However, synthetic polymer drilling fluids are currently limited above 200℃ because the temperature and pH value cause flocculation and gelation of the drilling fluid, especially when the drilling fluid is contaminated by salt and formation pollutants, the filtration loss cannot be controlled. At present, the market is in urgent need of a fluid loss reducer that is resistant to 200℃ or above and salt-resistant, has the ability to withstand the flocculation and gelation of drilling fluids, and has a good fluid loss reduction effect under high temperature and high salt conditions. Summary of the invention
[0005] The present invention provides a 220°C to 230°C salt-resistant fluid loss reducer and a preparation method thereof, which overcomes the above-mentioned deficiencies of the prior art and can effectively solve the problems that the existing synthetic polymer drilling fluid of the fluid loss reducer is limited above 200°C, and the drilling fluid flocculation and gelation caused by temperature and pH value, thereby resulting in uncontrollable fluid loss.
[0006] One of the technical solutions of the present invention is achieved by the following measures: a 220°C to 230°C salt-resistant filtrate reducer, the process preparation process includes a first unit, a second unit and a third unit, in the first unit, the raw materials include 250 to 350 parts of water, 30 to 70 parts of sodium carbonate, 30 to 70 parts of acrylic acid, 30 to 70 parts of acrylamide, and 60 to 140 parts of sodium p-styrene sulfonate in parts by weight; in the second unit, the raw materials include 200 to 300 parts of water, 20 to 60 parts of sodium hydroxide, 90 to 210 parts of 2-acrylamido-2-methylpropane sulfonic acid, and 60 to 140 parts of n-vinyl pyrrolidone in parts by weight; in the third unit, the raw materials include 60 to 140 parts of acrylonitrile, 30 to 70 parts of 3-butene-1-ol, 150 to 280 parts of alkylphenol polyoxyethylene ether OP-10, sorbitan oleate Span-80 in parts by weight. 60 to 180 parts, 500 to 950 parts of white oil, 5 to 18 parts of persulfate, 3 to 12 parts of azobisisobutyronitrile, and 35 to 60 parts of demulsifier.
[0007] The following is a further optimization and / or improvement of one of the above-mentioned technical solutions: In the first unit, the raw materials include 280 to 320 parts of water, 38 to 60 parts of sodium carbonate, 40 to 58 parts of acrylic acid, 37 to 70 parts of acrylamide, and 72 to 128 parts of sodium p-styrene sulfonate in parts by weight; in the second unit, the raw materials include 230 to 285 parts of water, 20 to 50 parts of sodium hydroxide, 126 to 200 parts of 2-acrylamido-2-methylpropanesulfonic acid, and 60 to 130 parts of n-vinyl pyrrolidone in parts by weight; in the third unit, the raw materials include 65 to 123 parts of acrylonitrile, 37 to 62 parts of 3-butene-1-ol, 175 to 262 parts of alkylphenol polyoxyethylene ether OP-10, and sorbitan oleate Span-80 in parts by weight. 72 to 157 parts, white oil 550 to 880 parts, persulfate 6 to 16 parts, azobisisobutyronitrile 4 to 10 parts, demulsifier 40 to 60 parts.
[0008] The above-mentioned 220°C to 230°C salt-resistant fluid loss reducer is prepared according to the following steps: S1, preparing a first mixed solution of the first unit according to the raw material components of the first unit; S2, preparing a second mixed solution of the second unit according to the raw material components of the second unit; S3, preparing an emulsifier mixed solution of the third unit according to the raw material components of the third unit; S4, mixing the required amount of white oil and the emulsifier mixed solution under high shear stirring conditions, adding the first mixed solution and the second mixed solution, and then adding the required amount of 3-butene-1-ol and acrylonitrile to carry out After high-shear stirring, an emulsion mixture is obtained; S5, adding the required amount of persulfate and azobisisobutyronitrile to the emulsion mixture, stirring and heating to 50°C to 70°C for reaction, and keeping warm for 2h to 3h, then cooling to 12°C to 22°C, and keeping warm for 2h to 3h until the reaction is completed to obtain a reaction mixture; S6, adding the required amount of demulsifier to the reaction mixture, stirring evenly, standing until the demulsification reaction is completed, and vacuum drying at 80°C to 95°C to obtain a 220°C to 230°C salt-resistant filtration reducer.
[0009] In the above step S1, the first mixed solution is prepared according to the following steps: the first step is to add the required amount of water and sodium carbonate to the first reaction container at room temperature, and after the sodium carbonate is completely dissolved, add the required amount of acrylic acid to the first reaction container and stir to obtain a first mixed solution; the second step is to add the required amount of acrylamide and sodium p-styrene sulfonate to the first mixed solution and stir evenly to obtain a first mixed solution, and let it stand for use.
[0010] When preparing the first mixed solution, in the first step, the stirring time is 30 min to 60 min, and the pH value of the first mixed solution is 8 to 10.
[0011] In the above step S2, the second mixed solution is prepared according to the following steps: first, at room temperature, add the required amount of water, sodium hydroxide, and acrylamide-2-methylpropane sulfonic acid to the second reaction container and stir evenly to obtain a second mixed solution; second, add the required amount of n-vinyl pyrrolidone to the second mixed solution and stir evenly to obtain a second mixed solution, and let it stand for use.
[0012] When preparing the second mixed solution, in the first step, the stirring time is 30 min to 60 min, and the pH value of the second mixed solution is 8 to 10.
[0013] In the above step S3, the emulsifier mixture is prepared according to the following steps: adding the required amount of alkylphenol polyoxyethylene ether OP-10 and sorbitan oleate Span-80 into the third reaction container, mixing evenly to obtain the emulsifier mixture, and letting it stand for use.
[0014] In the above step S5, the persulfate is ammonium persulfate or potassium persulfate.
[0015] The second technical solution of the present invention is achieved by the following measures: a preparation method of a 220°C to 230°C salt-resistant fluid loss reducer, which is carried out according to the following steps: S1, preparing a first mixed liquid of the first unit according to the raw material components of the first unit; S2, preparing a second mixed liquid of the second unit according to the raw material components of the second unit; S3, preparing an emulsifier mixed liquid of the third unit according to the raw material components of the third unit; S4, mixing the required amount of white oil and the emulsifier mixed liquid under high shear stirring conditions, adding the first mixed liquid and the second mixed liquid, and then adding the required amount of the third mixed liquid; -Butene-1-ol and acrylonitrile are stirred evenly under high shear to obtain an emulsion mixture; S5, add the required amount of persulfate and azobisisobutyronitrile to the emulsion mixture, stir and heat to 50°C to 70°C for reaction, and keep warm for 2h to 3h, then cool to 12°C to 22°C, and keep warm for 2h to 3h until the reaction is completed to obtain a reaction mixture; S6, add the required amount of demulsifier to the reaction mixture, stir evenly, let it stand until the demulsification reaction is completed, and vacuum dry at 80°C to 95°C to obtain a 220°C to 230°C salt-resistant filtrate reducer.
[0016] The present invention introduces a benzene ring group into the main chain of the molecule, thereby improving the rigidity of the molecular chain, improving its temperature and salt resistance and stability at high temperatures, so that the filtrate still has good filtration loss and viscosity reduction performance in a saturated salt environment of 220°C to 230°C, and can meet the drilling requirements of deep wells or ultra-deep wells. BRIEF DESCRIPTION OF THE DRAWINGS
[0017] Attached Figure 1 It is a chemical structural formula diagram of the main product of the present invention, 220°C to 230°C salt-resistant filtrate reducer. DETAILED DESCRIPTION
[0018] The present invention is not limited by the following embodiments, and the specific implementation method can be determined according to the technical scheme of the present invention and the actual situation. Unless otherwise specified, the various chemical reagents and chemicals mentioned in the present invention are all chemical reagents and chemicals known and used in the prior art; unless otherwise specified, the percentages in the present invention are all mass percentages; unless otherwise specified, the solutions in the present invention are all aqueous solutions with water as the solvent, for example, hydrochloric acid solution is a hydrochloric acid aqueous solution; the normal temperature and room temperature in the present invention generally refer to a temperature of 15°C to 25°C, and are generally defined as 25°C.
[0019] The present invention will be further described below in conjunction with embodiments: Embodiment 1: The 220°C to 230°C salt-resistant filtrate reducer, the process preparation process includes the first unit, the second unit and the third unit. In the first unit, the raw materials include 250 to 350 parts of water, 30 to 70 parts of sodium carbonate, 30 to 70 parts of acrylic acid, 30 to 70 parts of acrylamide, and 60 to 140 parts of sodium p-styrene sulfonate in parts by weight; in the second unit, the raw materials include 200 to 300 parts of water, 20 to 60 parts of sodium hydroxide, 90 to 210 parts of 2-acrylamido-2-methylpropane sulfonic acid, and 60 to 140 parts of n-vinyl pyrrolidone in parts by weight; in the third unit, the raw materials include 60 to 140 parts of acrylonitrile, 30 to 70 parts of 3-butene-1-ol, 150 to 280 parts of alkylphenol polyoxyethylene ether OP-10, sorbitan oleate Span-80 in parts by weight. 60 to 180 parts, 500 to 950 parts of white oil, 5 to 18 parts of persulfate, 3 to 12 parts of azobisisobutyronitrile, and 35 to 60 parts of demulsifier.
[0020] Drilling fluid is a fluid composed of sodium-based bentonite as the basic slurry material. Fluid loss reducer is one of the most critical treatment agents. As the well depth increases, the bottom hole temperature rises, and the fluid loss reducer cannot adapt to this temperature environment and loses its application performance. At present, the highest temperature resistance of domestic fluid loss reducers is 180℃. When the temperature exceeds this, the fluid loss reducer cannot achieve the ability to reduce the fluid loss.
[0021] The 220°C to 230°C salt-resistant fluid loss reducer of the present invention is a temperature-resistant and salt-resistant fluid loss reducer made of synthetic acrylamide polymers, which has a novel structure, introduces a benzene ring group into the main chain of the molecule, greatly improves the rigidity of the molecular chain, and thus improves the temperature and salt resistance of the polymer. Adsorption groups are introduced through monomer acrylamide, carboxylic acid hydration groups are introduced through monomer acrylic acid, benzene rings and sulfonic acid groups are introduced through monomer sodium p-styrene sulfonate, sulfonic acid groups are provided by monomer 2-acrylamide-2-methylpropane sulfonic acid, acrylonitrile provides nitrile groups, heterocyclic alkanones are provided by monomer n-vinyl pyrrolidone, and hydroxyl groups are provided by monomer 3-butene-1-ol. Among them, benzene rings and alkanones are rigid groups, which can improve the rigidity of the molecular chain, and can improve the temperature and salt resistance and water solubility of the molecule together with the sulfonic acid group with a larger molecular radius, so that it has good stability under high temperature and high salt conditions, that is, when the bottom hole temperature is 220°C to 230°C.
[0022] All raw materials used in the present invention are commercially available products, which are easy to purchase and can be put into large-scale production.
[0023] Embodiment 2: The 220°C to 230°C salt-resistant filtrate reducer, the process preparation process includes the first unit, the second unit and the third unit. In the first unit, the raw materials include 250 parts or 350 parts of water, 30 parts or 70 parts of sodium carbonate, 30 parts or 70 parts of acrylic acid, 30 parts or 70 parts of acrylamide, and 60 parts or 140 parts of sodium p-styrene sulfonate in parts by weight; in the second unit, the raw materials include 200 parts or 300 parts of water, 20 parts or 60 parts of sodium hydroxide, 90 parts or 210 parts of 2-acrylamido-2-methylpropanesulfonic acid, and 60 parts or 140 parts of n-vinyl pyrrolidone in parts by weight; in the third unit, the raw materials include 60 parts or 140 parts of acrylonitrile, 30 parts or 70 parts of 3-butene-1-ol, 150 parts or 280 parts of alkylphenol polyoxyethylene ether OP-10, sorbitan oleate Span-80 in parts by weight. 60 parts or 180 parts, 500 parts or 950 parts of white oil, 5 parts or 18 parts of persulfate, 3 parts or 12 parts of azobisisobutyronitrile, and 35 parts or 60 parts of demulsifier.
[0024] Embodiment 3: As an optimization of the above embodiment, in the first unit, the raw materials include 280 to 320 parts of water, 38 to 60 parts of sodium carbonate, 40 to 58 parts of acrylic acid, 37 to 70 parts of acrylamide, and 72 to 128 parts of sodium p-styrene sulfonate in parts by weight; in the second unit, the raw materials include 230 to 285 parts of water, 20 to 50 parts of sodium hydroxide, 126 to 200 parts of 2-acrylamido-2-methylpropanesulfonic acid, and 60 to 130 parts of n-vinyl pyrrolidone in parts by weight; in the third unit, the raw materials include 65 to 123 parts of acrylonitrile, 37 to 62 parts of 3-butene-1-ol, 175 to 262 parts of alkylphenol polyoxyethylene ether OP-10, and sorbitan oleate Span-80 in parts by weight. 72 to 157 parts, white oil 550 to 880 parts, persulfate 6 to 16 parts, azobisisobutyronitrile 4 to 10 parts, demulsifier 40 to 60 parts.
[0025] Example 4: As an optimization of the above example, the following steps are used to prepare the first mixed solution of the first unit according to the raw material components of the first unit; S2, the second mixed solution of the second unit is prepared according to the raw material components of the second unit; S3, the emulsifier mixed solution of the third unit is prepared according to the raw material components of the third unit; S4, the required amount of white oil and the emulsifier mixed solution are mixed under high shear stirring conditions, the first mixed solution and the second mixed solution are added, and the required amount of 3-butene-1-ol and acrylonitrile are added to carry out After high-shear stirring, an emulsion mixture is obtained; S5, adding the required amount of persulfate and azobisisobutyronitrile to the emulsion mixture, stirring and heating to 50°C to 70°C for reaction, and keeping warm for 2h to 3h, then cooling to 12°C to 22°C, and keeping warm for 2h to 3h until the reaction is completed to obtain a reaction mixture; S6, adding the required amount of demulsifier to the reaction mixture, stirring evenly, standing until the demulsification reaction is completed, and vacuum drying at 80°C to 95°C to obtain a 220°C to 230°C salt-resistant filtration reducer.
[0026] Example 5: As an optimization of the above example, in step S1, the first mixed solution is prepared according to the following steps: the first step is to add the required amount of water and sodium carbonate to the first reaction container at room temperature, and after the sodium carbonate is completely dissolved, add the required amount of acrylic acid to the first reaction container and stir to obtain a first mixed solution; the second step is to add the required amount of acrylamide and sodium p-styrene sulfonate to the first mixed solution and stir evenly to obtain a first mixed solution, which is then allowed to stand for use.
[0027] Example 6: As an optimization of the above example, when preparing the first mixed solution, in the first step, the stirring time is 30 min to 60 min, and the pH value of the first solution of the mixture is 8 to 10.
[0028] Example 7: As an optimization of the above example, in step S2, the second mixed solution is prepared according to the following steps: the first step is to add the required amount of water, sodium hydroxide, and acrylamide-2-methylpropane sulfonic acid to the second reaction container at room temperature and stir evenly to obtain a second mixed solution; the second step is to add the required amount of n-vinyl pyrrolidone to the second mixed solution and stir evenly to obtain a second mixed solution, which is then allowed to stand for use.
[0029] Example 8: As an optimization of the above example, when preparing the second mixed solution, in the first step, the stirring time is 30 min to 60 min, and the pH value of the second solution of the mixture is 8 to 10.
[0030] Example 9: As an optimization of the above example, in step S3, the emulsifier mixture is prepared according to the following steps: Add the required amount of alkylphenol polyoxyethylene ether OP-10 and sorbitan oleate Span-80 into the third reaction container, mix well to obtain an emulsifier mixture, and let it stand for use.
[0031] Example 10: As an optimization of the above example, in step S5, the persulfate is ammonium persulfate or potassium persulfate, and in step S6, the demulsifier is an existing well-known and commonly used commercial product, code-named fsm-1.
[0032] Example 11: The preparation method of the 220°C to 230°C salt-resistant fluid loss reducer is carried out according to the following steps: S1, preparing a first mixed solution of the first unit according to the raw material components of the first unit; S2, preparing a second mixed solution of the second unit according to the raw material components of the second unit; S3, preparing an emulsifier mixed solution of the third unit according to the raw material components of the third unit; S4, mixing a required amount of white oil and an emulsifier mixed solution under high shear stirring conditions, adding the first mixed solution and the second mixed solution, and then adding a required amount of 3-butene-1-ol and After acrylonitrile is stirred evenly under high shear, an emulsion mixture is obtained; S5, the required amount of persulfate and azobisisobutyronitrile are added to the emulsion mixture, the mixture is stirred and heated to 50°C to 70°C for reaction, and the mixture is kept warm for 2h to 3h, then the mixture is cooled to 12°C to 22°C, and the mixture is kept warm for 2h to 3h until the reaction is completed to obtain a reaction mixture; S6, the required amount of demulsifier is added to the reaction mixture, the mixture is stirred evenly, and the mixture is allowed to stand until the demulsification reaction is completed, and the mixture is vacuum dried at 80°C to 95°C to obtain a 220°C to 230°C salt-resistant filtrate reducer.
[0033] The chemical structural formula of the main product of the 20°C to 230°C salt-resistant fluid loss reducer obtained by the present invention is as follows: Figure 1 shown.
[0034] Embodiment 12: Prepare the first mixed solution of the first unit: at room temperature, add 295 parts of water and 42 parts of sodium carbonate to a reactor 1 equipped with a stirring device. After the sodium carbonate is completely dissolved, add 50 parts of acrylic acid and stir for 50 minutes. The pH value is 8.5. Then add 42 parts of acrylamide and 85 parts of sodium p-styrene sulfonate and stir evenly to obtain a first mixed solution. Let it stand for use.
[0035] Prepare the second mixed solution of the second unit: at room temperature, add 248 parts of water, 26 parts of sodium hydroxide, and 135 parts of 2-acrylamide-2-methylpropanesulfonic acid to a reactor 2 equipped with a stirring device. After stirring evenly, the pH value is 9.5. Add 75 parts of n-vinyl pyrrolidone and continue to stir evenly to obtain a second mixed solution, which is allowed to stand for use.
[0036] Prepare the emulsifier mixture of the third unit: mix 182 parts of alkylphenol polyoxyethylene ether OP-10 and 78 parts of sorbitan oleate Span-80 in a stirring tank to obtain an emulsifier mixture, and let it stand for use; Add 650 parts of white oil and an emulsifier mixture to a reactor 3 with a high shear stirring device having heating and cooling functions, slowly add the first mixture in the reactor 1 and the second mixture in the reactor 2 under high shear stirring conditions, add 43 parts of 3-butene-1-ol and 77 parts of acrylonitrile after the addition, and stir evenly under high shear to obtain an emulsion mixture; add 8.5 parts of ammonium persulfate and 5 parts of azobisisobutyronitrile to the emulsion mixture, heat it to 57°C while stirring, and keep it warm for 2.5 hours. When the reactant starts to heat up, cool it down to 14°C quickly, stir it and keep it warm for 2 hours. When the reactant has a constant temperature for 1 hour without any change, the reaction is completed, and a reaction mixture is obtained; Add 46 parts of demulsifier to the reaction mixture, stir evenly, let it stand, and when fine alum flowers appear, the demulsification is completed. Vacuum dry at 90°C to obtain a salt-resistant filtrate reducer with a temperature of 220°C to 230°C.
[0037] Embodiment 13: Prepare the first mixed solution of the first unit: at room temperature, add 300 parts of water and 53 parts of sodium carbonate to a reactor 1 equipped with a stirring device. After the sodium carbonate is completely dissolved, add 53 parts of acrylic acid and stir for 45 minutes. The pH value is 8. Then add 61 parts of acrylamide and 105 parts of sodium p-styrene sulfonate and stir evenly to obtain a first mixed solution. Let it stand for use.
[0038] Prepare the second mixed solution of the second unit: at room temperature, add 275 parts of water, 45 parts of sodium hydroxide, and 183 parts of 2-acrylamide-2-methylpropanesulfonic acid to a reactor 2 equipped with a stirring device. After stirring evenly, the pH value is 9. Add 118 parts of n-vinyl pyrrolidone and continue to stir evenly to obtain a second mixed solution, which is allowed to stand for use.
[0039] Prepare the emulsifier mixture of the third unit: mix 236 parts of alkylphenol polyoxyethylene ether OP-10 and 132 parts of sorbitan oleate Span-80 in a stirring tank to obtain an emulsifier mixture, and let it stand for use; Add 760 parts of white oil and an emulsifier mixture to a reactor 3 with a high shear stirring device having heating and cooling functions, slowly add the first mixture in the reactor 1 and the second mixture in the reactor 2 under high shear stirring conditions, add 52 parts of 3-butene-1-ol and 115 parts of acrylonitrile after the addition, and stir evenly under high shear to obtain an emulsion mixture; add 14 parts of ammonium persulfate and 8 parts of azobisisobutyronitrile to the emulsion mixture, heat it to 63°C while stirring, and keep it warm for 2 hours, when the reactant starts to heat up, quickly cool it to 16°C, stir it while keeping it warm for 2.5 hours, and wait until the reactant has a constant temperature for 1 hour without changing, indicating that the reaction is completed, and a reaction mixture is obtained; Add 55 parts of demulsifier to the reaction mixture, stir evenly, let it stand, and when fine alum flowers appear, the demulsification is completed. Vacuum dry at 93°C to obtain a salt-resistant filtrate reducer with a temperature of 220°C to 230°C.
[0040] Embodiment 14: Prepare the first mixed solution of the first unit: at room temperature, add 304 parts of water and 50 parts of sodium carbonate to a reactor 1 equipped with a stirring device. After the sodium carbonate is completely dissolved, add 53 parts of acrylic acid and stir for 55 minutes. The pH value is 9. Then add 60 parts of acrylamide and 96 parts of sodium p-styrene sulfonate and stir evenly to obtain a first mixed solution. Let it stand for use.
[0041] Prepare the second mixed solution of the second unit: at room temperature, add 278 parts of water, 47 parts of sodium hydroxide, and 164 parts of 2-acrylamide-2-methylpropanesulfonic acid to a reactor 2 equipped with a stirring device. After stirring evenly, the pH value is 9. Add 111 parts of n-vinyl pyrrolidone and continue to stir evenly to obtain a second mixed solution, which is allowed to stand for use.
[0042] Prepare the emulsifier mixture of the third unit: mix 217 parts of alkylphenol polyoxyethylene ether OP-10 and 84 parts of sorbitan oleate Span-80 in a stirring tank to obtain an emulsifier mixture, and let it stand for use; Add 650 parts of white oil and an emulsifier mixture to a reactor 3 with a high shear stirring device having heating and cooling functions, slowly add the first mixture in the reactor 1 and the second mixture in the reactor 2 under high shear stirring conditions, add 50 parts of 3-butene-1-ol and 100 parts of acrylonitrile after the addition, and stir evenly under high shear to obtain an emulsion mixture; add 13 parts of potassium persulfate and 6 parts of azobisisobutyronitrile to the emulsion mixture, heat it to 64°C while stirring, and keep it warm for 2.5 hours, when the reactant starts to heat up, quickly cool it to 17°C, stir it while keeping it warm for 2.5 hours, and wait until the reactant has a constant temperature for 0.5 hours without changing, indicating that the reaction is completed, and a reaction mixture is obtained; Add 55 parts of demulsifier to the reaction mixture, stir evenly, let it stand, and when fine alum flowers appear, the demulsification is completed. Vacuum dry at 90°C to obtain a salt-resistant filtrate reducer with a temperature of 220°C to 230°C.
[0043] The drilling fluid performance test of the 220°C to 230°C salt-resistant filtrate reducer obtained in Examples 12 to 14 of the present invention was carried out, and the results are shown in Tables 1 and 2, wherein Table 1 is 2% standard soil + 5% embodiment sample + 30% NaCl + 20% NaOH, and Table 2 is 2% standard soil + 5% embodiment sample + 25% NaCl + 7% KCl + 20% NaOH.
[0044] It can be seen from Table 1 and Table 2 that the 220°C to 230°C salt-resistant fluid loss reducer of the present invention has good fluid loss and viscosity reduction performance, and can meet the actual use requirements of deep well or ultra-deep well drilling.
[0045] In summary, the present invention improves the rigidity of the molecular chain, improves its temperature and salt resistance and stability at high temperatures by introducing a benzene ring group into the main chain of the molecule, so that it still has good filtration loss and viscosity reduction performance in a saturated salt environment of 220°C to 230°C, and can meet the drilling requirements of deep wells or ultra-deep wells.
[0046] The above technical features constitute the embodiments of the present invention, which have strong adaptability and implementation effect. Non-essential technical features can be added or reduced according to actual needs to meet the requirements of different situations.
Claims
1. A 220°C to 230°C salt-resistant fluid loss reducer, characterized in that The process preparation includes a first unit, a second unit and a third unit. In the first unit, the raw materials include 250 to 350 parts of water, 30 to 70 parts of sodium carbonate, 30 to 70 parts of acrylic acid, 30 to 70 parts of acrylamide, and 60 to 140 parts of sodium p-styrene sulfonate in parts by weight; in the second unit, the raw materials include 200 to 300 parts of water, 20 to 60 parts of sodium hydroxide, 90 to 210 parts of 2-acrylamido-2-methylpropanesulfonic acid, and 60 to 140 parts of n-vinyl pyrrolidone in parts by weight; in the third unit, the raw materials include 60 to 140 parts of acrylonitrile, 30 to 70 parts of 3-butene-1-ol, 150 to 280 parts of alkylphenol polyoxyethylene ether OP-10, sorbitan oleate Span-80 in parts by weight. 60 to 180 parts, 500 to 950 parts of white oil, 5 to 18 parts of persulfate, 3 to 12 parts of azobisisobutyronitrile, and 35 to 60 parts of demulsifier.
2. The 220°C to 230°C salt-resistant fluid loss reducer according to claim 1, characterized in that In the first unit, the raw materials include 280 to 320 parts of water, 38 to 60 parts of sodium carbonate, 40 to 58 parts of acrylic acid, 37 to 70 parts of acrylamide, and 72 to 128 parts of sodium p-styrene sulfonate in parts by weight; in the second unit, the raw materials include 230 to 285 parts of water, 20 to 50 parts of sodium hydroxide, 126 to 200 parts of 2-acrylamido-2-methylpropanesulfonic acid, and 60 to 130 parts of n-vinyl pyrrolidone in parts by weight; in the third unit, the raw materials include 65 to 123 parts of acrylonitrile, 37 to 62 parts of 3-butene-1-ol, 175 to 262 parts of alkylphenol polyoxyethylene ether OP-10, and sorbitan oleate Span-80 in parts by weight. 72 to 157 parts, white oil 550 to 880 parts, persulfate 6 to 16 parts, azobisisobutyronitrile 4 to 10 parts, demulsifier 40 to 60 parts.
3. The 220°C to 230°C salt-resistant fluid loss reducer according to claim 1 or 2, characterized in that The preparation is carried out according to the following steps: S1, preparing the first mixed solution of the first unit according to the raw material components of the first unit; S2, preparing the second mixed solution of the second unit according to the raw material components of the second unit; S3, preparing the emulsifier mixed solution of the third unit according to the raw material components of the third unit; S4, mixing the required amount of white oil and the emulsifier mixed solution under high shear stirring conditions, adding the first mixed solution and the second mixed solution, and then adding the required amount of 3-butene-1-ol and acrylonitrile to high shear stirring to obtain an emulsion mixed solution; S5, adding the required amount of persulfate and azobisisobutyronitrile to the emulsion mixed solution, stirring and heating to 50°C to 70°C for reaction, and keeping the temperature for 2h to 3h, then cooling to 12°C to 22°C, keeping the temperature for 2h to 3h until the reaction is completed, to obtain a reaction mixture; S6, adding the required amount of demulsifier to the reaction mixture, stirring evenly, standing, and after the demulsification reaction is completed, vacuum drying at 80°C to 95°C to obtain a 220°C to 230°C salt-resistant filtrate reducer.
4. The 220°C to 230°C salt-resistant fluid loss reducer according to claim 1, characterized in that In step S1, the first mixed solution is prepared according to the following steps: first, at room temperature, a required amount of water and sodium carbonate are added to a first reaction container, and after the sodium carbonate is completely dissolved, a required amount of acrylic acid is added to the first reaction container and stirred to obtain a first mixed solution; second, a required amount of acrylamide and sodium p-styrene sulfonate are added to the first mixed solution and stirred evenly to obtain a first mixed solution, which is allowed to stand for use.
5. The 220°C to 230°C salt-resistant fluid loss reducer according to claim 4, characterized in that When preparing the first mixed solution, in the first step, the stirring time is 30 min to 60 min, and the pH value of the first mixed solution is 8 to 10.
6. The 220°C to 230°C salt-resistant fluid loss reducer according to claim 3, 4 or 5, characterized in that In step S2, the second mixed solution is prepared according to the following steps: first, at room temperature, add the required amount of water, sodium hydroxide, and acrylamide-2-methylpropane sulfonic acid to the second reaction container and stir evenly to obtain a second mixed solution; second, add the required amount of n-vinyl pyrrolidone to the second mixed solution and stir evenly to obtain a second mixed solution, and let it stand for use.
7. The 220°C to 230°C salt-resistant fluid loss reducer according to claim 6, characterized in that When preparing the second mixed solution, in the first step, the stirring time is 30 min to 60 min, and the pH value of the second mixed solution is 8 to 10.
8. The 220°C to 230°C salt-resistant fluid loss reducer according to claim 3, 4, 5, 6 or 7, characterized in that In step S3, the emulsifier mixture is prepared according to the following steps: adding the required amount of alkylphenol polyoxyethylene ether OP-10 and sorbitan oleate Span-80 into the third reaction container, mixing evenly to obtain the emulsifier mixture, and letting it stand for use.
9. The 220°C to 230°C salt-resistant fluid loss reducer according to any one of claims 3 to 8, characterized in that In step S5, the persulfate is ammonium persulfate or potassium persulfate.
10. A method for preparing the 220°C to 230°C salt-resistant fluid loss reducer according to claim 1 or 2 or 4 or 5 or 6 or 7 or 8 or 9, characterized in that The process is carried out according to the following steps: S1, preparing the first mixed solution of the first unit according to the raw material components of the first unit; S2, preparing the second mixed solution of the second unit according to the raw material components of the second unit; S3, preparing the emulsifier mixed solution of the third unit according to the raw material components of the third unit; S4, mixing the required amount of white oil and the emulsifier mixed solution under high shear stirring conditions, adding the first mixed solution and the second mixed solution, and then adding the required amount of 3-butene-1-ol and acrylonitrile to carry out high shear stirring to obtain an emulsion mixed solution; S5, adding the required amount of persulfate and azobisisobutyronitrile to the emulsion mixed solution, stirring and heating to 50°C to 70°C for reaction, and keeping the temperature for 2h to 3h, then cooling to 12°C to 22°C, keeping the temperature for 2h to 3h until the reaction is completed, and obtaining a reaction mixture; S6, adding the required amount of demulsifier to the reaction mixture, stirring evenly, standing, and after the demulsification reaction is completed, vacuum drying at 80°C to 95°C to obtain a 220°C to 230°C salt-resistant filtrate reducer.
Citation Information
Patent Citations
Temperature-resistant and salt-resistant fluid loss additive emulsion and preparation method thereof
CN103694407A
High-temperature-resistant fluid loss agent and preparation method thereof as well as water-based drilling fluid
CN108342188A
High-temperature-resistant composite salt-resistant low-viscosity fluid loss reducer for drilling fluid and preparation method thereof
CN109021942A
Preparation method of high temperature-resistant and salt-resistant nano-emulsion copolymer filtrate reducer for drilling fluids
CN109777378A
High-molecular polymer and preparation method and application thereof
CN112175135A
Cited By
Ultrahigh-density consolidation plugging agent and preparation method thereof as well as diluent and preparation method and application thereof
CN119331153A
Ultra-high density consolidation plugging agent and preparation method thereof, and diluent and preparation method and application thereof
CN119331153B
Expanded graphite reinforced modified lignite filtrate reducer and preparation method thereof
CN122563562A