Perfluoropolymer porous sponge and preparation method thereof
By using water-soluble polymer as auxiliary molding carrier, combined with low-temperature freezing and high-temperature sintering processes, the molding and bonding problems in the preparation of perfluoropolymer porous sponges are solved, and the efficient and green preparation of perfluoropolymer porous sponges is achieved. Excellent pore structure and performance have broadened the application field.
Patent Information
- Application Number
- CN202411116229.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-14
- Publication Date
- 2024-11-26
AI Technical Summary
In the preparation process of perfluoropolymer porous sponges, the existing technology faces challenges such as suspension component selection, sol-gel structure stability, pore structure regulation and self-support molding, which leads to the inability to form a continuous three-dimensional network structure of PTFE resin, which limits the possibility of PTFE resin to form a continuous three-dimensional network structure. Its performance improvements.
Water-soluble polymer is used as the auxiliary molding carrier, and the pore structure molding is controlled through low-temperature freeze-drying and high-temperature sintering processes to form a stable perfluoropolymer porous sponge to ensure that the resin bonds to form a three-dimensional network structure.
The prepared perfluoropolymer porous sponge has a controllable pore structure, low density, superhydrophobicity, self-supporting and wide application prospects. It has a green process and no pollution, achieving better performance and broader application fields. .
Smart Images

Figure CN119019746A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of porous materials, and in particular relates to a perfluoropolymer porous sponge and a preparation method thereof. Background Art
[0002] Perfluoropolymers have good chemical stability, thermal stability, durability and excellent hydrophobic properties due to their all-CF structure. Among them, polytetrafluoroethylene (PTFE) stands out among perfluoropolymers due to its unique molecular structure. In the molecular structure of PTFE, each carbon atom is connected to two fluorine atoms, forming a symmetrical and dense protective layer composed of fluorine atoms. This spatial configuration of CF bonds promotes a special crystalline structure, which in turn enables PTFE to exhibit enhanced heat resistance, hydrophobicity, chemical inertness, high mechanical toughness and good biocompatibility. Therefore, PTFE is widely used in many fields such as membrane separation, biomedicine, aerospace, fuel cells, etc.
[0003] Porous sponge is a three-dimensional porous material with low density, high porosity, large specific surface area and low thermal conductivity. It has shown wide application potential in thermal insulation, electromagnetic shielding / absorption, water treatment, solar-driven interfacial evaporation, energy storage and conversion, adsorption, catalyst support and biomedicine. Ice template method is a common method for preparing three-dimensional porous materials. The pore structure of porous sponge is controlled by regulating the growth of ice crystals in the suspension. However, there are many challenges in the preparation of porous sponge from perfluoropolymer emulsion, including the selection of suspension components, the stable formation of sol-gel structure, the appropriate drying method, the regulation and optimization of pore structure, the formation of primary self-supporting perfluoropolymer porous sponge, and the determination of post-processing process. Nevertheless, perfluoropolymer porous sponge has the potential to combine its inherent properties with the unique three-dimensional porous structure of porous sponge to create a new structure with unprecedented unique properties, and show better performance and broader application prospects.
[0004] According to literature reports, Yury M. Shulga et al. (DOI: 10.1021 / acs.energyfuels.0c01094, 10.1021 / acs.langmuir.8b04028) from the Institute of Chemical Physics of the Russian Academy of Sciences used graphene oxide (GO) as a connector to prevent the aggregation of PTFE emulsion during gelation and successfully prepared PTFE-based porous sponges with densities of 0.026 to 0.035 g / cm 3Zheng Wenjiang et al. (DOI: 10.1007 / s10971-023-06261-0) from Sichuan University of Science and Engineering added PTFE emulsion to the preparation of silica (SiO2) aerogel to prevent precipitation during the gelation process. After drying under ambient pressure, hydrophobic and corrosion-resistant SiO2 / PTFE aerogel was obtained with a density of 0.0874-0.1632 g / cm 3 However, the poor compatibility of GO and SiO2 with PTFE results in the inability of PTFE resin to bond to form a continuous three-dimensional network structure, limiting the further improvement of its performance. Summary of the invention
[0005] In view of the shortcomings of the prior art, one object of the present invention is to provide a method for preparing a perfluoropolymer porous sponge; another object of the present invention is to provide a perfluoropolymer porous sponge prepared by the above method.
[0006] To this end, the present invention adopts the following technical solutions:
[0007] A method for preparing a perfluoropolymer porous sponge comprises the following steps:
[0008] S1, preparation of a suspension: uniformly mixing an aqueous solution of a water-soluble polymer and an aqueous perfluoropolymer emulsion to obtain a suspension, wherein the mass ratio of the perfluoropolymer to the water-soluble polymer is (1-20):1;
[0009] S2, preparation of a primary perfluoropolymer-based porous sponge: freezing the suspension at -195 to -10°C for 10 min to 24 h to obtain a uniformly dispersed perfluoropolymer-based sol-gel, and freeze-drying to obtain a primary perfluoropolymer-based porous sponge;
[0010] S3, post-treatment of the perfluoropolymer porous sponge: sintering the primary perfluoropolymer porous sponge obtained in S2 to oxidatively decompose the water-soluble polymer to obtain a perfluoropolymer porous sponge.
[0011] In step S1, the functional nanoparticles can be uniformly dispersed in the aqueous solution of the water-soluble polymer first, and then mixed with the perfluoropolymer water-based emulsion. The functional nanoparticles are one of titanium dioxide (TiO2), ferrous oxide (Fe3O4), zinc oxide (ZnO), aluminum oxide (Al2O3), cerium oxide (CeO2), MXene, carbon nanotubes (CNTs) and graphene (Gra). The solid content ratio of the functional nanoparticles to the perfluoropolymer is (0.001-1):10.
[0012] Preferably, the water-soluble polymer in step S1 is one of polyvinyl alcohol (PVA), polyethylene oxide (PEO), polyethylene glycol (PEG), polyvinyl pyrrolidone (PVP) and sodium alginate (SA); and the mass fraction of the water-soluble polymer in the aqueous solution of the water-soluble polymer is 0.1 to 2 wt%.
[0013] Preferably, the perfluoropolymer water-based emulsion in S1 is one of PTFE water-based emulsion, FEP (polyperfluoroethylene propylene) water-based emulsion and PFA (polyperfluoroalkoxy vinyl ether) water-based emulsion; and the solid content of the perfluoropolymer water-based emulsion is 40-60wt%.
[0014] Preferably, the preparation method of the suspension in S1 is: at room temperature, after blending the perfluoropolymer water-based emulsion and the water-soluble polymer aqueous solution, magnetically stirring at a speed of 200 to 400 r / min for 1 to 6 hours, and standing to degas.
[0015] Preferably, the freeze drying in S2 is carried out at a temperature of -10 to -40°C for 9 to 36 hours; and the sintering in S3 is carried out at a temperature of 250 to 400°C for 10 to 60 minutes.
[0016] The present invention also provides a perfluoropolymer porous sponge prepared by the above preparation method, with a density of 0.0430-0.1503 g / cm 3 The porosity is 71.64-98.05%, and the water contact angle is greater than 150°.
[0017] The present invention mixes a perfluoropolymer emulsion and a water-soluble polymer solution, wherein the water-soluble polymer is used as an auxiliary molding carrier, and controls the pore structure molding by low-temperature freezing. After freeze-drying, a self-supporting perfluoropolymer primary porous sponge is obtained, and then the water-soluble polymer is directly sintered at high temperature to obtain a perfluoropolymer porous sponge, which can be used in the fields of oil-water separation, seawater desalination, solar interface evaporation, adsorption, catalyst carrier, etc.
[0018] Compared with the prior art, the present invention has the following beneficial effects:
[0019] 1. The present invention selects high-viscosity and high-temperature-decomposable water-soluble polymers such as polyethylene oxide (PEO), polyvinyl alcohol (PVA), polyethylene glycol (PEG), polyvinyl pyrrolidone (PVP), sodium alginate (SA), etc. as auxiliary molding carriers, which not only ensures the uniform dispersion of the perfluoropolymer emulsion and prevents the precipitation of the perfluoropolymer during the freeze casting process, but also ensures that a precursor perfluoropolymer-based porous sponge with stable self-supporting properties can be formed after freeze drying. Finally, the water-soluble polymer is removed through a high-temperature sintering process, so that the perfluoropolymer resin is bonded to form a stable three-dimensional porous sponge structure.
[0020] 2. The perfluoropolymer porous sponge prepared by the present invention has controllable pore structure, uniform pore size, softness, low density, large specific surface area, super hydrophobicity, good self-supporting property, high porosity and wide application range. At the same time, due to its unique perfluoro structure, the porous sponge has good thermal stability and chemical stability, showing unprecedented unique performance.
[0021] 3. The present invention uses a water-soluble polymer solution as an auxiliary molding carrier, and removes the auxiliary molding carrier during the post-processing sintering process to obtain a flexible perfluoropolymer porous sponge. The preparation process does not involve organic solvents, is green and pollution-free, and has low requirements on equipment, and can achieve continuous production.
[0022] 4. The present invention uses an ice template method to prepare a perfluoropolymer porous sponge, which is simple, efficient, and controllable. The obtained perfluoropolymer porous sponge has a three-dimensional porous structure.
[0023] 5. The present invention promotes the self-assembly behavior of the polymer by controlling the formation mode of the ice template (freezing mode and freezing process) during the freezing process, thereby achieving the regulation of the microstructure of the perfluoropolymer porous sponge.
[0024] 6. The present invention can effectively regulate the pore morphology, pore size and density of the perfluoropolymer porous sponge through a sintering process.
[0025] 7. The present invention can add functional nanoparticles to the perfluoropolymer suspension to give the perfluoropolymer porous sponge corresponding functions, thereby broadening the application field of the perfluoropolymer porous sponge.
[0026] 8. The perfluoropolymer porous sponge prepared by the present invention does not require additional super-hydrophobic treatment agent during use and has super-hydrophobic self-cleaning properties. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] Figure 1 This is a surface microstructure diagram of the PTFE porous sponge prepared in Example 1 of the present invention;
[0028] Figure 2 This is a surface microstructure diagram of the self-supporting primary PTFE-based porous sponge prepared in Example 3 of the present invention;
[0029] Figure 3 This is a state diagram of the PTFE porous sponge prepared in Example 3 of the present invention placed on a dandelion;
[0030] Figure 4 This is a surface microstructure diagram of the FEP porous sponge prepared in Example 6 of the present invention;
[0031] Figure 5This is a physical picture of the PTFE / MXene porous sponge prepared in Example 8 of the present invention;
[0032] Figure 6 This is a thermal infrared image of the PTFE / MXene porous sponge prepared in Example 8 of the present invention;
[0033] Figure 7 This is a surface microstructure diagram of the PTFE porous sponge prepared in Example 9 of the present invention;
[0034] Figure 8 This is a thermal infrared image of the PTFE porous sponge prepared in Example 9 of the present invention on a heating platform;
[0035] Fig. 9 A cross-sectional view of a PTFE porous sponge prepared in Example 10 of the present invention;
[0036] Fig.10 This is the water contact angle of the Al2O3 / PTFE porous sponge prepared in Example 11 of the present invention. DETAILED DESCRIPTION
[0037] The preparation method of the present invention is described in detail below with reference to the accompanying drawings and examples.
[0038] Example 1
[0039] A method for preparing a perfluoropolymer porous sponge comprises the following steps:
[0040] S1, preparation of suspension: a PEO aqueous solution with a mass fraction of 1 wt% and a PTFE water-based emulsion with a solid content of 40 wt% are magnetically stirred at room temperature for 1 h at a speed of 400 r / min, wherein the solid content ratio of PTFE to PEO is 3:1, and after standing and degassing, a suspension is obtained;
[0041] S2, preparation of primary PTFE-based porous sponge: using ice template method to control ice crystal growth to obtain primary PTFE-based porous sponge (same as the following examples).
[0042] The suspension prepared in S1 was poured into a container and placed in a -80°C low-temperature refrigerator for 1 hour to obtain a uniformly dispersed PTFE sol-gel; and then freeze-dried at -40°C for 9 hours to obtain a self-supporting primary PTFE-based porous sponge;
[0043] S3, post-treatment of primary PTFE-based porous sponge: the self-supporting primary PTFE-based porous sponge obtained in S2 is sintered at a sintering temperature of 350°C and a sintering time of 30 minutes. In a high-temperature air atmosphere, the water-soluble polymer PEO is oxidatively decomposed and the PTFE resin is bonded to finally obtain a porous sponge containing only PTFE.
[0044] Depend on Figure 1 It can be seen that the PTFE porous sponge prepared in this embodiment has a three-dimensional porous structure. After testing, the density of the PTFE porous sponge is 0.0466 g / cm 3 , the porosity is 97.12%.
[0045] Example 2
[0046] A method for preparing a perfluoropolymer porous sponge comprises the following steps:
[0047] S1, preparation of suspension: magnetically stirring a PVA aqueous solution with a mass fraction of 0.5wt% and a PTFE water-based emulsion with a solid content of 50wt% at room temperature for 2h at a speed of 300r / min, wherein the solid content ratio of PTFE to PVA is 5:1, and standing for degassing to obtain a suspension;
[0048] S2, preparation of primary PTFE-based porous sponge: pour the suspension into a container, freeze it in a -40°C low-temperature refrigerator for 5 h to obtain a uniformly dispersed PTFE sol-gel, and freeze-dry it at -30°C for 12 h to obtain a self-supporting primary PTFE-based porous sponge;
[0049] S3, post-treatment of primary PTFE-based porous sponge: The self-supporting primary PTFE-based porous sponge obtained in S2 is sintered at a temperature of 350° C. and a sintering time of 60 min. In a high-temperature air atmosphere, the water-soluble polymer PVA is oxidized and decomposed, and the PTFE resin is bonded to obtain a porous sponge containing only PTFE.
[0050] After testing, the density of PTFE porous sponge is 0.0471g / cm 3 , the porosity is 97.86%.
[0051] Example 3
[0052] A method for preparing a perfluoropolymer porous sponge comprises the following steps:
[0053] S1, preparation of suspension: magnetically stirring a PEO aqueous solution with a mass fraction of 0.3 wt% and a PTFE water-based emulsion with a solid content of 60 wt% at room temperature for 3 h at a rotation speed of 200 r / min, wherein the solid content ratio of PTFE to PEO is 8:1, and standing for degassing to obtain a suspension;
[0054] S2, preparation of primary PTFE-based porous sponge: pour the suspension into a container, freeze it in a -20°C low-temperature refrigerator for 15 hours to obtain a uniformly dispersed PTFE sol-gel, and then freeze-dry it at -10°C for 36 hours to obtain a self-supporting primary PTFE-based porous sponge, the surface microstructure of which is as follows Figure 2As shown, it can be seen that the self-supporting primary PTFE-based porous sponge has continuity and self-support, the pore morphology is regular, and it has a three-dimensional through-pore structure;
[0055] S3, post-treatment of the primary PTFE-based porous sponge: The self-supporting primary PTFE-based porous sponge obtained in S2 is sintered at a temperature of 350° C. and a sintering time of 30 min. During this process, the water-soluble polymer PEO is oxidized and decomposed, and the PTFE resin is bonded, and finally a porous sponge containing only PTFE is obtained.
[0056] Figure 3 The porous PTFE sponge prepared in this embodiment is placed on a dandelion. It can be seen from the figure that the prepared PTFE porous sponge is light in weight. After testing, its density is 0.0541 g / cm 3 , the porosity is 97.90%.
[0057] Example 4
[0058] This embodiment is basically the same as embodiment 3, except that in S3, the sintering temperature is 360°C.
[0059] Example 5
[0060] This embodiment is basically the same as embodiment 3, except that in S3, the sintering temperature is 380°C.
[0061] The sintering temperature, holding time and density of the prepared PTFE porous sponge of Examples 3-5 are shown in Table 1.
[0062] Table 1
[0063] serial number Sintering temperature(℃) Insulation time (min) <![CDATA[Density (mg / cm 3 )]]> Example 3 350 30 0.0541 Example 4 360 30 0.0562 Example 5 380 30 0.0584
[0064] It can be seen from Table 1 that as the sintering temperature increases, the density of the PTFE porous sponge prepared by the present invention also increases. Therefore, PTFE porous sponges with different densities can be obtained by adjusting the sintering temperature.
[0065] Example 6
[0066] A method for preparing a perfluoropolymer porous sponge comprises the following steps:
[0067] S1, preparation of suspension: a PEO aqueous solution with a mass fraction of 0.5wt% and a FEP water-based emulsion with a solid content of 60wt% were magnetically stirred at room temperature for 3h at a speed of 250r / min, wherein the solid content ratio of FEP to PEO was 8:1, and after standing and degassing, a suspension was obtained;
[0068] S2, preparation of nascent FEP-based porous sponge: pour the suspension into a container, freeze it in a -60°C low-temperature refrigerator for 15 hours to obtain a uniformly dispersed FEP sol-gel, and freeze-dry it at -40°C for 10 hours to obtain a self-supporting nascent FEP-based porous sponge;
[0069] S3, post-treatment of primary FEP-based porous sponge: The self-supporting primary PTFE-based porous sponge obtained in S2 was sintered at a temperature of 250°C and a sintering time of 10 min. The water-soluble polymer PEO was oxidized and decomposed to obtain a porous sponge containing only FEP, and its surface microstructure is as follows: Figure 4 shown.
[0070] As can be seen from the figure, the prepared FEP porous sponge has a three-dimensional porous structure. After testing, the density of the FEP porous sponge is 0.0656 g / cm 3 , porosity is 97.47%
[0071] Example 7
[0072] A method for preparing a perfluoropolymer porous sponge comprises the following steps:
[0073] S1, preparation of suspension: magnetically stirring a PEO aqueous solution with a mass fraction of 0.5 wt% and a PFA water-based emulsion with a solid content of 50 wt% at room temperature for 3 h at a speed of 200 r / min, wherein the solid content ratio of PFA to PEO is 10:1, and standing to degas, to obtain a suspension;
[0074] S2, preparation of nascent PFA-based porous sponge: pour the suspension into a container, freeze it in a low temperature environment of -80°C for 15 hours to obtain a uniformly dispersed PFA sol-gel, and freeze-dry it at -40°C for 10 hours to obtain a self-supporting nascent PFA-based porous sponge;
[0075] S3, post-treatment of the primary PFA-based porous sponge: the self-supporting primary PFA-based porous sponge obtained in S2 is sintered at a sintering temperature of 300° C. and a sintering time of 10 min. The water-soluble polymer PEO is oxidatively decomposed to obtain a porous sponge containing only PFA.
[0076] After testing, the density of PFA porous sponge is 0.0807g / cm 3 , porosity is 96.66%
[0077] Example 8
[0078] A method for preparing a perfluoropolymer porous sponge comprises the following steps:
[0079] S1, preparation of suspension: ultrasonically disperse the MXene dispersion in a PEO aqueous solution with a mass fraction of 0.5wt% for 30min, then add a PTFE water-based emulsion with a solid content of 50wt%, and magnetically stir at room temperature for 3h at a speed of 200r / min, wherein the solid content ratio of PTFE, PEO and MXene is 5:1:0.02, and after standing and degassing, a suspension is obtained;
[0080] S2, preparation of a nascent loaded functional PTFE-based porous sponge: pouring the suspension into a container, freezing it in a low temperature environment of -80°C for 15 hours to obtain a uniformly dispersed PTFE sol-gel, and freeze-drying it at -40°C for 10 hours to obtain a self-supporting nascent loaded functional PTFE-based porous sponge;
[0081] S3, post-treatment of the primary loaded functional PTFE-based porous sponge: The self-supporting primary loaded functional PTFE-based porous sponge obtained in S2 was sintered at a sintering temperature of 340°C and a sintering time of 10 min. PEO was oxidatively decomposed to obtain a PTFE / MXene three-dimensional porous sponge with photothermal conversion performance. The physical picture is shown in FIG. Figure 5 As shown in the figure, the surface thermal infrared imaging under simulated sunlight is as follows Figure 6 shown.
[0082] Depend on Figure 5 It can be seen that the PTFE / MXene porous sponge prepared in this example is black. Figure 6 It can be seen that the surface temperature of the PTFE / MXene porous sponge reaches a high temperature of 81.7°C under simulated sunlight (the temperature scale on the right represents the temperature range in the picture), and it has photothermal conversion performance; in addition, the three-dimensional porous structure can promote water transfer and can be applied to solar interface evaporation desalination of seawater.
[0083] Example 9
[0084] A method for preparing a perfluoropolymer porous sponge comprises the following steps:
[0085] S1, preparation of suspension: a SA aqueous solution with a mass fraction of 0.1wt% and a PTFE water-based emulsion with a solid content of 50wt% were magnetically stirred at room temperature for 3h at a speed of 300r / min, wherein the solid content ratio of PTFE to SA was 20:1, and after standing and degassing, a suspension was obtained;
[0086] S2, preparation of primary PTFE-based porous sponge: pour the suspension into a container, place it in liquid nitrogen (-195° C.) for two-way freezing for 2 h to obtain a uniformly dispersed PTFE sol-gel; then freeze-dry it at -40° C. for 12 h to obtain a self-supporting primary PTFE-based porous sponge;
[0087] S3, post-treatment of primary PTFE-based porous sponge: The self-supporting primary PTFE-based porous sponge obtained in S2 is sintered at a sintering temperature of 380°C and a sintering time of 60 min. SA is oxidatively decomposed to obtain a PTFE porous sponge, whose surface microstructure is as follows: Figure 7 As shown in the figure, the thermal infrared imaging of the PTFE porous sponge surface after 20 minutes on a 100℃ heating platform is as follows Figure 8 shown.
[0088] Depend on Figure 7 It can be seen that the bidirectionally frozen PTFE porous sponge prepared in this embodiment has a pore structure arranged in layers. Figure 8 It can be seen that when the working temperature of the bottom heating table reaches 110°C, the surface temperature of the PTFE porous sponge is still 48.1°C, which proves that the PTFE porous sponge has good thermal stability and thermal insulation properties.
[0089] Example 10
[0090] A method for preparing a perfluoropolymer porous sponge comprises the following steps:
[0091] S1, preparation of suspension: magnetically stirring a water-based emulsion of PVP with a mass fraction of 0.1 wt% and PTFE with a solid content of 60 wt% at room temperature for 3 h at a speed of 400 r / min, wherein the solid content ratio of PTFE to PVP is 8:1, and standing for degassing to obtain a suspension;
[0092] S2, preparation of primary PTFE-based porous sponge: pour the suspension into a container, place it in liquid nitrogen (-195° C.) for directional freezing for 2 h to obtain a uniformly dispersed PTFE sol-gel; and then freeze-dry it at -40° C. for 24 h to obtain a self-supporting primary PTFE-based porous sponge;
[0093] S3, post-treatment of primary PTFE-based porous sponge: the self-supporting primary PTFE-based porous sponge obtained in S2 is sintered at a sintering temperature of 380° C. and a sintering time of 10 min to obtain a PTFE porous sponge.
[0094] Depend on Fig. 9 It can be seen that the directionally frozen PTFE porous sponge prepared in this embodiment has a directionally arranged pore structure.
[0095] Embodiment 11
[0096] A method for preparing a perfluoropolymer porous sponge comprises the following steps:
[0097] S1, preparation of suspension: Al2O3 nanoparticles are ultrasonically dispersed in a PEG aqueous solution with a mass fraction of 0.1wt%, and then a PTFE water-based emulsion with a solid content of 60wt% is added, and magnetic stirring is performed at room temperature for 3h at a speed of 300r / min, wherein the solid content ratio of PTFE, PEG and Al2O3 is 5:1:0.001, and after standing and degassing, a suspension is obtained;
[0098] S2, preparation of primary PTFE-based porous sponge: pour the suspension into a container, freeze it in a -70°C low-temperature refrigerator for 1 hour to obtain a uniformly dispersed Al2O3 / PTFE sol-gel; and then freeze-dry it at -40°C for 18 hours to obtain a self-supporting primary Al2O3 / PTFE-based porous sponge;
[0099] S3, post-treatment of primary PTFE-based porous sponge: The self-supporting primary Al2O3 / PTFE-based porous sponge obtained in S2 was sintered at a sintering temperature of 380°C and a sintering time of 10 min to obtain an Al2O3 / PTFE three-dimensional porous sponge.
[0100] Depend on Fig.10 It can be seen that the water contact angle of the Al2O3 / PTFE porous sponge prepared in this embodiment is greater than 150°, and has superhydrophobic properties.
Claims
1. A method for preparing a perfluoropolymer porous sponge, characterized in that The following steps are involved: S1, preparation of suspension: uniformly mixing an aqueous solution of a water-soluble polymer and an aqueous perfluoropolymer emulsion to obtain a suspension, wherein the solid content ratio of the perfluoropolymer to the water-soluble polymer is (1-20):1; S2, preparation of a primary perfluoropolymer-based porous sponge: freezing the suspension at -195 to -10°C for 10 min to 24 h to obtain a uniformly dispersed perfluoropolymer-based sol-gel, and freeze-drying to obtain a primary perfluoropolymer-based porous sponge; S3, post-treatment of the perfluoropolymer porous sponge: sintering the primary perfluoropolymer porous sponge obtained in S2 to oxidatively decompose the water-soluble polymer to obtain a perfluoropolymer porous sponge.
2. The preparation method according to claim 1, characterized in that: In S1, the functional nanoparticles are firstly uniformly dispersed in the aqueous solution of the water-soluble polymer, and then mixed with the perfluoropolymer water-based emulsion.
3. The preparation method according to claim 2, characterized in that: The functional nanoparticles are one of titanium dioxide, ferroferric oxide, zinc oxide, aluminum oxide, cerium oxide, MXene, carbon nanotubes and graphene; the solid content ratio of the functional nanoparticles to the perfluoropolymer is (0.001-1):
10.
4. The preparation method according to claim 1, characterized in that: In S1, the water-soluble polymer is one of polyvinyl alcohol, polyethylene oxide, polyethylene glycol, polyvinyl pyrrolidone and sodium alginate; in the aqueous solution of the water-soluble polymer, the mass fraction of the water-soluble polymer is 0.1-2wt%.
5. The preparation method according to claim 1, characterized in that: In S1, the perfluoropolymer water-based emulsion is one of PTFE water-based emulsion, FEP water-based emulsion and PFA water-based emulsion.
6. The preparation method according to claim 5, characterized in that: In S1, the solid content of the perfluoropolymer water-based emulsion is 40-60 wt%.
7. The preparation method according to claim 1, characterized in that: In S1, the suspension is prepared by: blending a perfluoropolymer water-based emulsion and a water-soluble polymer aqueous solution at room temperature, stirring the mixture magnetically at a speed of 200 to 400 r / min for 1 to 6 hours, and standing the mixture for degassing.
8. The preparation method according to claim 1, characterized in that: In S2, the freeze-drying temperature is -10 to -40°C and the time is 9 to 36 hours.
9. The preparation method according to claim 1, characterized in that: In S3, the sintering temperature is 250 to 400°C and the sintering time is 10 to 60 minutes.
10. A porous perfluoropolymer sponge prepared by the preparation method according to any one of claims 1 to 9, characterized in that: Density: 0.0430~0.1503g / cm 3 The porosity is 71.64-98.05%, and the water contact angle is greater than 150°.