Surface amino modified piezoelectric polyvinylidene fluoride trifluoroethylene as well as preparation and application thereof

By performing amino modification on the surface of polyvinylidene fluoride trifluoroethylene, piezoelectric materials with adjustable potential are prepared, which solves the limitations and performance damage problems of surface modification methods in the prior art, and achieves efficient organization in the field of biomedical medicine Repair and regeneration effects.

CN119019739APending Publication Date: 2024-11-26ZHEJIANG UNIV

Patent Information

Application Number
CN202411130985.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-16
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

The existing polyvinylidene fluoride trifluoroethylene (PVTF) has limited surface modification methods in the biomedical field, and common methods may damage their piezoelectric properties and mechanical properties, or require harsh conditions such as high temperature and radiation, and the surface potential is not easy. Regulation makes it difficult to adapt to the diverse cellular microenvironment.

Method used

By performing amino modification on the PVTF surface and using polarization treatment and covalent bonding methods, amino modified piezoelectric polyvinylidene fluoride trifluoroethylene with adjustable surface potential can be prepared, which can achieve surface modification under mild conditions. Provides static and dynamic electrical signal stimulation, suitable for biomedical implants.

Benefits of technology

It achieves high stability of surface potential and retains piezoelectric effect, avoids complex operation and infection risks of external power supply, is suitable for a variety of cellular microenvironments, promotes tissue repair and regeneration, and is simple and easy to prepare.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure HDA0004997803700000011
    Figure HDA0004997803700000011
  • Figure HDA0004997803700000012
    Figure HDA0004997803700000012
  • Figure HDA0004997803700000021
    Figure HDA0004997803700000021
Patent Text Reader

Abstract

The invention discloses surface amino modified piezoelectric polyvinylidene fluoride trifluoroethylene as well as preparation and application thereof, and belongs to the field of biomedical materials. The surface amino-modified piezoelectric polyvinylidene fluoride trifluoroethylene is composed of PVTF subjected to polarization treatment and amino functional groups grafted on the surface of the PVTF, the surface potential of the surface amino-modified piezoelectric polyvinylidene fluoride trifluoroethylene is adjustable, meanwhile, the PVTF has high piezoelectricity, static surface potential and dynamic piezoelectric potential stimulation can be applied to cells on the surface of a material at the same time, and the surface amino-modified piezoelectric polyvinylidene fluoride trifluoroethylene can be applied to cells on the surface of the material. The material can be used as a biomedical implant or an implant surface modification coating, can regulate and control cell behaviors, and especially can promote the repair and regeneration of bone tissues.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of biomedical materials, and in particular to amino-modified piezoelectric polyvinylidene fluoride trifluoroethylene and preparation and application thereof. Background Art

[0002] Natural bone is composed of organic and inorganic phases. The most abundant component in the organic matrix is ​​type I collagen, and it also includes some amorphous matrices such as fibronectin. These organic components play an extremely important role in bone mineralization, cell signal transduction, and tissue metabolism. The main components of the inorganic phase are hydroxyapatite and some metal ions (such as calcium, magnesium, sodium, phosphorus, chloride, etc.), which often provide mechanical support for natural bone. Bone tissue is a natural piezoelectric body with intrinsic electrical activity. Natural bone tissue is in a state of dynamic stress, and appropriate external force stimulation is of great significance to its growth and repair: mechanical stimulation will affect bone growth, specifically, appropriate mechanical stimulation promotes bone formation, and bone resorption will occur without external force stimulation for a long time. Under the stimulation of external force, bone tissue as a piezoelectric body can complete the conversion of mechanical energy into electrical energy, which is a necessary condition for maintaining the normal physiological activity and metabolism of natural bone tissue. The current mainstream view on the source of the piezoelectric effect of bone is that the piezoelectric effect of bone is caused by the breakage and sliding of a large number of collagen fibers in the bone when the bone is subjected to force, and the formation of asymmetric collagen molecules in natural bone tissue. The piezoelectricity of natural bone tissue has inspired people to use piezoelectric materials as bone repair materials to mimic the piezoelectric effect of natural bone. Giving electrical stimulation to the bone defect through piezoelectric materials and restoring its normal electrical environment will induce the bone's repair ability and promote the healing of bone defects, thereby achieving the purpose of bone repair and regeneration. This is the main design concept of bionic electroactive bone repair materials.

[0003] A large number of research reports have confirmed that piezoelectric materials have the potential to be used for bone defect repair and treatment. Polyvinylidene fluoride trifluoroethylene (P(VDF-TrFE), PVTF) is a type of piezoelectric material with good flexibility and stability. Its excellent piezoelectric and mechanical properties make it more advantageous in clinical bone defect repair applications. Studies have reported that it has a promoting effect on cell osteogenic differentiation and bone defect repair. Stem cells can be induced to differentiate into osteoblasts by implanting polarized PVTF membranes. However, studies have also reported that PVTF membrane materials reduce the expression of osteogenesis-related genes. The above completely opposite results are presented because bone healing is a very complex physiological process. The actual cell microenvironment is complex. In addition to electrical signals, it also includes cells, extracellular matrix, secreted factors, temperature, pH and other factors. On the one hand, the surface potential of electroactive biomaterials will affect cell adhesion, proliferation and differentiation. Especially in the early stages of cell response, the charged surface significantly affects the adhesion state, proliferation and migration of cells. Moreover, surface potential also plays an important role in the adsorption of proteins on the surface of materials, because proteins are amphiphilic molecules and the charge they carry depends on the surrounding pH value. The electrical properties of proteins are also different at different pH values. On the other hand, the surface properties of materials, such as the surface morphology of materials, have a great influence on their bone integration ability. Compared with the macro- and micro-scale implant surfaces, bone cells are more adapted to the nano-roughness of implant surfaces. Therefore, further modification of the surface of electroactive materials to simulate or adapt to various cellular microenvironmental factors is expected to achieve better effects in promoting bone tissue repair and regeneration.

[0004] However, due to the strong polarity of its carbon-fluorine bond, the surface modification methods available for polyvinylidene fluoride trifluoroethylene in the biomedical field are very limited. At present, there are two main types of surface modification methods for polyvinylidene fluoride trifluoroethylene: one is to use dopamine, tannin and other adhesive substances containing catechol groups to modify the surface by using intermolecular interaction forces. This method introduces additional adhesive substances during the application process, and its biological effects and biocompatibility need to be considered in the biomedical field. In addition, it is also necessary to consider the binding strength and shedding ratio of the adhesive substance, and whether there is a possibility of failure during the application process. The other type is to modify by covalent bonds, but the CF bond length in the PVTF molecule is short, and its bond energy is high. Its activation needs to be carried out under more harsh conditions, such as fluorine sulfonation, electron beam radiation, plasma treatment, etc., which often involve special reaction conditions such as high temperature, irradiation or highly toxic reagents, which hinders its application in the biomedical field. In addition, the reaction conditions used in the above-mentioned modification methods may also damage the piezoelectric properties and mechanical properties of polyvinylidene fluoride trifluoroethylene. Summary of the invention

[0005] In view of this, the purpose of the present invention is to provide a surface amino-modified piezoelectric polyvinylidene fluoride trifluoroethylene and its preparation and application. The present invention realizes the modification of the surface of polyvinylidene fluoride trifluoroethylene under mild conditions, and the surface potential of the obtained surface amino-modified piezoelectric polyvinylidene fluoride trifluoroethylene is adjustable, which can provide static electrical signal stimulation to cells; at the same time, under the action of external mechanical deformation, piezoelectric potential can be generated through the piezoelectric effect to apply dynamic electrical signal stimulation to cells. The surface amino-modified piezoelectric polyvinylidene fluoride trifluoroethylene can be used as a biomedical implant to promote corresponding tissue repair and regeneration.

[0006] In order to achieve the above object, the present invention adopts the following technical solutions:

[0007] The invention provides a piezoelectric polyvinylidene fluoride trifluoroethylene with surface amino groups modified, which is composed of polarized PVTF and amino functional groups grafted on the surface of the PVTF.

[0008] In some specific examples of the present invention, the piezoelectric coefficient d of the polarized PVTF is 33 Satisfy: -25pC / N≤d 33 <0pC / N or 0pC / N<d 33 ≤25pC / N.

[0009] Preferably, the piezoelectric coefficient d of the polarized PVTF is 33 Satisfy -15pC / N≤d 33 ≤-5pC / N or 5pC / N≤d 33 ≤15pC / N.

[0010] At the same time, the present invention also provides a method for preparing the above-mentioned surface amino-modified piezoelectric polyvinylidene fluoride trifluoroethylene, comprising the following steps:

[0011] (1) adding PVTF powder to N,N-dimethylformamide solvent at a solid-liquid ratio of 1 g: (4-10) mL, stirring for 2-4 hours to obtain a PVTF solution; forming a film of the PVTF solution on a substrate, and then heat treating at 180° C. to 240° C. for 0.5 hours to 2 hours to obtain a PVTF film, wherein the thickness of the PVTF film is 30-80 μm;

[0012] (2) performing polarization treatment on the PVTF film obtained in step (1) to obtain a polarized PVTF film;

[0013] (3) placing the polarized PVTF membrane obtained in step (2) in an aqueous solution of an organic amino base, heating it in a water bath to 30° C. to 70° C., reacting it for 0.5 h to 12 h, then washing it with deionized water and drying it to obtain the target product.

[0014] In some specific examples of the present invention, in step (2), the polarization treatment is a contact polarization treatment.

[0015] In some specific examples of the present invention, in step (2), the high voltage electric field intensity of the contact polarization treatment is 30 to 90 kV / mm, and the polarization treatment time is 3 to 10 min.

[0016] In some specific embodiments of the present invention, in step (2), the piezoelectric coefficient d of the PVTF film layer obtained by polarization treatment is 33 Satisfy: -25pC / N≤d 33 <0pC / N or 0pC / N<d 33 ≤25pC / N.

[0017] Preferably, in step (2), the piezoelectric coefficient d of the PVTF film obtained by polarization treatment is 33 Satisfy: -15pC / N≤d 33 ≤-5pC / N or 5pC / N≤d 33 ≤15pC / N.

[0018] In some specific examples of the present invention, in step (3), the organic amino-containing base is monoethanolamine, ethylenediamine, isopropanolamine or isobutanolamine.

[0019] In some specific examples of the present invention, in step (3), the concentration of the aqueous solution of the organic amino base is 5 to 16.7 mol / L, preferably 16 mol / L.

[0020] In addition, the present invention also provides the application of the above-mentioned surface amino-modified piezoelectric polyvinylidene fluoride trifluoroethylene, for example, in the preparation of biomedical implants, and is particularly useful in the field of promoting tissue repair, such as in the preparation of bone defect repair materials or in promoting osteogenic differentiation, etc.

[0021] Compared with the prior art, the present invention has the following beneficial effects:

[0022] (1) The surface amino-modified piezoelectric polyvinylidene fluoride trifluoroethylene of the present invention has an adjustable surface potential, and the amino groups are covalently bonded to the surface of the material, so that the surface potential has high stability and can continue to play a role. Different cells and tissues have different electrical microenvironments, and different states of the same tissue also have different electrical microenvironments. Therefore, the adjustable surface potential of the material can meet the needs of various application scenarios.

[0023] (2) The surface amino-modified piezoelectric polyvinylidene fluoride trifluoroethylene of the present invention has a certain piezoelectric effect, which can generate piezoelectric potential under the mechanical deformation caused by daily physiological activities, and apply electrical stimulation to the tissue, thereby avoiding the complicated operation caused by electrical stimulation through an external power source and the risk of infection caused by leaving connecting electrodes at the implanted tissue.

[0024] (3) The preparation method of the present invention is simple and easy to implement, has high operability, does not require special conditions or equipment, and is easy to implement. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1 It is the Fourier infrared spectra of the target product obtained in Example 1 and the final product obtained in Comparative Example 1.

[0026] Figure 2 It is the photoelectron spectrum of the target product obtained in Example 1 and the final product obtained in Comparative Example 1.

[0027] Figure 3 These are the water contact angle test results of the target product obtained in Example 1 and the final product obtained in Comparative Example 1.

[0028] Figure 4A and Figure 4B They are surface SEM images of the final product obtained in Comparative Example 1 and the target product obtained in Example 1.

[0029] Figure 5A and Figure 5B They are AFM images of the final product obtained in Comparative Example 1 and the target product obtained in Example 1.

[0030] Figure 6 This is a result diagram of the static piezoelectric coefficient d33 of the target product obtained in Example 1 and the PVTF film after polarization treatment obtained in step (2).

[0031] Fig. 7A This is a graph showing the piezoelectric signal output results of the final product obtained in Example 2.

[0032] Figure 7B This is a graph showing the piezoelectric signal output result of the target product obtained in Example 1.

[0033] Figure 8 It is a comparison chart of the tensile strength of the target product obtained in Example 1 and the product obtained in step (2).

[0034] Fig.9A and Fig. 9B The surface potential of the target product obtained in Example 1 and the surface potential of the final product obtained in Comparative Example 1 were measured using a Kelvin probe microscope.

[0035] Fig.10This is a graph showing the adsorption of bovine serum albumin by the target product obtained in Example 1 and the final product obtained in Comparative Example 1.

[0036] Fig.11 It is a graph of cell viability of the target products obtained in Example 1, Example 2 and Example 3 and the final product obtained in Comparative Example 1 measured after 3 days of stem cell inoculation and culture.

[0037] Fig.12 It is a graph showing the activity of alkaline phosphatase (ALP), an indicator of osteogenic differentiation of cells, measured for the target products obtained in Examples 1, 2 and 3 and the final product obtained in Comparative Example 1 after 7 days of stem cell inoculation and culture. DETAILED DESCRIPTION

[0038] In order to better illustrate the present invention and facilitate understanding of the technical solution of the present invention, the present invention is further described in detail below in conjunction with the accompanying drawings and specific embodiments. It should be understood that the following embodiments are only used to illustrate the present invention and do not represent or limit the scope of protection of the present invention. The scope of protection of the present invention shall be subject to the claims.

[0039] In the following examples and comparative examples, the reagents or instruments used without indicating the manufacturer are all conventional products available on the market. For example, the glass plate is a tempered glass plate, and polyvinylidene fluoride-trifluoroethylene (i.e., vinylidene fluoride-trifluoroethylene copolymer, Poly(vinylidene fluoride-trifluoroethylene), P(VDF-TrFE), abbreviated as PVTF) is produced by Piezotech, France, and the product model is: FC30, wherein the molar ratio of vinylidene fluoride monomer to trifluoroethylene monomer is 7:3.

[0040] Preparation of PVTF film by blade coating: Dissolve polyvinylidene fluoride trifluoroethylene (PVTF) powder in N,N-dimethylformamide (DMF) solvent to form a solution. After mixing evenly, add the solution dropwise onto a clean glass plate. Use a blade coater to disperse and shape the solution into a liquid film of a specific height. The coater height is set to 0.4-1 mm.

[0041] Polarization device: It includes a high-voltage DC power supply, a copper counter electrode (consisting of a copper sheet electrode and a base copper plate electrode) and a dimethyl silicone oil tray. The output end of the high-voltage DC power supply is connected to the copper counter electrode with a wire. The PVTF film to be polarized is placed between the counter electrodes. The electric field between the counter electrodes is regulated by adjusting the output voltage. The entire device is immersed in dimethyl silicone oil to exclude water and air to avoid breakdown. The polarization device can be built by yourself or purchased commercially.

[0042] Contact polarization method: Cover the 0.85cm×0.85cm copper sheet electrode on the 1cm×1cm sample to be polarized, transfer the whole to another base copper plate electrode in the tray, press it with a conductive clip, and immerse the whole device in dimethyl silicone oil. Apply a certain voltage (called polarization voltage) between the copper sheet and the base copper plate, and maintain it for a certain time (called polarization time), take out the sample, and wash it with anhydrous ethanol and deionized water to remove the dimethyl silicone oil on it.

[0043] Preparation of monoethanolamine solution: Mix 47.9 mL of monoethanolamine and 2.1 mL of deionized water, stir evenly, and obtain a monoethanolamine aqueous solution with a concentration of 16 mol / L.

[0044] Piezoelectric effect test: Use conductive carbon glue or silver paste, spray gold to prepare counter electrodes on both sides of the film to be tested, connect them with copper wires, and package the whole with PET sheets to obtain a packaged film to be tested. Use a power generator and an exciter to generate a stable and regular mechanical stimulus (bend a 2cm×1cm rectangular sample 45 degrees along the long axis in the middle), place the packaged film to be tested under the stimulus, and connect the oscilloscope to test the piezoelectric signal generated on the surface of the film to be tested through copper wires.

[0045] Protein adsorption test: Use PBS buffer as solvent to prepare a bovine serum albumin (BSA) solution with a concentration of 10 mg / mL. Place the clean sample to be tested in each well of a 24-well plate, add an equal amount of 1 mL of the above-prepared BSA protein solution to each well, and place it in a 4°C refrigerator for 24 hours (for protein adsorption). Then take out the sample to be tested, wash it with PBS first (to remove the weakly adsorbed and residual protein solution), and then elute the protein adsorbed on the surface of the sample to be tested with a 1 mg / mL sodium dodecyl sulfate aqueous solution, and use a special BCA kit (Thermo Scientific) to test the protein concentration in the eluate, so as to calculate the protein adsorption amount of the sample to be tested.

[0046] Cell counting kit-8 was used to determine cell activity: frozen rat bone marrow mesenchymal stem cells (MSCs) were revived and cultured in DMEM low-glucose medium for 3 days, then digested with trypsin, resuspended, and prepared at a concentration of 1.0×10 5Cell suspension of 100 μL / mL was inoculated on the sample surface of 1 cm × 1 cm in each well of a 24-well plate. 0.5 ml of cell suspension was added to each well, and then placed in a constant temperature and humidity incubator at 37 ° C and a carbon dioxide concentration of 5%. Fresh DMEM low-glucose medium was replaced every other day. After 3 days of culture, the sample was transferred to a new 24-well plate. Under light-proof conditions, 500 μL of DMEM low-glucose medium and 50 μL of CCK-8 were added to each well, and incubated at 37 ° C for 2 hours. Finally, the absorbance (OD value) at 450 nm was measured using an ELISA reader.

[0047] Alkaline phosphatase (ALP) test for osteogenic differentiation: Cryopreserved rat bone marrow mesenchymal stem cells (MSCs) were revived and cultured in DMEM low-glucose medium for 3 days, then digested with trypsin, resuspended, and prepared at a concentration of 1.0×10 5 / mL cell suspension, add 0.5ml cell suspension to each well, inoculate on the sample surface of 1cm×1cm in each well of the 24-well plate, and then place in a constant temperature and humidity incubator at 37°C and 5% carbon dioxide concentration, and replace with fresh DMEM low-glucose medium every other day. After 7 days of culture, transfer the sample to a new 24-well plate, wash it with PBS, add cell lysis solution to each well, and then place the 24-well plate in an ice box for reaction for 30 minutes, then draw out the lysed liquid from each well and place it in a centrifuge tube, centrifuge at 12000g at 4°C for 15 minutes, take each supernatant and use the ALP kit to detect the ALP activity in each supernatant.

[0048] Example 1

[0049] (1) 1 g of PVTF powder was added to 5.5 mL of N,N-dimethylformamide (DMF) and magnetically stirred for 3 h to obtain a PVTF solution; the PVTF solution was dispersed and shaped into a liquid film of a specific height on a glass plate using a doctor blade applicator, and the applicator height was set to 0.6 mm; then, the glass plate was placed in a muffle furnace for heat treatment at 210 ° C for 1 h to obtain a PVTF film, and the thickness of the PVTF film was measured to be 50 μm;

[0050] (2) The PVTF film obtained in step (1) was polarized by contact polarization method. The electric field intensity of the contact polarization treatment was 40 kV / mm and the polarization treatment time was 3 min. The piezoelectric coefficient d of the PVTF film after polarization treatment was measured. 33 10pC / N;

[0051] (3) Place 30 mL of a 16 mol / L monoethanolamine (MEA) aqueous solution in a 100 mL beaker, and then immerse the polarized PVTF membrane obtained in step (2) in the monoethanolamine aqueous solution (the membrane is completely immersed in the solution). Then place the beaker in a water bath, heat the water bath to 60°C, and react for 4 hours under continuous stirring. Finally, wash with deionized water to remove the residual monoethanolamine solution on the membrane surface, and dry at 37°C to obtain the target product.

[0052] Comparative Example 1

[0053] (1) 1 g of PVTF powder was added to 5.5 mL of N,N-dimethylformamide (DMF) and magnetically stirred for 3 h to obtain a PVTF solution; the PVTF solution was dispersed and shaped into a liquid film of a specific height on a glass plate using a doctor blade applicator, and the applicator height was set to 0.6 mm; then, the glass plate was placed in a muffle furnace for heat treatment at 210 ° C for 1 h to obtain a PVTF film, and the thickness of the PVTF film was measured to be 50 μm;

[0054] (2) The PVTF film obtained in step (1) was polarized by contact polarization method. The electric field intensity of the contact polarization treatment was 40 kV / mm and the polarization treatment time was 3 min. The piezoelectric coefficient d of the PVTF film after polarization treatment was measured. 33 10pC / N;

[0055] (3) The polarized PVTF membrane obtained in step (2) was immersed in deionized water (the membrane was completely immersed in the deionized water), heated to 60°C in a water bath, reacted for 4 hours under continuous stirring, and then taken out and dried at 37°C to obtain the final product.

[0056] Comparative Example 2

[0057] (1) 1 g of PVTF powder was added to 5.5 mL of N,N-dimethylformamide (DMF) and magnetically stirred for 3 h to obtain a PVTF solution; the PVTF solution was dispersed and shaped into a liquid film of a specific height on a glass plate using a scraper coater, and the coater height was set to 0.6 mm; then, the glass plate was placed in a muffle furnace and heat treated at 210 ° C for 1 h to obtain a final product, which was a PVTF film. The thickness of the PVTF film was measured to be 50 μm.

[0058] Performance and testing:

[0059] The target product obtained in Example 1 and the final product obtained in Comparative Example 1 were subjected to Fourier transform infrared spectroscopy comparative analysis. The results are as follows: Figure 1 shown. Figure 1 Medium, 843cm -1 The absorption peak at corresponds to CH 2 Swing and CF 2Mixed mode of asymmetric stretching vibration, 1286 cm -1 The absorption peak at corresponds to CF 2 The stretching vibration mode of CC and these characteristic peaks are the infrared spectrum characteristic peaks of PVTF; 1559cm -1 The absorption peak at corresponds to NH 2 Bending vibration mode of NH in 1639cm -1 The absorption peak at 3278 cm corresponds to the stretching vibration mode of the C=C bond. -1 The absorption peak at corresponds to the stretching vibration mode of NH and OH. The target product obtained in Example 1 is marked as "PVTF-MEA-4h", and the final product obtained in Comparative Example 1 is marked as "PVTF-H2O-4h". Figure 1 It can be seen that the final product obtained in Comparative Example 1 is PVTF, while the target product obtained in Example 1 contains amino groups in addition to PVTF, indicating that the polarized PVTF in Example 1 has successfully reacted in the MEA solution, thereby successfully achieving amino modification of the material.

[0060] The elemental composition of the target product obtained in Example 1 and the final product obtained in Comparative Example 1 was determined by XPS. Figure 2 shown. Figure 2 In the embodiment 1, the target product obtained is marked as "PVTF-MEA-4h", and the final product obtained in the comparative example 1 is marked as "PVTF-H2O-4h". Figure 2 It can be seen that the spectra of the target product obtained in Example 1 and the final product obtained in Comparative Example 1 both have obvious F1s absorption peaks, O1s absorption peaks and C1s absorption peaks. The difference is that, in addition to these, the target product obtained in Example 1 also has an obvious N1s absorption peak in the spectrum, and its N element content is 6.3%; while there is no N1s peak in the spectrum of the final product obtained in Comparative Example 1, and its N element content is only 1.1% (this may be derived from the adsorption of nitrogen in the air). This shows that there is N element on the surface of the target product obtained in Example 1, while there is no N element on the surface of the final product obtained in Comparative Example 1. Combined with the above FT-IR spectrum, it can be inferred that after the polarized PVTF in Example 1 is treated with MEA, the amino group is successfully modified to the surface of the material.

[0061] The contact angles of the target product obtained in Example 1 and the final product obtained in Comparative Example 1 were tested, and the contact angles were 65° and 101.4°, respectively. Figure 3 As shown, it can be seen that the surface water contact angle of the PVTF subjected to polarization treatment in Example 1 is significantly reduced after being treated with MEA, which means that the surface hydrophobic properties of the material of the target product obtained in Example 1 have changed.

[0062] The surface morphologies of the final product obtained in Comparative Example 1 (labeled as "PVTF-H2O-4h") and the target product obtained in Example 1 (labeled as "PVTF-MEA-4h") were observed by SEM, as shown in FIG. Figure 4A and Figure 4B shown. Figure 4A and Figure 4B The typical wrinkle morphology after PVTF crystallization is shown. This result shows that the MEA treatment in Example 1 did not damage or affect the structure.

[0063] The roughness of the final product obtained in Comparative Example 1 (labeled as "PVTF-H2O-4h") and the target product obtained in Example 1 (labeled as "PVTF-MEA-4h") were characterized by atomic force microscopy, as shown in FIG. Figure 5A and Figure 5B The surface roughness of the final product obtained in Comparative Example 1 is Ra=381nm, and the surface roughness of the target product obtained in Example 1 is Ra=394nm, which are almost equal. This result shows that the MEA treatment in Example 1 does not change the morphology of the material surface.

[0064] Using the static piezoelectric coefficient d 33 The measuring instrument analyzes and compares the target product obtained in Example 1 and the polarized PVTF film obtained in step (2). 33 The numerical measurement results are as follows Figure 6 shown. Figure 6 In the embodiment, the product obtained in step (2) is marked as "before treatment", and the target product obtained in Example 1 is marked as "after treatment". Figure 6 It can be seen that compared with the product obtained in step (2), the target product obtained in Example 1 has a d 33 The values ​​did not change significantly, and there was no significant difference between the two. This result shows that the MEA treatment in Example 1 did not affect the static piezoelectric coefficient d of PVTF. 33 That is, the piezoelectric properties of polyvinylidene fluoride trifluoroethylene did not change significantly after surface amino modification, and the excellent piezoelectric properties were basically retained.

[0065] The piezoelectric effect test was performed on the final product obtained in Comparative Example 2 and the target product obtained in Example 1 under the same deformation conditions using an oscilloscope. The results are as follows: Fig. 7A and Figure 7B shown. Fig. 7A and Figure 7BIn the figure, Comparative Example 2 is marked as "unpolarized PVTF" and the target product obtained in Example 1 is marked as "PVTF-MEA-4h". It can be seen that the output voltage of Comparative Example 2 is always 0V under mechanical deformation, indicating that the PVTF without polarization treatment does not have piezoelectric effect; while the target product obtained in Example 1 has an output voltage under mechanical deformation and shows the same periodic change as mechanical stimulation, indicating that the target product obtained in Example 1 has piezoelectric potential output performance and has piezoelectric effect.

[0066] The tensile strength of the target product obtained in Example 1 was analyzed using a universal material testing machine. The tensile strength results are as follows: Figure 8 For comparison, the tensile strength of the polarized PVTF film obtained in step (2) was also tested. Figure 8 In the embodiment, the product obtained in step (2) is marked as "before treatment", and the target product obtained in Example 1 is marked as "after treatment". Figure 8 It can be seen that the tensile strength of the sample before the treatment in step (2) is 23.3 MPa, and the tensile strength of the sample after the treatment in Example 1 is 20.6 MPa. This result shows that the surface amino modification in Example 1 only slightly reduces the tensile strength, and the target product obtained in Example 1 still has a relatively high strength. That is, the mechanical properties of polyvinylidene fluoride trifluoroethylene do not change significantly after the surface amino modification, and the excellent mechanical properties are basically retained.

[0067] The surface potential of the target product obtained in Example 1 and the surface potential of the final product obtained in Comparative Example 1 were characterized by Kelvin probe microscopy. Fig.9A and Fig. 9B From Fig.9A and Fig. 9B It can be seen that the surface potential of the target product obtained in Example 1 is 0.33 V, while the surface potential of the final product obtained in Comparative Example 1 is -5.57 V. This result shows that the surface potential of the target product obtained by surface amino modification in Example 1 has become positive, compared with the surface potential of the final product obtained in Comparative Example 1, which is obviously negative. Therefore, surface amino modification significantly changes the surface potential of the material.

[0068] The protein adsorption capacity of the target product obtained in Example 1 and the final product obtained in Comparative Example 1 was measured using the BCA kit and the aforementioned protein adsorption capacity test method. The results are as follows: Fig.10 As shown. Fig.10 It can be seen that the protein adsorption amounts of the target product obtained in Example 1 and the final product obtained in Comparative Example 1 are 0.0739 mg / cm 2 and 0.0303mg / cm 2It can be seen that the target product obtained in Example 1 has a higher protein adsorption amount, while the protein adsorption amount of the final product obtained in Comparative Example 1 is significantly less, which means that in the target product obtained in Example 1, the surface modified by amino group is more conducive to protein adsorption and can provide a more suitable protein microenvironment for cell growth.

[0069] Rat bone marrow mesenchymal stem cells (rBMSCs) were inoculated onto the target product obtained in Example 1 and the final product obtained in Comparative Example 1, respectively. After culturing for 3 days, the cell activity was determined using the CCK-8 method. The results were as follows: Fig.11 As shown. Fig.11 It can be seen that the target product obtained in Example 1 ( Fig.11 The OD value of cells inoculated on PVTF-MEA-4h) is higher than that of the final product obtained in Comparative Example 1 ( Fig.11 The OD value of the cells inoculated on PVTF-H2O-4h) is higher, and there is a significant difference between the two, indicating that the stem cells adhered to the target product obtained in Example 1 have stronger proliferation ability and cell viability, proving that the surface of the material constructs a microenvironment that is more conducive to cell proliferation.

[0070] Rat bone marrow mesenchymal stem cells (rBMSCs) were inoculated onto the target product obtained in Example 1 and the final product obtained in Comparative Example 1, respectively. After culturing for 7 days, the osteogenic differentiation trend of the cells was determined using an ALP kit. The results are as follows: Fig.12 As shown. Fig.12 As can be seen in Example 1 ( Fig.12 The ALP (cell osteogenic differentiation indicator alkaline phosphatase) activity of cells inoculated on PVTF-MEA-4h) was higher than that of comparative example 1 ( Fig.12 PVTF-H 2 The ALP activity of the cells inoculated on 0-4h) was significantly higher, and there was a significant difference between the two, indicating that the target product obtained in Example 1 can more strongly promote the osteogenic differentiation of stem cells.

[0071] In summary, the target product obtained in the above Example 1 is a piezoelectric polyvinylidene fluoride trifluoroethylene with surface amino modification. The amino modification does not substantially change the surface morphology and roughness of the piezoelectric polyvinylidene fluoride trifluoroethylene. The piezoelectric polyvinylidene fluoride trifluoroethylene with surface amino modification retains the excellent mechanical properties and piezoelectric properties of the piezoelectric polyvinylidene fluoride trifluoroethylene. At the same time, the surface potential changes toward a positive potential, a microenvironment more conducive to cell proliferation is constructed on the surface of the material, and the material can more strongly promote the osteogenic differentiation of stem cells.

[0072] Example 2

[0073] (1) 1 g of PVTF powder was added to 5.5 mL of N,N-dimethylformamide (DMF) and magnetically stirred for 3 h to obtain a PVTF solution; the PVTF solution was dispersed and shaped into a liquid film of a specific height on a glass plate using a doctor blade applicator, and the applicator height was set to 0.6 mm; then, the glass plate was placed in a muffle furnace for heat treatment at 210 ° C for 1 h to obtain a PVTF film, and the thickness of the PVTF film was measured to be 50 μm;

[0074] (2) The PVTF film obtained in step (1) was polarized by contact polarization method. The electric field intensity of the contact polarization treatment was 40 kV / mm and the polarization treatment time was 3 min. The piezoelectric coefficient d of the PVTF film after polarization treatment was measured. 33 10pC / N;

[0075] (3) Place 30 mL of a 16 mol / L monoethanolamine aqueous solution in a 100 mL beaker, and then immerse the polarized PVTF membrane obtained in step (2) in the monoethanolamine aqueous solution (the membrane is completely immersed in the solution). Place the beaker in a water bath, heat the water bath to 60°C, and react for 0.5 h under continuous stirring. Finally, wash with deionized water to remove the residual monoethanolamine solution on the membrane surface, and dry at 37°C to obtain the target product.

[0076] After testing, the target product obtained in Example 2 is piezoelectric polyvinylidene fluoride trifluoroethylene with surface amino groups modified; the surface potential thereof was analyzed using a Kelvin probe microscope, and the surface potential thereof was -1.07V.

[0077] Example 3

[0078] (1) 1 g of PVTF powder was added to 5.5 mL of N,N-dimethylformamide (DMF) and magnetically stirred for 3 h to obtain a PVTF solution; the PVTF solution was dispersed and shaped into a liquid film of a specific height on a glass plate using a doctor blade applicator, and the applicator height was set to 0.6 mm; then, the glass plate was placed in a muffle furnace for heat treatment at 210 ° C for 1 h to obtain a PVTF film, and the thickness of the PVTF film was measured to be 50 μm;

[0079] (2) The PVTF film obtained in step (1) was polarized by contact polarization method. The electric field intensity of the contact polarization treatment was 40 kV / mm and the polarization treatment time was 3 min. The piezoelectric coefficient d of the PVTF film after polarization treatment was measured. 33 10pC / N;

[0080] (3) Place 30 mL of a 16 mol / L monoethanolamine aqueous solution in a 100 mL beaker, and then immerse the polarized PVTF membrane obtained in step (2) in the monoethanolamine aqueous solution (the membrane is completely immersed in the solution). Place the beaker in a water bath, heat the water bath to 60°C, and react for 1 hour under continuous stirring. Finally, wash with deionized water to remove the residual monoethanolamine solution on the membrane surface, and dry at 37°C to obtain the target product.

[0081] After testing, the target product obtained in Example 3 is piezoelectric polyvinylidene fluoride trifluoroethylene modified with surface amino groups. The surface potential thereof was analyzed using a Kelvin probe microscope, and the surface potential thereof was -0.55 V.

[0082] Example 4

[0083] (1) 1 g of PVTF powder was added to 5.5 mL of N,N-dimethylformamide (DMF) and magnetically stirred for 3 h to obtain a PVTF solution; the PVTF solution was dispersed and shaped into a liquid film of a specific height on a glass plate using a doctor blade applicator, and the applicator height was set to 0.6 mm; then, the glass plate was placed in a muffle furnace for heat treatment at 210 ° C for 1 h to obtain a PVTF film, and the thickness of the PVTF film was measured to be 50 μm;

[0084] (2) The PVTF film obtained in step (1) was polarized by contact polarization method. The electric field intensity of the contact polarization treatment was 40 kV / mm and the polarization treatment time was 3 min. The piezoelectric coefficient d of the PVTF film after polarization treatment was measured. 33 10pC / N;

[0085] (3) Place 30 mL of a 16 mol / L monoethanolamine aqueous solution in a 100 mL beaker, and then immerse the polarized PVTF membrane obtained in step (2) in the monoethanolamine aqueous solution (the membrane is completely immersed in the solution). Place the beaker in a water bath, heat the water bath to 60°C, and react for 2 hours under continuous stirring. Finally, wash with deionized water to remove the residual monoethanolamine solution on the membrane surface, and dry at 37°C to obtain the target product.

[0086] After testing, the target product obtained in Example 4 is piezoelectric polyvinylidene fluoride trifluoroethylene modified with surface amino groups. The surface potential thereof was analyzed using a Kelvin probe microscope, and the surface potential thereof was -0.29V.

[0087] Example 5

[0088] (1) 1 g of PVTF powder was added to 5.5 mL of N,N-dimethylformamide (DMF) and magnetically stirred for 3 h to obtain a PVTF solution; the PVTF solution was dispersed and shaped into a liquid film of a specific height on a glass plate using a doctor blade applicator, and the applicator height was set to 0.6 mm; then, the glass plate was placed in a muffle furnace for heat treatment at 210 ° C for 1 h to obtain a PVTF film, and the thickness of the PVTF film was measured to be 50 μm;

[0089] (2) The PVTF film obtained in step (1) was polarized by contact polarization method. The electric field intensity of the contact polarization treatment was 40 kV / mm and the polarization treatment time was 3 min. The piezoelectric coefficient d of the PVTF film after polarization treatment was measured. 33 10pC / N;

[0090] (3) Place 30 mL of a 16 mol / L monoethanolamine aqueous solution in a 100 mL beaker, and then immerse the polarized PVTF membrane obtained in step (2) in the monoethanolamine aqueous solution (the membrane is completely immersed in the solution). Place the beaker in a water bath, heat the water bath to 60°C, and react for 8 hours under continuous stirring. Finally, wash with deionized water to remove the residual monoethanolamine solution on the membrane surface, and dry at 37°C to obtain the target product.

[0091] After testing, the target product obtained in Example 5 is piezoelectric polyvinylidene fluoride trifluoroethylene with surface amino groups modified. The surface potential thereof was analyzed by Kelvin probe microscope, and the surface potential thereof was 0.59V.

[0092] The cell viability of the target products obtained in Example 1, Example 2 and Example 3 (respectively labeled as: PVTF-MEA-4h, PVTF-MEA-0.5h, PVTF-MEA-1h) and the final product obtained in Comparative Example 1 (labeled as: PVTF-H2O-4h) after 3 days of inoculation and culture of stem cells was tested. The results are as follows Fig.11 As mentioned above, with the increase of ethanolamine treatment time, the number of amino groups modified on the PVTF surface gradually increases, and the surface potential of PVTF gradually changes to the positive surface potential direction. Fig.11 It can be seen that after 3 days of culture, stem cells also showed a change pattern that the cell activity continued to increase as the surface potential of the material changed to a positive surface potential. This result shows that the surface potential of PVTF changed after amino modification, which improved the protein adsorption characteristics and was conducive to the adhesion and proliferation of stem cells on PVTF.

[0093] The target products obtained in Example 1, Example 2 and Example 3 (respectively labeled as: PVTF-MEA-4h, PVTF-MEA-0.5h, PVTF-MEA-1h) and the final product obtained in Comparative Example 1 (labeled as: PVTF-H2O-4h) were tested for the activity of alkaline phosphatase (ALP), an indicator of osteogenic differentiation of cells, after 7 days of inoculation and culture of stem cells. The results are as follows Fig.12 As shown. Fig.12 It can be seen that as the surface potential of PVTF gradually changes toward the positive surface potential, the osteogenic differentiation ability of stem cells on the PVTF surface also gradually increases, showing a positive correlation with the surface potential. This result shows that regulating the surface potential of PVTF by amino modification is an effective means to enhance its ability to promote cell osteogenic differentiation and bone repair.

[0094] In combination with Examples 1 to 5, it can be found that: as the reaction time of MEA water bath heating in step (3) increases, the surface potential of the target product obtained in each Example, the amino-modified piezoelectric polyvinylidene fluoride trifluoroethylene, will gradually change from a negative surface potential to a positive surface potential. It can be seen that by adjusting the parameters of water bath heating (such as reaction time, reaction temperature), amino-modified piezoelectric polyvinylidene fluoride trifluoroethylene with different surface potentials can be obtained; in addition, by adjusting the polarization parameters, PVTF with different degrees of electric dipole orientation can be formed. Therefore, the surface potential of the target product obtained by each embodiment of the present invention is controllable, and the reaction parameters can be adjusted according to actual needs to obtain it, so as to provide suitable binding sites for proteins in different media, adsorb proteins of different concentrations and types to the surface of the material, and provide cells with a good microenvironment (microenvironment is a cell niche, which refers to a comprehensive environmental state including cells, ECM, secretory factors and physicochemical conditions in the process of growth and differentiation), which can effectively promote cell adhesion and proliferation; at the same time, the material also has certain piezoelectric properties, and can generate piezoelectric potential under the mechanical deformation caused by daily physiological activities, and apply electrical stimulation to surrounding cells and tissues to promote their osteogenic differentiation and bone regeneration, avoiding the complex operation and infection risk of external power supply and electrodes; in addition, the method forms a covalently bonded surface modification, which has high stability, can play a role for a long time, and also has a certain mechanical strength, which can be used as a barrier membrane to prevent unwanted tissue from growing into the defect site, which is conducive to the repair and regeneration of the defect. At the same time, the method of the present invention is also applicable to PVTF materials with different forms other than membranous materials, as long as the surface exists, it can be immersed in an alkaline solution to react for modification. Therefore, the surface amino-modified piezoelectric polyvinylidene fluoride trifluoroethylene obtained by the present invention can construct a bionic microenvironment rich in proteins and electrical signals at the material-cell interface, and the material can also generate piezoelectric potential under daily mechanical stimulation, realize self-excited electrical signal stimulation, and do not require the dangerous operation of external electrodes and power supplies, realize the construction of bionic microenvironment and controllable electrical signal stimulation to coordinately regulate cell fate, and can be used as a biomedical implant to promote corresponding tissue repair and regeneration, such as for promoting osteogenic differentiation and accelerating bone regeneration. At the same time, the preparation method of the present invention is very simple, does not require special conditions or equipment, and is easy to implement.

[0095] It can be seen that the purpose of the present invention has been completely and effectively achieved. The functional and structural principles of the present invention have been demonstrated and explained in the embodiments. Without departing from the principles, the implementation methods can be modified arbitrarily. Therefore, the present invention includes all modified implementation methods based on the spirit and scope of the claims.

Claims

1. A piezoelectric polyvinylidene fluoride trifluoroethylene with amino groups modified on the surface, It is characterized in that The invention is composed of polarized PVTF and amino functional groups grafted on the surface of the PVTF.

2. The surface amino-modified piezoelectric polyvinylidene fluoride trifluoroethylene according to claim 1, It is characterized in that The piezoelectric coefficient d of the polarized PVTF 33 Satisfy: -25pC / N≤d 33 <0pC / N or 0pC / N<d 33 ≤25pC / N.

3. The surface amino-modified piezoelectric polyvinylidene fluoride trifluoroethylene according to claim 1, It is characterized in that The piezoelectric coefficient d of the polarized PVTF 33 Satisfy: -15pC / N≤d 33 ≤-5pC / N or 5pC / N≤d 33 ≤15pC / N.

4. The method for preparing the surface amino-modified piezoelectric polyvinylidene fluoride trifluoroethylene according to any one of claims 1 to 3, The following steps are involved: (1) adding PVTF powder to N,N-dimethylformamide solvent at a solid-liquid ratio of 1 g: (4-10) mL, stirring for 2-4 hours to obtain a PVTF solution; forming a film of the PVTF solution on a substrate, and then heat treating at 180° C. to 240° C. for 0.5 hours to 2 hours to obtain a PVTF film, wherein the thickness of the PVTF film is 30-80 μm; (2) performing polarization treatment on the PVTF film obtained in step (1) to obtain a polarized PVTF film; (3) placing the polarized PVTF membrane obtained in step (2) in an aqueous solution of an organic amino base, heating it in a water bath to 30° C. to 70° C., reacting it for 0.5 h to 12 h, then washing it with deionized water and drying it to obtain the target product.

5. The method for preparing the surface amino-modified piezoelectric polyvinylidene fluoride trifluoroethylene according to claim 4, It is characterized in that In step (2), the polarization treatment is a contact polarization treatment.

6. The method for preparing the surface amino-modified piezoelectric polyvinylidene fluoride trifluoroethylene according to claim 5, It is characterized in that In step (2), the high voltage electric field intensity of the contact polarization treatment is 30 to 90 kV / mm, and the polarization treatment time is 3 to 10 min.

7. The method for preparing the surface amino-modified piezoelectric polyvinylidene fluoride trifluoroethylene according to claim 4, It is characterized in that In step (2), the piezoelectric coefficient d of the PVTF film obtained by polarization treatment is 33 Satisfy: -25pC / N≤d 33 <0pC / N or 0pC / N<d 33 ≤25pC / N.

8. The method for preparing the surface amino-modified piezoelectric polyvinylidene fluoride trifluoroethylene according to claim 4, It is characterized in that In step (3), the organic amino-containing base is monoethanolamine, ethylenediamine, isopropanolamine or isobutanolamine.

9. Use of the surface amino-modified piezoelectric polyvinylidene fluoride trifluoroethylene according to any one of claims 1 to 3 in the preparation of biomedical implants.

10. The use according to claim 9, It is characterized in that Use of the surface amino-modified piezoelectric polyvinylidene fluoride trifluoroethylene according to any one of claims 1 to 3 in the preparation of bone defect repair materials.

Citation Information

Patent Citations

  • Preparation of ultra-hydrophobic polyvinylidene fluoride membrane and product thereof

    CN101463140A

  • Method for modifying interpenetrating polymer network on surface of polyvinylidene fluoride porous membrane

    CN101485960A

  • Method for preparing pollution preventing self-cleaning polyvinylidene fluoride (PVDF) film and product thereof

    CN101649065A

  • Polarization process for polyvinylidene fluoride film

    CN104425704A

  • Preparation method of flexible piezoelectric film

    CN114122252A

Cited By

  • Anodized aluminum oxide / polyvinylidene fluoride trifluoroethylene film and preparation thereof

    CN119607264A