Copper-plated conductive film
By constructing a composite layer structure on both sides of the substrate of the copper-plated conductive film, using a hybrid target blackening layer and a metal Si layer, the problem of insufficient oxidation resistance of the copper-plated conductive film is solved, and higher oxidation resistance and attachment Focus on adapting to the use needs of various environments.
Patent Information
- Application Number
- CN202411138244.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-19
- Publication Date
- 2024-11-26
AI Technical Summary
The top blackening layer of the existing copper-plated conductive film has weak oxidation resistance and is prone to oxidation and discoloration, resulting in a decrease in productivity.
A composite layer structure is constructed on both sides of the substrate, a hybrid target blackening layer and a metal Si layer are arranged, and a base layer and a resin hard layer are combined to improve oxidation resistance and adhesion.
It significantly improves the oxidation resistance of the copper-plated conductive film, avoids oxidation and discoloration, enhances adhesion and physical properties, and adapts to different environments.
Smart Images

Figure CN119019736A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of film materials, and in particular relates to a copper-plated conductive film. Background Art
[0002] Copper-plated conductive film is mainly used in large-size touch screens due to its low resistance value of 0.04-0.3Ω. It can reduce losses while improving the touch sensitivity of the screen, such as all-in-one machines, large-size notebook computers, interactive teaching platforms, commercial displays and other devices. The top black layer of copper-plated conductive film in the prior art is usually made of pure copper target material, but the black layer prepared by pure copper target material has weak oxidation resistance. After coating, the black layer oxidizes and discolors slightly faster, and there are unstable factors in long-term storage, which may reduce the production yield of the client.
[0003] The information disclosed in this background technology section is only intended to enhance the understanding of the overall background of the invention and should not be regarded as an acknowledgment or any form of suggestion that the information constitutes the prior art already known to a person skilled in the art. Summary of the invention
[0004] The object of the present invention is to provide a copper-plated conductive film which has good anti-oxidation performance and is not easily oxidized and discolored.
[0005] In order to achieve the above object, a specific embodiment of the present invention provides a copper-plated conductive film, which includes a substrate and a composite layer structure constructed on both sides of the substrate; the composite layer structure includes:
[0006] The first structure comprises a base layer, a black layer, a metal functional layer, a mixed target black layer, and a metal Si layer stacked in sequence from the inside to the outside on one side of the substrate; wherein the mixed target black layer comprises 80-98wt% copper and 2-20wt% stainless steel;
[0007] The second structure includes a base layer, a blackening layer, a metal functional layer, a mixed target blackening layer, and a metal Si layer stacked in sequence from the inside to the outside from the other side of the substrate; wherein the mixed target blackening layer includes 80-98wt% copper and 2-20wt% stainless steel.
[0008] In one or more embodiments of the present invention, the thickness of the blackening layer of the first structure and / or the second structure is between 5nm and 100nm; and / or the blackening layer of the first structure and / or the second structure is a copper oxynitride layer.
[0009] In one or more embodiments of the present invention, the thickness of the metal functional layer of the first structure and / or the second structure is between 100 nm and 1000 nm; and / or the metal functional layer of the first structure and / or the second structure is a Cu layer.
[0010] In one or more embodiments of the present invention, the thickness of the mixed target blackening layer of the first structure and / or the second structure is between 10 nm and 150 nm.
[0011] In one or more embodiments of the present invention, the base layer of the first structure and / or the second structure is selected from one of SiO2, Si, MgF2, SiO, HfO2, SnO2 and Y2O3; and / or the thickness of the base layer is between 0.1nm-10nm.
[0012] In one or more embodiments of the present invention, the thickness of the metal Si layer of the first structure and / or the second structure is between 0.1 nm and 5 nm.
[0013] In one or more embodiments of the present invention, the substrate is selected from one of PET, TAC, SRF, COP and PC; and / or the thickness of the substrate is between 5.7 μm and 250 μm.
[0014] In one or more embodiments of the present invention, a resin hardening layer is provided between the substrate and the primer layer of the first structure and / or the second structure; and / or the thickness of the resin hardening layer is between 5nm and 150nm.
[0015] In one or more embodiments of the present invention, the first structure and the second structure are symmetrically arranged on both sides of the substrate.
[0016] In one or more embodiments of the present invention, a protective layer is provided on the surface of the first structure and / or the second structure.
[0017] Compared with the prior art, the copper-plated conductive film of the present invention can improve the anti-oxidation ability of the copper-plated conductive film and avoid oxidative discoloration of the copper-plated conductive film by constructing a composite layer structure on both sides of the substrate and arranging a mixed target blackening layer in the composite layer structure. The surface of the mixed target blackening layer is provided with a metal Si layer, which can further improve the anti-oxidation property of the copper-plated conductive film. In addition, the provision of a primer layer can improve the adhesion of the copper conductive film. BRIEF DESCRIPTION OF THE DRAWINGS
[0018] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the prior art descriptions are briefly introduced below. Obviously, the drawings described below are only some embodiments recorded in the present invention, and for ordinary technicians in this field, other drawings can be obtained based on these drawings without creative work.
[0019] Figure 1 It is a schematic diagram of a copper-plated conductive film in one embodiment of the present invention;
[0020] Figure 2 is a reflection curve of Example 1 in one embodiment of the present invention;
[0021] Figure 3 It is the reflection curve of comparative example 4 in one embodiment of the present invention.
[0022] Description of main reference numerals:
[0023] 1-substrate, 2-priming layer, 3-blackening layer, 4-metal functional layer, 5-mixed target blackening layer, 6-metal Si layer, A-first structure, B-second structure. DETAILED DESCRIPTION
[0024] In order to enable those skilled in the art to better understand the technical solutions in the present invention, the technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work should fall within the scope of protection of the present invention.
[0025] like Figure 1 As shown, a copper-plated conductive film in one embodiment of the present invention includes a substrate 1 and a composite layer structure constructed on both sides of the substrate 1. The composite layer structure includes: a first structure A and a second structure B. The first structure A includes a base layer 2, a blackening layer 3, a metal functional layer 4, a mixed target blackening layer 5, and a metal Si layer 6 stacked in sequence from the inside to the outside on one side of the substrate 1. Among them, the mixed target blackening layer 5 includes 80-98wt% copper and 2-20wt% stainless steel. The second structure B includes a base layer 2, a blackening layer 3, a metal functional layer 4, a mixed target blackening layer 5, and a metal Si layer 6 stacked in sequence from the inside to the outside on the other side of the substrate 1; Among them, the mixed target blackening layer 5 includes 80-98wt% copper and 2-20wt% stainless steel.
[0026] In the above embodiment, the copper-plated conductive film of the present invention can improve the oxidation resistance of the copper-plated conductive film and avoid oxidation discoloration of the copper-plated conductive film by constructing a composite layer structure on both sides of the substrate 1 and arranging a mixed target blackening layer 5 in the composite layer structure.
[0027] In one embodiment, both the first structure A and the second structure B include a base layer 2, a black layer 3, a metal functional layer 4, a mixed target black layer 5, and a metal Si layer 6 stacked in sequence from the inside to the outside. The base layer 2 of the first structure A can be selected from one of SiO2, Si, MgF2, SiO, HfO2, SnO2 and Y2O3. The thickness of the base layer 2 of the first structure A is between 0.1nm and 10nm.
[0028] The base layer 2 of the second structure B can be selected from one of SiO2, Si, MgF2, SiO, HfO2, SnO2 and Y2O3, and the thickness of the base layer 2 of the second structure B is between 0.1nm and 10nm. The base layer 2 can increase the adhesion of the substrate 1, and the use of the above base layer 2 can improve the physical properties of the film surface of the copper-plated conductive film.
[0029] The blackening layer 3 is magnetron sputtered on the surface of the base layer 2. The thickness of the blackening layer 3 of the first structure A can be between 5nm and 100nm. The thickness of the blackening layer 3 of the second structure B can be between 5nm and 100nm. The blackening layer 3 of the first structure A can be a copper oxynitride layer. The blackening layer 3 of the second structure B can be a copper oxynitride layer. The copper oxynitride layer as the blackening layer 3 has a certain anti-oxidation effect and better color stability during the coating process.
[0030] The metal functional layer 4 is plated on the surface of the black layer 3 to reduce the square resistance of the copper-plated conductive film. In one embodiment, the metal functional layer 4 of the first structure A can be a Cu layer. The metal functional layer 4 of the second structure B can be a Cu layer. The thickness of the metal functional layer 4 of the first structure A can be between 100nm and 1000nm. The thickness of the metal functional layer 4 of the second structure B can be between 100nm and 1000nm.
[0031] The hybrid target blackening layer 5 is plated on the surface of the metal functional layer 4. The thickness of the hybrid target blackening layer 5 of the first structure A may be between 10 nm and 150 nm. The thickness of the hybrid target blackening layer 5 of the second structure B may also be between 10 nm and 150 nm.
[0032] By controlling the thickness of the mixed target blackening layer 5 of the first structure A and the second structure B and using a mixed target material of stainless steel and copper to prepare the mixed target blackening layer 5, the mixed target blackening layer 5 can have stronger oxidation resistance than the pure copper blackening layer in the prior art.
[0033] The metal Si layer 6 is plated on the surface of the hybrid target blackening layer 5. The thickness of the metal Si layer 6 of the first structure A can be between 0.1nm and 5nm. The thickness of the metal Si layer 6 of the second structure B can be between 0.1nm and 5nm. The metal Si layer 6 is arranged on the surface of the hybrid target blackening layer 5, and also has an anti-oxidation effect, thereby further improving the anti-oxidation property of the copper-plated conductive film.
[0034] In one embodiment, the substrate 1 is selected from PET, TAC, SRF, COP and PC, wherein the thickness of the substrate 1 may be between 5.7 μm and 250 μm.
[0035] In order to improve the hardness of the copper-plated conductive film, a resin hardening layer may be provided between the substrate 1 and the base layer 2 of the first structure A. A resin hardening layer may also be provided between the substrate 1 and the base layer 2 of the second structure B. The thickness of the resin hardening layer may be between 5nm and 150nm.
[0036] In one embodiment, a protective layer may be provided on the surface of the first structure A. A protective layer may be provided on the surface of the second structure B. The protective layer may further prevent the copper-plated conductive film from being oxidized due to humidity in the air during storage.
[0037] In one embodiment, the first structure A and the second structure B may be symmetrically arranged on both sides of the substrate 1 , and the thicknesses of corresponding layers in the first structure A and the second structure B may be unequal or equal.
[0038] The present invention is further described below in conjunction with embodiments and comparative examples.
[0039] Example 1
[0040] Substrate 1: PET, 20 μm;
[0041] First structure A: Base layer 2: MgF2 layer, thickness 2nm. Black layer 3: Copper oxynitride layer, thickness 10nm. Metal functional layer 4: Cu layer, thickness 200nm. Mixed target black layer 5: 85wt% copper, 15wt% stainless steel, thickness 15nm. Metal Si layer 6: thickness 2nm.
[0042] Second structure B: Base layer 2: MgF2 layer, thickness 2nm. Black layer 3: Copper oxynitride layer, thickness 10nm. Metal functional layer 4: Cu layer, thickness 200nm. Mixed target black layer 5: 85wt% copper, 15wt% stainless steel, thickness 15nm. Metal Si layer 6: thickness 2nm.
[0043] Comparative Example 1
[0044] Substrate: PET, 20 μm;
[0045] First structure A: Base layer: MgF2 layer, thickness 2nm. Black layer: Copper oxynitride layer, thickness 10nm. Metal functional layer: Cu layer, thickness 200nm. Mixed target black layer: 70wt% copper, 30wt% stainless steel, thickness 15nm. Metal Si layer: thickness 2nm.
[0046] Second structure B: Base layer: MgF2 layer, thickness 2nm. Black layer: Copper oxynitride layer, thickness 10nm. Metal functional layer: Cu layer, thickness 200nm. Mixed target black layer: 70wt% copper, 30wt% stainless steel, thickness 15nm. Metal Si layer: thickness 2nm.
[0047] Comparative Example 2
[0048] Substrate: PET, 20 μm;
[0049] First structure: Base layer: MgF2 layer, thickness 2nm. Black layer: Copper oxynitride layer, thickness 10nm. Metal functional layer: Cu layer, thickness 200nm. Mixed target black layer: 60wt% copper, 40wt% stainless steel, thickness 15nm. Metal Si layer: thickness 2nm.
[0050] Second structure: Base layer: MgF2 layer, thickness 2nm. Black layer: Copper oxynitride layer, thickness 10nm. Metal functional layer: Cu layer, thickness 200nm. Mixed target black layer: 60wt% copper, 40wt% stainless steel, thickness 15nm. Metal Si layer: thickness 2nm.
[0051] Comparative Example 3
[0052] Substrate: PET, 20 μm;
[0053] First structure: Base layer: MgF2 layer, thickness 2nm. Black layer: Copper oxynitride layer, thickness 10nm. Metal functional layer: Cu layer, thickness 200nm. Mixed target black layer: 99wt% copper, 1wt% stainless steel, thickness 15nm. Metal Si layer: thickness 2nm.
[0054] Second structure: Base layer: MgF2 layer, thickness 2nm. Black layer: Copper oxynitride layer, thickness 10nm. Metal functional layer: Cu layer, thickness 200nm. Mixed target black layer: 99wt% copper, 1wt% stainless steel, thickness 15nm. Metal Si layer: thickness 2nm.
[0055] Comparative Example 4
[0056] Substrate: PET, 20 μm;
[0057] First structure: Base layer: MgF2 layer, thickness 5nm. Black layer: Copper oxynitride layer, thickness 10nm. Metal functional layer: Cu layer, thickness 200nm. Mixed target black layer: 100wt% copper, thickness 15nm. Metal layer: Al layer, thickness 2nm.
[0058] Second structure: Base layer: MgF2 layer, thickness 5nm. Black layer: Copper oxynitride layer, thickness 10nm. Metal functional layer: Cu layer, thickness 200nm. Mixed target black layer: 100wt% copper, thickness 15nm. Metal layer: Al layer, thickness 2nm.
[0059] The copper-plated conductive films of Example 1 and Comparative Examples 1-3 were tested. The test method is as follows: the copper-plated conductive films of Example 1 and Comparative Examples 1-3 were cut into A4 paper size, and then cut with a grid knife after being placed under different conditions for a period of time, and then 3M company 600 type tape was used. After being pressed and pressed, the tape was pulled off after standing for more than 30 seconds. No peeling was 5B; slight peeling was 3B-4B, barely judged OK; 2B and below were judged unqualified. The test conditions are as follows: ① Boiled in 100℃ water for 0.5h; ② Boiled in 100℃ water for 1h; ③ Placed in a high temperature of 85℃ and a high humidity of 85% environment for 5 days; ④ Placed in a high temperature of 85℃ and a high humidity of 85% environment for 10 days; ⑤ Placed at a high temperature of 95℃ for 5 days; ⑥ Placed at a high temperature of 95℃ for 10 days; ⑦ Placed at a low temperature of -40℃ for 5 days; ⑧ Placed at a low temperature of -40℃ for 10 days. The specific test results are shown in Table 1 below.
[0060] Table 1 Hundred-grid test results of Example 1 and Comparative Examples 1-3
[0061]
[0062]
[0063] It can be seen from Table 1 that the copper-plated conductive film of Example 1 has better adhesion under different environments than the copper-plated conductive films of Comparative Examples 1-3, and can adapt to different usage environments.
[0064] The film material of Example 1 was subjected to a color test. The test method and conditions are as follows: Take a finished product with a width of 200-400 mm and a length of 1200 mm, hang it on the wall, place it at room temperature for 50 days, and test the surface color with a Konica colorimeter. If the surface blackening color does not change, it is judged to be qualified. The test results are shown in Table 2 below.
[0065] Table 2 Color test results of copper-plated conductive film of Example 1
[0066]
[0067] It can be seen from Table 2 above that the copper-plated conductive film of Example 1 has almost no color change when placed at room temperature and has better anti-oxidation performance.
[0068] The copper-plated conductive films of Example 1 and Comparative Example 4 were subjected to reflection test, haze test and square resistance test. The reflection test method is: the copper-plated conductive films of Example 1 and Comparative Example 4 are placed flat on the Olympus test table, and the reflection curves of the left, middle and right points of the film are tested. The test results are shown in Table 3 and Figure 2 and Figure 3 shown.
[0069] Haze test: The copper-plated conductive films of Example 1 and Comparative Example 4 were etched with a dedicated copper film etching solution, and the transmittance and haze were tested after etching. The test results are shown in Table 3.
[0070] Sheet resistance test: The copper-plated conductive films of Example 1 and Comparative Example 4 were placed flat on a test bench, and the surface sheet resistance of 13 points from left to right was tested using a sheet resistance meter. The test results are shown in Table 4.
[0071] Table 3 Reflection test and haze test results of copper-plated conductive films of Example 1 and Comparative Example 4
[0072]
[0073] Table 4 Square resistance test results of copper-plated conductive films of Example 1 and Comparative Example 4
[0074]
[0075] As shown in Table 3 and Figure 2-3 As shown, the average reflectivity of the left, middle and right points of the copper-plated conductive film of comparative example 4 between 380-780nm is 13.15%, 12.78% and 13.04% respectively. The average reflectivity of the left, middle and right points of the copper-plated conductive film of embodiment 1 between 380-780nm is 13.41%, 12.93% and 13.12% respectively. As shown in Tables 3 and 4, it is shown that the optical performance of the copper-plated conductive film of embodiment 1 is slightly better than that of the copper-plated conductive film of comparative example 4, and the square resistance performance is similar. However, it can be seen from Tables 1 and 2 that embodiment 1 has better adhesion and oxidation resistance.
[0076] In summary, the copper-plated conductive film of the present invention can improve the oxidation resistance of the copper-plated conductive film and prevent the copper-plated conductive film from being oxidized and discolored by constructing a composite layer structure on both sides of the substrate 1 and arranging a mixed target blackening layer 5 in the composite layer structure. The surface of the mixed target blackening layer 5 is provided with a metal Si layer 6, which can further improve the oxidation resistance of the copper-plated conductive film. In addition, the provision of a primer layer 2 can improve the adhesion of the copper conductive film.
[0077] It will be apparent to those skilled in the art that the invention is not limited to the details of the exemplary embodiments described above and that the invention can be implemented in other specific forms without departing from the spirit or essential features of the invention. Therefore, the embodiments should be considered exemplary and non-limiting in all respects, and the scope of the invention is defined by the appended claims rather than the foregoing description, and it is intended that all variations falling within the meaning and scope of the equivalent elements of the claims be included in the invention. Any reference numeral in a claim should not be considered as limiting the claim to which it relates.
[0078] In addition, it should be understood that although the present specification is described according to implementation modes, not every implementation mode contains only one independent technical solution. This description of the specification is only for the sake of clarity. Those skilled in the art should regard the specification as a whole. The technical solutions in each embodiment may also be appropriately combined to form other implementation modes that can be understood by those skilled in the art.
Claims
1. A copper-plated conductive film, characterized in that: The invention comprises a substrate and a composite layer structure constructed on both sides of the substrate; the composite layer structure comprises: The first structure comprises a base layer, a black layer, a metal functional layer, a mixed target black layer, and a metal Si layer stacked in sequence from the inside to the outside on one side of the substrate; wherein the mixed target black layer comprises 80-98wt% copper and 2-20wt% stainless steel; The second structure includes a base layer, a blackening layer, a metal functional layer, a mixed target blackening layer, and a metal Si layer stacked in sequence from the inside to the outside from the other side of the substrate; wherein the mixed target blackening layer includes 80-98wt% copper and 2-20wt% stainless steel.
2. The copper-plated conductive film according to claim 1, characterized in that: The thickness of the blackening layer of the first structure and / or the second structure is between 5nm and 100nm; and / or the blackening layer of the first structure and / or the second structure is a copper oxynitride layer.
3. The copper-plated conductive film according to claim 1, characterized in that: The thickness of the metal functional layer of the first structure and / or the second structure is between 100 nm and 1000 nm; and / or the metal functional layer of the first structure and / or the second structure is a Cu layer.
4. The copper-plated conductive film according to claim 1, characterized in that: The thickness of the mixed target blackening layer of the first structure and / or the second structure is between 10 nm and 150 nm.
5. The copper-plated conductive film according to claim 1, characterized in that: The base layer of the first structure and / or the second structure is selected from one of SiO2, Si, MgF2, SiO, HfO2, SnO2 and Y2O3; and / or the thickness of the base layer is between 0.1nm and 10nm.
6. The copper-plated conductive film according to claim 1, characterized in that: The thickness of the metal Si layer of the first structure and / or the second structure is between 0.1 nm and 5 nm.
7. The copper-plated conductive film according to claim 1, characterized in that: The substrate is selected from one of PET, TAC, SRF, COP and PC; and / or the thickness of the substrate is between 5.7 μm and 250 μm.
8. The copper-plated conductive film according to claim 1, characterized in that: A resin hardening layer is provided between the substrate and the primer layer of the first structure and / or the second structure; and / or the thickness of the resin hardening layer is between 5nm and 150nm.
9. The copper-plated conductive film according to claim 1, characterized in that: The first structure and the second structure are symmetrically arranged on both sides of the substrate.
10. The copper-plated conductive film according to claim 1, characterized in that: A protective layer is provided on the surface of the first structure and / or the second structure.