Compound, preparation method thereof, interface bonding agent and application

By preparing an interface binder with amide chains and silane groups, the problem of poor processing performance and flame retardant effect of existing silane coupling agents at high temperatures is solved, and the mechanical and heat resistance of nylon is improved , and improves the flame retardant effect in the halogen-free flame retardant system.

CN119019676APending Publication Date: 2024-11-26HUIZHOU WATER NEW MATERIAL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411205927.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-30
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

The existing silane coupling agents have poor processing performance and flame retardant effects on aromatic nylon at high temperatures, and are prone to burning and trapping during injection molding, affecting the mechanical properties and heat resistance of the material.

Method used

Provide a compound and a preparation method thereof, by mixing compounds A, B and C for ring opening and polycondensation reactions, to form intermediate products, and undergo dehydration and condensation reactions with compound D under an inert gas atmosphere to prepare amide chains and silane groups The interfacial bonding agent of the group is used to improve the interfacial bonding between nylon and glass fiber or inorganic mineral powder.

Benefits of technology

Improves the mechanical properties, heat resistance and processing properties of nylon, forms a flexible interface layer, enhances compatibility with resin, is suitable for medium and high temperature application environments, and has both flame retardant synergistic effects in halogen-free flame retardant systems. , improves the mechanical properties and airtightness of the material.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119019676A_ABST
    Figure CN119019676A_ABST
Patent Text Reader

Abstract

The invention discloses a compound and a preparation method thereof, an interface binding agent and application. The structural general formula of the compound is # imgabs0 #. Wherein R1 is selected from any one of the following groups: # imgabs1 # # imgabs2 #, Ra is independently selected from-H,-D, carboxyl, C2-C5 alkyl substituted by carboxyl or unsubstituted C1-C5 alkyl when appearing each time, at least one Ra is selected from carboxyl or C2-C5 alkyl substituted by carboxyl, R2 is-Rb-or-Rb-NH-Rb-, Rb is independently selected from C1-C5 alkylene when appearing each time, R3, R4 and R5 are independently selected from C1-C5 alkyl or C1-C5 alkoxy, and at least one of Ra and Rb is independently selected from C1-C5 alkyl or C1-C5 alkoxy. And n is an integer from 10 to 20. One section of the compound has an amide chain with a certain length, and the other end of the compound is a silane group which reacts with the surface of glass fiber or inorganic mineral powder and the like to generate a chemical bond, so that a flexible interface layer can be formed between two phases, and the interface bonding force between the nylon material and the glass fiber or the inorganic mineral powder is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of polymer materials, in particular to a compound, a preparation method thereof, an interface binder and applications thereof. Background Art

[0002] Nylon, developed by the distinguished American scientist Carothers and a research team led by him, is the world's first synthetic fiber. The emergence of nylon revolutionized the textile industry, and its synthesis marked a major breakthrough in the synthetic fiber industry and a significant milestone in polymer chemistry. Due to its many excellent properties, nylon is widely used in automobiles, electrical equipment, mechanical structures, transportation equipment, textiles, papermaking, and machinery. For automakers and even the entire automotive industry, lightweighting vehicles is becoming increasingly practical and an inevitable trend. Among numerous lightweight materials, automotive plastics have quietly risen to prominence, and replacing steel with plastic will be a key trend in the development of lightweight vehicles.

[0003] Silane coupling agent, as a traditional modified material, can significantly improve the mechanical properties of the material. However, the processing temperature of nylon is above 250 degrees, especially the processing temperature of aromatic nylon is higher, above 300 degrees. The existing coupling agents on the market have a low flash point, are not heat-resistant, and are prone to produce burning and trapped gas during injection molding. They have no obvious effect on high-temperature nylon. Excessive addition of coupling agent also has a negative impact on the flame retardant effect of flame-retardant nylon materials. Summary of the Invention

[0004] Based on this, in order to improve the mechanical properties, heat resistance and processing properties of the material, especially to improve the interfacial bonding strength between nylon and metal, glass fiber and filler, it is necessary to provide a compound and its preparation method, interface binder and application.

[0005] The present invention provides a compound having the general structural formula:

[0006] ;

[0007] Wherein, R1 is selected from any of the groups shown in (1-1) to (1-2) , R a Each occurrence is independently selected from -H, -D, carboxyl, C2~C5 alkyl substituted by carboxyl or unsubstituted C1~C5 alkyl, and at least one R a is selected from carboxyl or C2~C5 alkyl substituted by carboxyl,

[0008] R2 is -R b -or-R b -NH-R b -, R bEach occurrence is independently selected from C1 to C5 alkylene,

[0009] R3, R4 and R5 are independently selected from C1~C5 alkyl or C1~C5 alkoxy,

[0010] n is an integer between 10 and 20.

[0011] In one embodiment, the relative molecular weight of the compound is 2000-4000.

[0012] In one embodiment, the compound satisfies one or more of the following characteristics:

[0013] (1) R a Each occurrence is selected from -H or carboxyl, at least one R a is a carboxyl group,

[0014] (2) R2 is -R b -or-R b -NH-R b -, R b Each occurrence is independently selected from a C1 to C3 straight chain alkylene group,

[0015] (3) R3, R4 and R5 are independently selected from C1~C3 alkyl or C1~C3 alkoxy.

[0016] In one embodiment, the structure of the compound is one of formula (2-1) and (2-5):

[0017]

[0018]

[0019]

[0020] .

[0021] Furthermore, the present invention also provides a method for preparing the above-mentioned compound, comprising the following steps:

[0022] Mixed compound A Compound B and compound C , heating to 160° C. to 180° C., the compound B undergoes a ring-opening reaction and a polycondensation reaction, and then undergoes a first dehydration condensation reaction with the compound A and the compound C, respectively, to prepare an intermediate product;

[0023] In an inert gas atmosphere at a temperature of 180°C to 200°C, the intermediate product and compound D are mixed. , the intermediate product and the compound D undergo a second dehydration condensation reaction.

[0024] In one embodiment, one or more of the following characteristics are met:

[0025] (1) The molar ratio of the compound A, the compound B and the compound C is 1:(0.5-0.8):(1-1.2);

[0026] (2) The compound A is selected from one or more of terephthalic acid, isophthalic acid, phthalic acid, 4,4'-biphenyldicarboxylic acid and naphthalene dicarboxylic acid;

[0027] (2) The compound D is a silane coupling agent having a primary amine terminal group.

[0028] In one embodiment, the compound D is selected from one or more of N-2-(aminoethyl)-3-aminopropyltrimethoxysilane, N-2-(aminoethyl)-3-aminopropyltriethoxysilane, γ-aminopropyltrimethoxysilane, γ-aminopropyltriethoxysilane, 3-aminopropylmethyldimethoxysilane, 3-aminopropylmethyldiethoxysilane and N,N-dimethyl-3-aminopropyltrimethoxysilane.

[0029] In one embodiment, one or more of the following characteristics are met:

[0030] (1) The reaction conditions for preparing the intermediate product include: the reaction environment contains a catalyst, and the amount of the catalyst added is 0.03% to 0.05% of the total mass of the compound A, the compound B, and the compound C;

[0031] (2) The reaction conditions of the second dehydration condensation reaction include: a molar ratio of the intermediate product to the compound D of 1.05 to 0.95.

[0032] The present invention also provides an interface binder comprising the above compound.

[0033] The present invention further provides the use of the above compound or the above interface binder in the preparation of high-temperature resistant nylon modified products.

[0034] One end of the compound's structure contains an amide chain of a certain length that is similar to the structure of nylon molecular chains and is intertwined with each other. The other end contains a silane group that can react with the surface of glass fiber or inorganic mineral powder to form a chemical bond. An interfacial binder containing this compound can form a flexible interface layer between the two phases, improving compatibility with the resin, improving the interfacial bonding between nylon and glass fiber or inorganic mineral powder, and enhancing the mechanical properties, heat resistance, and processing properties of nylon, allowing the preparation of high-modulus, high-rigidity materials. This compound or an interfacial binder containing this compound is suitable for use in medium- and high-temperature applications such as electronic appliances and automotive equipment using aromatic nylon materials, as well as applications requiring reflow soldering. DETAILED DESCRIPTION

[0035] The present invention can be implemented in many different forms and is not limited to the embodiments described herein. Rather, these embodiments are provided for the purpose of providing a more thorough and comprehensive understanding of the disclosure of the present invention. Of course, they are merely illustrative and are not intended to limit the present invention. Furthermore, the present invention may repeat reference numerals and / or letters in different examples. Such repetition is for the purpose of simplicity and clarity and does not in itself indicate the relationship between the various embodiments and / or arrangements discussed.

[0036] In addition, the terms "first" and "second" are used for descriptive purposes only and should not be understood as indicating or implying relative importance or implicitly indicating the number of the indicated technical features. Therefore, a feature defined as "first" or "second" may explicitly or implicitly include at least one of the features. In the description of the invention, the meaning of "plurality" is at least two, such as two, three, etc., unless otherwise clearly and specifically defined. In the description of the present invention, the meaning of "several" is at least one, such as one, two, etc., unless otherwise clearly and specifically defined.

[0037] Unless otherwise indicated, all percentages, fractions, and ratios are calculated based on the total weight of the compositions of the present invention. Unless otherwise indicated, all masses relating to listed ingredients are given as active ingredients and therefore do not include solvents or by-products that may be present in commercially available materials. The term "mass percentage content" may be expressed herein using the symbol "%.

[0038] As used herein, "comprises," "includes," "contains," "has," "has" or other variations are intended to encompass non-exclusive inclusions, and no distinction is made between these terms. The term "comprising" means that other steps and ingredients that do not affect the end result may be added. The term "comprising" also encompasses the terms "consisting of" and "consisting essentially of." The compositions and methods / processes of the present invention comprise, consist of, and consist essentially of the essential elements and limitations described herein, as well as any additional or optional ingredients, components, steps, or limitations described herein. No distinction is made between the terms "efficacy," "performance," "effect," and "efficacy" herein.

[0039] The terms "preferably," "more preferably," and the like, used herein refer to embodiments of the present invention that may provide certain benefits under certain circumstances. However, other embodiments may also be preferred under the same or other circumstances. Furthermore, the recitation of one or more preferred embodiments does not imply that other embodiments are not useful, nor is it intended to exclude other embodiments from the scope of the present invention.

[0040] When a numerical range is disclosed herein, the range is considered continuous and includes the minimum and maximum values ​​of the range, as well as every value between such minimum and maximum values. Further, when a range refers to an integer, every integer between the minimum and maximum values ​​of the range is included. In addition, when multiple ranges are provided to describe a feature or characteristic, the ranges can be combined. In other words, unless otherwise indicated, all ranges disclosed herein are understood to include any and all subranges subsumed therein.

[0041] Unless otherwise specified, when a group has one or more connectable sites, any one or more sites of the group can be connected to other groups through chemical bonds. When the chemical bond connection mode is non-positional and there is an H atom at the connectable site, when the chemical bond is connected, the number of H atoms at the site will decrease accordingly with the number of connected chemical bonds, and the group will become a group with a corresponding valence. The chemical bond connecting the site to other groups can be represented by a straight solid bond ( )、straight dashed line key( ), or a wavy line ( ) represents. For example, the straight solid bond in -OCH3 represents the connection to other groups through the oxygen atom in the group; The straight dashed bond in the group indicates that the two ends of the nitrogen atom in the group are connected to other groups; The wavy line in the phenyl group indicates that it is connected to other groups through the carbon atoms at positions 1 and 2 in the phenyl group; Indicates that any linkable site on the piperidinyl group can be connected to other groups through a chemical bond, including at least 、 、 、 In these four connection methods, even if an H atom is drawn on -N-, Still includes For groups connected in this way, when one chemical bond is connected, the H at that site will be reduced by one and become a corresponding monovalent piperidine group.

[0042] The present invention provides a compound having the general structural formula:

[0043] ;

[0044] Wherein, R1 is selected from any of the groups shown in (1-1) to (1-2) , R a Each occurrence is independently selected from -H, -D, carboxyl, C2~C5 alkyl substituted by carboxyl or unsubstituted C1~C5 alkyl, and at least one R a is selected from carboxyl or C2~C5 alkyl substituted by carboxyl,

[0045] R2 is -R b -or-R b -NH-R b -, R b Each occurrence is independently selected from C1 to C5 alkylene,

[0046] R3, R4 and R5 are independently selected from C1~C5 alkyl or C1~C5 alkoxy,

[0047] n is an integer between 10 and 20.

[0048] In a specific example, the relative molecular weight of the compound is 2000-4000.

[0049] Furthermore, the viscosity of the compound in the test method of relative viscosity of semi-aromatic copolyamide resin in GB12006.1-89 is 1.9-2.2. Specifically, the viscosity of the above compound can be but is not limited to 1.9, 1.95, 2, 2.05, 2.1, 2.15 or 2.2.

[0050] In a specific example, R a Each occurrence is selected from -H or carboxyl, at least one R a It is a carboxyl group.

[0051] In a specific example, -R b -or-R b -NH-R b -, R b Each occurrence is independently selected from C1 to C3 straight chain alkylene.

[0052] In a specific example, R3, R4 and R5 are independently selected from C1~C3 alkyl or C1~C3 alkoxy.

[0053] In a specific example, the structure of the compound is one of formulas (2-1) and (2-5):

[0054]

[0055]

[0056]

[0057] .

[0058] Furthermore, the present invention also provides a method for preparing the above-mentioned compound, comprising the following steps:

[0059] Step S1: Mixing Compound A Compound B and compound C , heating to 160° C. to 180° C., compound B undergoes a ring-opening reaction and a polycondensation reaction, and then undergoes a first dehydration condensation reaction with compound A and compound C, respectively, to prepare an intermediate product;

[0060] Step S2: Mix the intermediate product and compound D in an inert gas atmosphere at a temperature of 180°C to 200°C. , the intermediate product and compound D undergo a second dehydration condensation reaction.

[0061] In a specific example, the molar ratio of compound A, compound B, and compound C is 1:(0.5-0.8):(1-1.2).

[0062] Furthermore, in step S1, the reaction environment contains a catalyst, and the amount of the catalyst added is 0.03% to 0.05% of the total mass of compound A, compound B and compound C.

[0063] In a specific example, compound A is selected from one or more of terephthalic acid, isophthalic acid, phthalic acid, 4,4'-biphenyldicarboxylic acid, and naphthalene dicarboxylic acid.

[0064] In a specific example, compound C is selected from one or more of p-aminobenzoic acid, m-aminobenzoic acid, and o-aminobenzoic acid.

[0065] In a specific example, compound D is selected from silane coupling agents whose terminal groups are primary amine groups.

[0066] Furthermore, compound D is selected from one or more of N-2-(aminoethyl)-3-aminopropyltrimethoxysilane, N-2-(aminoethyl)-3-aminopropyltriethoxysilane, γ-aminopropyltrimethoxysilane, γ-aminopropyltriethoxysilane, 3-aminopropylmethyldimethoxysilane, 3-aminopropylmethyldiethoxysilane and N,N-dimethyl-3-aminopropyltrimethoxysilane.

[0067] In a specific example, in step S1, compound A, compound B, and compound C react until no more water is produced, thereby obtaining an intermediate product that is a light yellow transparent liquid.

[0068] Furthermore, the heating rate in step S1 is 10° C. / min to 18° C. / min, preferably 15° C. / min.

[0069] Furthermore, the reaction system needs to be cooled to 100° C. to 120° C. within 1 h to 1.5 h.

[0070] In a specific example, the mixed intermediate product, compound D and a catalyst, wherein the molar ratio of the intermediate product to the compound D is 1.05-0.95.

[0071] Preferably, the molar ratio of the intermediate product to compound D is 1.

[0072] Furthermore, the catalyst is selected from one or more of sodium phosphite, magnesium phosphite, calcium phosphite, zinc phosphite, potassium phosphate, magnesium phosphate, calcium phosphate, zinc phosphate, potassium hypophosphite, sodium hypophosphite, magnesium hypophosphite, calcium hypophosphite, zinc hypophosphite, tetrabutyl titanate, tetra-n-butyl titanate and tetraisopropyl titanate.

[0073] The reaction time in step S2 is 20 min to 40 min, preferably 30 min.

[0074] Furthermore, the crude product obtained by the reaction of the intermediate product with compound D is a milky white solid after cooling, and a purification step is required after step S2.

[0075] The purification step includes purifying with an extractor for 20 hours to 30 hours and then drying in a vacuum oven at 40° C. to 70° C.

[0076] It can be understood that the inert gas is selected from one or more of nitrogen, carbon dioxide, argon and helium, preferably nitrogen.

[0077] The present invention also provides an interface binder comprising the above compound.

[0078] The present invention further provides the use of the above-mentioned compound or the above-mentioned interface binder in the preparation of high-temperature resistant nylon modified products.

[0079] One end of the compound's structure contains an amide chain of a certain length that is similar to the structure of nylon molecular chains and is intertwined with each other. The other end contains a silane group that can react with the surface of glass fiber or inorganic mineral powder to form a chemical bond. An interfacial binder containing this compound can form a flexible interface layer between the two phases, improving compatibility with the resin, improving the interfacial bonding between nylon and glass fiber or inorganic mineral powder, and enhancing the mechanical properties, heat resistance, and processing properties of nylon, allowing the preparation of high-modulus, high-rigidity materials. This compound or an interfacial binder containing this compound is suitable for use in medium- and high-temperature applications such as electronic appliances and automotive equipment using aromatic nylon materials, as well as applications requiring reflow soldering.

[0080] The interface binder and its preparation method of the present invention are further described in detail below with reference to specific examples. The raw materials used in the following examples are all commercially available products unless otherwise specified.

[0081] Example 1

[0082] In a reactor equipped with a water separator, a spherical condenser and a thermometer, 56.5g of caprolactam, 166.13g of terephthalic acid, 137.14g of m-aminobenzoic acid and 0.1g of catalyst were selected according to a preset ratio, and the raw materials were added to the reactor purged with nitrogen. The stirring device was turned on with a stirring speed of 60r / min. The air reserved in the reactor was replaced with nitrogen at least three times, and 0.02MPa of nitrogen was reserved as a protective gas. The reactor was heated by circulating heat transfer oil at a heating rate of 15°C per minute to 180°C. (There is a heat preservation process in this process, in which the reactor is kept warm when the reactor temperature is 90°C for 2h. After the heat preservation is completed, the reactor is heated and the pressure rises accordingly. The pressure of the reactor is relieved by releasing the water vapor generated by the reaction of the system). The polycondensation reaction was initiated and maintained at a constant temperature until no more water was produced in the water separator (to promptly remove any water generated in the system). The intermediate product was a slightly yellow, transparent liquid. After the reaction was complete, the temperature was lowered, and the pressure in the autoclave was slowly reduced to 100-120°C over 1.0-1.5 hours. Under inert gas protection, 221.4 g of 3-aminopropyltriethoxysilane was added, and the reaction temperature was 180-200°C. The reaction was terminated after 30 minutes. After the reaction was complete, nitrogen was introduced into the autoclave, and the product was cooled to obtain a milky white solid. Purify the solid using a Soxhlet extractor for 24 hours, dry it in a vacuum oven at 60°C, and grind it for later use.

[0083] The relative viscosity of semi-aromatic copolyamide resins was tested using the method described in GB 12006.1-89, "Determination of Polyamide Viscosity." Specifically, the relative viscosity η of a polyamide at a concentration of 10 mg / ml was measured in 98% concentrated sulfuric acid at 25 ± 0.01°C. The final product obtained in this example had a relative viscosity of 2.05.

[0084]

[0085] Example 2

[0086] In a vessel equipped with a water separator, a spherical condenser, and a thermometer, 90.4 g of caprolactam, 166.13 g of phthalic acid, 164 g of m-aminobenzoic acid, and 0.15 g of a catalyst were selected according to a preset ratio, and the raw materials were added to a nitrogen-filled reactor. The stirring device was turned on with a stirring speed of 60 r / min. The air reserved in the reactor was replaced with nitrogen at least three times, and 0.02 MPa of nitrogen was reserved as a protective gas. The reactor was heated by circulating heat-conducting oil at a heating rate of 15°C per minute to 180°C. (There is a heat preservation process in this process, in which the reactor is kept warm when the reactor temperature is 90°C for 2 hours. After the heat preservation is completed, the reactor is heated and the pressure rises accordingly. The pressure of the reactor is relieved by releasing the water vapor generated by the reaction of the system). The polycondensation reaction was initiated and maintained at a constant temperature until no more water was produced in the water separator (to promptly remove any water generated in the system). The intermediate product was a slightly yellow, transparent liquid. After the reaction was complete, the temperature was lowered, and the pressure in the autoclave was slowly reduced to 100-120°C over 1.0-1.5 hours. Under inert gas protection, 264 g of N-2-(aminoethyl)-3-aminopropyltriethoxysilane was added. The reaction temperature was 180-200°C, and the reaction was terminated after 30 minutes. After the reaction was complete, nitrogen was introduced into the autoclave, and the product was cooled to obtain a milky white solid. Purify the solid using a Soxhlet extractor for 24 hours, dry it in a vacuum oven at 60°C, and grind it for later use.

[0087] The relative viscosity of the final product was measured to be 2.1.

[0088] Example 3

[0089] In a reactor equipped with a water separator, a spherical condenser, and a thermometer, 67 g of caprolactam, 166.13 g of isophthalic acid, 150 g of p-aminobenzoic acid, and 0.2 g of a catalyst were selected according to a preset ratio, and the raw materials were added to a reactor purged with nitrogen. The stirring device was turned on with a stirring speed of 60 r / min. The air reserved in the reactor was replaced with nitrogen at least three times, and 0.02 MPa of nitrogen was reserved as a protective gas. The reactor was heated and heated at a heating rate of 15°C per minute by circulating heat-conducting oil to 180°C. (There is a heat preservation process in this process, in which the reactor is kept warm when the reactor temperature is 90°C for 2 hours. After the heat preservation is completed, the reactor is heated and the pressure rises accordingly. The pressure of the reactor is relieved by releasing the water vapor generated by the reaction of the system). The polycondensation reaction was initiated and maintained at a constant temperature until no more water was produced in the water separator (to promptly remove any water generated in the system). The intermediate product was a slightly yellow, transparent liquid. After the reaction was complete, the temperature was lowered, and the pressure in the autoclave was slowly reduced to 100-120°C over 1.0-1.5 hours. Under inert gas protection, 169 g of 3-aminopropylmethyldimethoxysilane was added. The reaction temperature was 180-200°C, and the reaction was terminated after 30 minutes. After the reaction was complete, nitrogen was introduced into the autoclave, and the product was cooled to obtain a milky white solid. Purify the solid using a Soxhlet extractor for 24 hours, dry it in a vacuum oven at 60°C, and grind it for later use.

[0090] The relative viscosity of the final product was measured to be 2.00.

[0091] Example 4

[0092] In a reactor equipped with a water separator, a spherical condenser, and a thermometer, 90.4 g of caprolactam, 166.13 g of terephthalic acid, 150 g of p-aminobenzoic acid, and 0.1 g of a catalyst were selected according to a preset ratio, and the raw materials were added to a nitrogen-filled reactor. The stirring device was turned on with a stirring speed of 60 r / min. The air reserved in the reactor was replaced with nitrogen at least three times, and 0.02 MPa of nitrogen was reserved as a protective gas. The reactor was heated and heated at a heating rate of 15°C per minute by circulating heat-conducting oil to 180°C. (There is a heat preservation process in this process, in which the reactor is kept warm when the reactor temperature is 90°C for 2 hours. After the heat preservation is completed, the reactor is heated and the pressure rises accordingly. The pressure of the reactor is relieved by releasing the water vapor generated by the reaction of the system). The polycondensation reaction was initiated and maintained at a constant temperature until no more water was produced in the water separator (to promptly remove any water generated in the system). The intermediate product was a slightly yellow, transparent liquid. After the reaction was complete, the temperature was lowered, and the pressure in the autoclave was slowly reduced to 100-120°C over 1.0-1.5 hours. Under inert gas protection, 84 g of 3-aminopropylmethyldimethoxysilane was added. The reaction temperature was 180-200°C, and the reaction was terminated after 30 minutes. After the reaction was complete, nitrogen was introduced into the autoclave, and the product was cooled to obtain a milky white solid. Purify the solid using a Soxhlet extractor for 24 hours, dry it in a vacuum oven at 60°C, and grind it for later use.

[0093] The relative viscosity of the final product was measured to be 2.00.

[0094] Example 5

[0095] In a vessel equipped with a water separator, a spherical condenser, and a thermometer, 79 g of caprolactam, 166.13 g of phthalic acid, 164 g of p-aminobenzoic acid, and 0.20 g of a catalyst were selected according to a preset ratio, and the raw materials were added to a reactor purged with nitrogen. The stirring device was turned on with a stirring speed of 60 r / min. The air reserved in the reactor was replaced with nitrogen at least three times, and 0.02 MPa of nitrogen was reserved as a protective gas. The reactor was heated and heated at a heating rate of 15°C per minute by circulating heat-conducting oil to 180°C. (There is a heat preservation process in this process, in which the reactor is kept warm when the reactor temperature is 90°C for 2 hours. After the heat preservation is completed, the reactor is heated and the pressure rises accordingly. The pressure of the reactor is relieved by releasing the water vapor generated by the reaction of the system). The polycondensation reaction was initiated and maintained at a constant temperature until no more water was produced in the water separator (to promptly remove any water generated in the system). The intermediate product was a slightly yellowish, transparent liquid. After the reaction was complete, the temperature was lowered, and the pressure in the autoclave was slowly reduced to 100-120°C over 1.0-1.5 hours. Under inert gas protection, 180 g of γ-aminopropyltrimethoxysilane was added. The reaction temperature was 180-200°C, and the reaction was terminated after 30 minutes. After the reaction was complete, nitrogen was introduced into the autoclave, and the product was cooled to obtain a milky white solid. Purify the solid using a Soxhlet extractor for 24 hours, dry it in a vacuum oven at 60°C, and grind it for later use.

[0096] The relative viscosity of the final product was measured to be 2.1.

[0097]

[0098] Test Example 1: 53% nylon PA6, 1% of the compound prepared in Example 1, and 16% of OP1400 halogen-free flame retardant were blended by mass percentage and added through the main feed port. 30% glass fiber was fed through the side feed port. The mixture was melt-blended in an extruder, extruded, pelletized, and dried, and then formed into standard bars on an injection molding machine. The temperatures of the nylon 6 extruder section were 235°C, 240°C, 245°C, 250°C, 245°C, and 240°C, respectively. The barrel speed was fixed at 15 rpm, and the screw speed was 180 rpm. The temperatures of the injection molding machine section were 235°C, 240°C, 245°C, and 250°C, respectively, and the mold temperature was 120°C.

[0099] Test Example 2: 53% nylon PA66, 1% of the compound prepared in Example 2, and 16% of OP1400 halogen-free flame retardant were blended by mass percentage and added through the main feed port. 30% glass fiber was fed through the side feed port. The mixture was melt-blended in an extruder, extruded, pelletized, and dried, and then formed into standard bars on an injection molding machine. The temperatures of the nylon 6 extruder section were 245°C, 250°C, 255°C, 260°C, 245°C, and 260°C, respectively. The barrel speed was fixed at 15 rpm, and the screw speed was 180 rpm. The temperatures of the injection molding machine section were 240°C, 245°C, 250°C, and 260°C, respectively, and the mold temperature was 120°C.

[0100] Test Example 3: 57% semi-aromatic nylon PA6T66, 1% of the compound prepared in Example 3, and 12% of OP1230 halogen-free flame retardant were blended by mass percentage and added through the main feed port. 30% glass fiber was fed through the side feed port. The mixture was melt-blended in an extruder, extruded, pelletized, and dried, and then formed into standard bars on an injection molding machine. The temperatures of the nylon 6 extruder section were 295°C, 300°C, 305°C, 310°C, 280°C, and 320°C, respectively. The barrel speed was fixed at 15 rpm, and the screw speed was 180 rpm. The temperatures of the injection molding machine section were 290°C, 295°C, 300°C, and 310°C, respectively, and the mold temperature was 120°C.

[0101] Test Example 4: 51% semi-aromatic nylon PA9T, 1% of the compound prepared in Example 4, and 18% of OP1400 halogen-free flame retardant were blended by mass percentage and added through the main feed port. 30% glass fiber was added through the side feed port. The mixture was melt-blended in an extruder, extruded, pelletized, and dried, and then formed into standard bars on an injection molding machine. The temperatures of the nylon 6 extruder section were 295°C, 300°C, 305°C, 310°C, 280°C, and 320°C, respectively. The barrel speed was fixed at 15 rpm, and the screw speed was 180 rpm. The temperatures of the injection molding machine section were 290°C, 295°C, 300°C, and 310°C, respectively, and the mold temperature was 120°C.

[0102] Test Example 5: 57% semi-aromatic nylon PA10T, 1% of the compound prepared in Example 5, and 12% of OP1230 halogen-free flame retardant were blended by mass percentage and added through the main feed port. 30% glass fiber was added through the side feed port. The mixture was melt-blended in an extruder, extruded, pelletized, and dried, and then formed into standard bars on an injection molding machine. The temperatures of the nylon 6 extruder section were 295°C, 300°C, 305°C, 310°C, 280°C, and 320°C, respectively. The barrel speed was fixed at 15 rpm, and the screw speed was 180 rpm. The temperatures of the injection molding machine section were 290°C, 295°C, 300°C, and 310°C, respectively, and the mold temperature was 120°C.

[0103] Comparative Example 1: 53% nylon PA6, 1% γ-aminopropyltrioxysilane coupling agent, and 16% OP1400 halogen-free flame retardant were blended, added through the main feed port, and 30% glass fiber was added through the side feed port. The mixture was melt-blended in an extruder, extruded, pelletized, and dried, and then formed into standard bars on an injection molding machine. The temperatures of the nylon 6 extruder section were 235°C, 240°C, 245°C, 250°C, 245°C, and 240°C, respectively. The barrel speed was fixed at 15 rpm, and the screw speed was 180 rpm. The temperatures of the injection molding machine section were 250°C, 245°C, 240°C, and 240°C, respectively, and the mold temperature was 120°C.

[0104] Comparative Example 2: 53% nylon PA66, 1% γ-aminopropyltriethoxysilane coupling agent, and 16% OP1400 halogen-free flame retardant were blended, added through the main feed port, and 30% glass fiber was added through the side feed port. The mixture was melt-blended in an extruder, extruded, pelletized, and dried, and then formed into standard bars on an injection molding machine. The nylon 66 extruder section temperatures were 245°C, 250°C, 255°C, 260°C, 245°C, and 260°C, respectively. The barrel speed was fixed at 15 rpm, and the screw speed was 180 rpm. The injection molding machine section temperatures were 240°C, 245°C, 250°C, and 260°C, respectively, and the mold temperature was 120°C.

[0105] Comparative Example 3: 57% semi-aromatic nylon PA6T66, 1% 3-(phenylamino)propyltriethoxysilane, and 12% OP1230 halogen-free flame retardant were blended, added through the main feed port, and 30% glass fiber was added through the side feed port. The mixture was melt-blended in an extruder, extruded, pelletized, and dried, and then formed into standard bars on an injection molding machine. The nylon 6 extruder section temperatures were set at 295°C, 300°C, 305°C, 310°C, 280°C, and 320°C, respectively. The barrel speed was fixed at 15 rpm, and the screw speed was 180 rpm. The injection molding machine section temperatures were set at 290°C, 295°C, 300°C, and 310°C, respectively, and the mold temperature was 120°C.

[0106] Comparative Example 4: 51% semi-aromatic nylon PA9T, 1% 3-(phenylamino)propyltriethoxysilane, and 18% OP1400 halogen-free flame retardant were blended, added through the main feed port, and 30% glass fiber was added through the side feed port. The mixture was melt-blended in an extruder, extruded, pelletized, and dried, and then formed into standard bars on an injection molding machine. The nylon 6 extruder section temperatures were set at 295°C, 300°C, 305°C, 310°C, 280°C, and 320°C, respectively. The barrel speed was fixed at 15 rpm, and the screw speed was 180 rpm. The injection molding machine section temperatures were set at 290°C, 295°C, 300°C, and 310°C, respectively, and the mold temperature was 120°C.

[0107] Comparative Example 5: 57% semi-aromatic nylon PA10T, 1% 3-aminopropylmethyldimethoxysilane, and 12% OP1230 halogen-free flame retardant were blended, added through the main feed port, and 30% glass fiber was added through the side feed port. The mixture was melt-blended in an extruder, extruded, pelletized, and dried, and then formed into standard bars on an injection molding machine. The nylon 6 extruder section temperatures were set at 295°C, 300°C, 305°C, 310°C, 280°C, and 320°C, respectively. The barrel speed was fixed at 15 rpm, and the screw speed was 180 rpm. The injection molding machine section temperatures were set at 290°C, 295°C, 300°C, and 310°C, respectively, and the mold temperature was 120°C.

[0108] Comparative Example 6: Based on mass percentage, 57% of semi-aromatic nylon PA6T66 and 1% of compound After blending, 12% OP1230 halogen-free flame retardant was added through the main feed port, and 30% glass fiber was fed through the side feed port. After melt blending in an extruder, the mixture was extruded, pelletized, and dried, and then formed into standard strips on an injection molding machine. The nylon 6 extruder section temperatures were 295°C, 300°C, 305°C, 310°C, 280°C, and 320°C, respectively. The barrel speed was fixed at 15 rpm, and the screw speed was 180 rpm. The injection molding machine section temperatures were 290°C, 295°C, 300°C, and 310°C, respectively, and the mold temperature was 120°C.

[0109] Comparative Example 7: 57% semi-aromatic nylon PA6T66, 1% commercially available interfacial binder Y, and 12% OP1230 halogen-free flame retardant were blended, measured by mass percentage, and added through the main feed port. 30% glass fiber was added through a side feed port. The mixture was melt-blended in an extruder, extruded, pelletized, and dried, and then formed into standard bars on an injection molding machine. The PA6T66 extruder section temperatures were set at 295°C, 300°C, 305°C, 310°C, 280°C, and 320°C, respectively. The barrel speed was fixed at 15 rpm, and the screw speed was 180 rpm. The injection molding machine section temperatures were set at 290°C, 295°C, 300°C, and 310°C, respectively, and the mold temperature was 120°C.

[0110] Blank Example 1: 58% semi-aromatic nylon PA6T66 and 12% OP1230 halogen-free flame retardant were blended by mass percentage and added through the main feed port. 30% glass fiber was added through the side feed port. Melt blended in an extruder, the mixture was extruded, pelletized, dried, and then formed into standard bars on an injection molding machine. The temperatures of the nylon 6 extruder sections were set at 295°C, 300°C, 305°C, 310°C, 280°C, and 320°C, respectively. The barrel speed was fixed at 15 rpm, and the screw speed was 180 rpm. The temperatures of the injection molding machine sections were set at 290°C, 295°C, 300°C, and 310°C, respectively, and the mold temperature was 120°C.

[0111] The following detection methods were used for each test example and comparative example using the interface binder of each embodiment:

[0112] The tensile properties are tested according to GB / T1040.1-2006, with a tensile rate of 50 mm / min, under constant temperature and humidity conditions.

[0113] The simply supported beam notched impact strength is tested according to GB / T1043 under constant temperature and humidity experimental conditions.

[0114] Bending strength GB / T9341-2008 test, pressing rate 2mm / min, tested under constant temperature and humidity conditions.

[0115] Rockwell hardness is tested according to ASTM D785-08.

[0116] The test results are shown in the following table.

[0117]

[0118] As shown in the table, adding 1% of the compound in Example 3 (amide-chain silane coupling agent) improved the impact strength by 18.75%, the tensile strength by 10%, the flexural strength by 5%, the flexural modulus by 10%, and the water absorption rate of the material by 25%. Over-temperature reflow soldering in the comparative example will cause blistering, and adding too much coupling agent will reduce the flame retardant effect, and will cause burning and gas trapping during injection molding. The mechanical properties and airtightness of the example are better than those of the commercially available comparative examples 6 and 7. This shows that the amide-chain silane interface binder prepared by the present invention can significantly improve the bonding strength between nylon and glass fiber and inorganic mineral powder. The prepared nylon material has much stronger adhesion to metal than ordinary nylon and better heat resistance than ordinary silane coupling agents. It meets the airtightness requirements of nylon-coated metals (copper, iron, etc.) in high-temperature aging environments. In the halogen-free flame retardant system, it also acts as a flame retardant synergist, improving the flame retardant effect of nylon.

[0119] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by one skilled in the art to which this invention pertains. The terms used in this specification of the present invention are for the purpose of describing specific embodiments only and are not intended to limit the present invention. The term "and / or" as used herein includes any and all combinations of one or more of the associated listed items.

[0120] The technical features of the above embodiments can be combined arbitrarily. To make the description concise, not all possible combinations of the technical features in the above embodiments are described. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.

[0121] The embodiments described above only express several implementation methods of the present invention, which are convenient for understanding the technical solutions of the present invention in a specific and detailed manner, but they cannot be understood as limiting the scope of protection of the invention patent. It should be pointed out that for ordinary technicians in this field, without departing from the concept of the present invention, several variations and improvements can be made, which all fall within the scope of protection of the present invention. It should be understood that the technical solutions obtained by those skilled in the art through logical analysis, reasoning or limited experiments on the basis of the technical solutions provided by the present invention are all within the scope of protection of the claims attached to the present invention. Therefore, the scope of protection of the patent of the present invention shall be based on the content of the attached claims, and the description can be used to interpret the content of the claims.

Claims

1. A compound, characterized in that The general structural formula is: ; Wherein, R1 is selected from any of the groups shown in (1-1) to (1-2) , R a Each occurrence is independently selected from -H, -D, carboxyl, C2-C5 alkyl substituted with carboxyl, or unsubstituted C1-C5 alkyl, and at least one R a is selected from carboxyl or C2~C5 alkyl substituted by carboxyl, R2 is -R b -or-R b -NH-R b -, R b Each occurrence is independently selected from C1 to C5 alkylene, R3, R4 and R5 are independently selected from C1~C5 alkyl or C1~C5 alkoxy, n is an integer between 10 and 20.

2. The compound according to claim 1, characterized in that The relative molecular weight of the compound is 2000-4000.

3. The compound according to claim 1 or 2, characterized in that The compound satisfies one or more of the following characteristics: (1) R a Each occurrence is selected from -H or carboxyl, at least one R a is carboxyl; (2) R2 is -R b -or-R b -NH-R b -, R b Each occurrence is independently selected from a C1-C3 straight chain alkylene group; (3) R3, R4 and R5 are independently selected from C1~C3 alkyl or C1~C3 alkoxy.

4. The compound according to claim 1 or 2, characterized in that The structure of the compound is one of the formulas (2-1) and (2-5): 。 5. A method for preparing the compound according to any one of claims 1 to 4, characterized in that: The following steps are involved: Mixed Compound A Compound B and compound C , heating to 160° C. to 180° C., the compound B undergoes a ring-opening reaction and a polycondensation reaction, and then undergoes a first dehydration condensation reaction with the compound A and the compound C, respectively, to prepare an intermediate product; In an inert gas atmosphere at a temperature of 180°C to 200°C, the intermediate product and compound D are mixed. , the intermediate product and the compound D undergo a second dehydration condensation reaction.

6. The preparation method according to claim 5, characterized in that: Meet one or more of the following characteristics: (1) The molar ratio of the compound A, the compound B and the compound C is 1:(0.5-0.8):(1-1.2); (2) The compound A is selected from one or more of terephthalic acid, isophthalic acid, phthalic acid, 4,4'-biphenyl dicarboxylic acid and naphthalene dicarboxylic acid; (3) The compound D is a silane coupling agent having a primary amine terminal group.

7. The preparation method according to claim 6, characterized in that: The compound D is selected from one or more of N-2-(aminoethyl)-3-aminopropyltrimethoxysilane, N-2-(aminoethyl)-3-aminopropyltriethoxysilane, γ-aminopropyltrimethoxysilane, γ-aminopropyltriethoxysilane, 3-aminopropylmethyldimethoxysilane, 3-aminopropylmethyldiethoxysilane and N,N-dimethyl-3-aminopropyltrimethoxysilane.

8. The preparation method according to any one of claims 5 to 7, characterized in that: Meet one or more of the following characteristics: (1) The reaction conditions for preparing the intermediate product include: the reaction environment contains a catalyst, and the amount of the catalyst added is 0.03% to 0.05% of the total mass of the compound A, the compound B and the compound C; (2) The reaction conditions of the second dehydration condensation reaction include: the molar ratio of the intermediate product to the compound D is 1.05-0.

95.

9. An interface bonding agent, characterized in that: Contains the compound according to any one of claims 1 to 4.

10. Use of the compound according to any one of claims 1 to 4 or the interface binder according to claim 9 in the preparation of a high temperature resistant nylon modified product.