Preparation method of novel cable sheath material and cable sheath

By introducing dynamic disulfide bonds and alginate into polyorganosiloxanes, a self-healing ceramic layer is formed, which solves the problem of structural collapse and mechanical properties of ceramicized silicone rubber during flame erosion, and realizes the self-healing of cable sheath Repair and flame retardant effects enhance the fire resistance of the cable.

CN119019764APending Publication Date: 2024-11-26XIAN UNIV OF TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411281464.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-13
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

The existing ceramic silicone rubber cable sheath collapses when flame erodes, and its mechanical properties decrease, causing moisture and dust to enter the cable, causing fire, and poor wear resistance and easy to damage.

Method used

Dynamic disulfide bonds are introduced into the polyorganosiloxane network by graft copolymerization, and alginate is added therein to form a self-healing ceramic layer to retardant and flame isolation, improving mechanical properties.

Benefits of technology

The self-repair and flame retardant properties of the cable sheath are realized, which avoids the entry of water and dust, enhances the mechanical properties, effectively hinders the spread of flames, and improves the fire resistance of the cable.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
Patent Text Reader

Abstract

The invention discloses a preparation method of a novel cable sheath material and a cable sheath, and the preparation method specifically comprises the following steps: carboxylating amino-terminated polysiloxane, grafting a dynamic disulfide bond to carboxyl-terminated polysiloxane, adding alginate into carboxyl-terminated polysiloxane, and carrying out a dehydration polymerization reaction to obtain the novel cable sheath material. And finally, drying and curing to obtain the novel cable sheath material. According to the cable sheath material, dynamic disulfide bonds are introduced into a polysiloxane network, so that a self-repairing function is realized, steam and dust are effectively prevented from invading, and a fire disaster is prevented. Metal elements are fused into a network by adopting alginate, so that the mechanical property of polysiloxane is enhanced. When the cable encounters flame, alginate and polysiloxane can be decomposed to absorb heat, and the decomposed product of alginate and amorphous SiO2 act together to form a compact ceramic layer to isolate internal cables from external oxygen and flame, so that the flame-retardant effect is achieved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of cable sheath material preparation, and in particular relates to a preparation method of a novel cable sheath material and a cable sheath. Background Art

[0002] The cable sheath is the outermost layer of the cable. As the most important barrier to protect the internal structure of the cable, it protects the cable from mechanical damage during and after installation. At the same time, when the cable catches fire, it can inhibit the spread of flames and implicate other cables, achieving flame retardancy with high efficiency. Ceramic silicone rubber is a new type of material prepared by adding special fillers to the silicone rubber matrix. It has excellent fire resistance, excellent electrical insulation, and excellent chemical stability. It is widely used in cable insulation fireproof layer, cable sheath, and battery thermal protection. However, there are many problems in the use of ceramic silicone rubber. In order to ensure that the structure of ceramic silicone rubber does not collapse and form a dense ceramic layer when it is eroded by flames, it is necessary to add some inorganic fillers such as flame retardants, fluxing agents, and supporting fillers to ceramic silicone rubber, which is easy to cause the agglomeration of inorganic fillers to damage the mechanical properties of ceramic silicone. At the same time, ceramic silicone has poor wear resistance and the cable sheath is easily damaged, which will cause water vapor and dust to enter the cable and cause breakdown and arcing, thereby causing fire. Therefore, the researchers modified the basic material of ceramic silicone rubber materials, polyorganosiloxane, and used its ceramicization mechanism at high temperature to compound it with functional materials to prepare a new cable sheath material with self-healing and flame retardant properties.

[0003] Polyorganosiloxane is a linear polymer composed of alternating silicon atoms and oxygen atoms, which has excellent electrical insulation, high heat resistance and excellent oxidation resistance. Graft copolymerization is a method of combining two or more monomers in the polymerization process to form a polymer material with a specific structure and performance. It can give the material special functionality by designing monomers with specific functional groups. Dynamic disulfide bonds are grafted into the network of polyorganosiloxane by graft copolymerization. Dynamic disulfide bonds can be reversibly broken and formed at a certain temperature, so that the material can restore the structure and function of the cable sheath through the rearrangement of disulfide bonds after being damaged, preventing external moisture and dust from entering the cable and causing insulation breakdown of the cable, causing fire. In addition, metal elements are introduced into the polyorganosiloxane network through alginate. When eroded by flame, alginate and polyorganosiloxane decompose and absorb heat. At the same time, the decomposition products of alginate react with the amorphous SiO2 produced by the decomposition of polyorganosiloxane to form a dense ceramic layer, which hinders the spread of flames and achieves the purpose of protecting the cable. Therefore, it is of great significance to prepare self-repairing intelligent ceramic cable sheaths.

[0004] Lin Musong et al. (Lin Musong, Li Zhi, Peng Lei, et al. Research on self-healing cable sheath materials with shape memory function [J]. Insulating Materials, 2023, 56(6): 1-8) used cyclodextrin-modified alumina nanoparticles as the main molecule and adamantane-containing acrylate as the guest molecule. The host-guest inclusion complex gave the material self-healing properties, and combined with the reversible non-covalent interaction of hydrogen bonds, the material had shape memory function. However, the material can only withstand a temperature of 200°C, which makes it difficult to prevent the spread of flames when a cable fire occurs.

[0005] The Chinese patent "A fire-resistant cable and its production process" (application number: 202410762355.8, publication number: CN118571576A, publication date: 2024.08.30) discloses a fire-resistant cable and its production process. On the basis of preparing ceramic silicone, loaded microspheres containing platinum particles and nitrogen-phosphorus-sulfur flame retardant system are introduced into the ceramic silicone system, which greatly modifies the carbon-forming ability of silicone rubber and promotes the formation of a denser ceramic layer of silicone rubber, so that the cable has better fire resistance. However, there are too many inorganic fillers in the ceramic silicone rubber, which is easy to form agglomerates during the preparation process, which damages the mechanical properties of the silicone rubber. Summary of the invention

[0006] The first aspect of the present invention aims to provide a method for preparing a novel cable sheath material, which solves the problem in the prior art that the cable sheath is damaged, causing moisture and dust to enter the interior of the cable, and that inorganic fillers agglomerate, causing the mechanical properties of the cable sheath to deteriorate.

[0007] In order to achieve the above object, the technical solution adopted by the present invention is:

[0008] A novel cable sheath material and a preparation method thereof are specifically implemented according to the following steps:

[0009] Step 1, preparation of carboxyl-terminated polyorganosiloxane

[0010] Adding acid anhydride to the amino-terminated polyorganosiloxane, and obtaining the carboxyl-terminated polyorganosiloxane after the reaction is complete;

[0011] Step 2: Preparation of sulfurized carboxyl-terminated polyorganosiloxane

[0012] Adding a photoinitiator to the carboxyl-terminated polyorganosiloxane prepared in step 1, mixing evenly, and then adding a monomer containing a disulfide bond to carry out grafting under UV irradiation to obtain a sulfurized carboxyl-terminated polyorganosiloxane;

[0013] Step 3, Preparation of Alginate

[0014] The alginic acid and the composite metal salt are reacted in an anhydrous ethanol solution until the pH of the solution is neutral, and then placed in a vacuum drying oven for drying to obtain alginate powder;

[0015] Step 4, prepare wet gel

[0016] Adding the alginate powder prepared in step 3 to the sulfurized carboxyl-terminated polyorganosiloxane in step 2, stirring with the aid of an organic solvent until the reaction is fully achieved to obtain a wet gel;

[0017] Step 5: Drying and curing

[0018] The wet gel prepared in step 4 is placed in a drying oven for drying and solidification to obtain a new cable sheath material.

[0019] Furthermore, in step 1, the amino-terminated polyorganosiloxane is any one of amino-terminated silicone oil, amino-terminated polydimethylsiloxane, silicone wax polyether aminopolysiloxane, and amino-terminated polyethylene glycol silane, the acid anhydride is any one of acetic anhydride, phthalic anhydride, maleic anhydride, and maleic anhydride, the molar mass ratio of the acid anhydride to the amino-terminated polyorganosiloxane is 0.75 to 1.5, the stirring speed of the stirring paddle is 5000 r / min to 8000 r / min, and the stirring time is 1 h to 2 h.

[0020] Furthermore, in step 2, the photoinitiator is any one of xanthone, benzophenone, hydrogen peroxide, α-carboxyl ketone, and α-amino ketone, the monomer containing a disulfide bond is any one of diphenylamine disulfide, sulfur disulfide, dodecanethiophosphoric acid, diphenyl disulfide, dimethyl disulfide, and diallyl disulfide, the UV ultraviolet wavelength is 300nm~400nm, the illumination time is 2h~4h, the mass ratio of the terminal carboxyl polyorganosiloxane to the photoinitiator is 10~20, the molar mass ratio of the terminal carboxyl polyorganosiloxane to the disulfide bond monomer is 1.1~1, the stirring speed of the stirring paddle is 5000r / min~8000r / min, and the stirring time is 1h~2h.

[0021] Furthermore, in step 3, the composite metal salt is any one of (MgCl2 and Mg(OH)2), (CaCl2 and Ca(OH)2), and (ZnCl2 and Zn(OH)2), the composite metal salt includes 70% to 90% of the strong base and 10% to 30% of the corresponding metal salt in terms of mass percentage, the sum of the above components is 100%, the mass ratio of the composite metal salt to alginic acid is 0.1 to 0.2, the mass fraction of the solute in anhydrous ethanol is 10wt.% to 20wt.%, the solution pH is 6 to 8, the stirring rate is 700r / min to 900r / min, the stirring time is 30min to 60min, the drying temperature is 30°C to 50°C, and the drying time is 24h to 48h.

[0022] Furthermore, in step 4, the mass ratio of the sulfurized terminal carboxyl polyorganosiloxane to the alginate is 0.5 to 2, the organic solvent is any one of tetrahydrofuran, cyclohexane, toluene, and chloroform, the mass ratio of the solute to the organic solvent is 10 to 20, the stirring speed of the stirring paddle is 5000 r / min to 8000 r / min, and the stirring time is 2 h to 4 h.

[0023] Furthermore, the wet gel in step 5 is placed in a drying oven at 60-100° C. for drying and curing for 3-5 hours.

[0024] The second aspect of the present invention aims to provide a cable sheath, which is made of the cable sheath material prepared by the above preparation method.

[0025] Compared with the prior art, the present invention has the following beneficial effects:

[0026] The new cable sheath material prepared by the present invention can self-repair by repolymerizing the dynamic disulfide bonds in the polyorganosiloxane network after the cable sheath is damaged by rocks and sharp tools, thereby maintaining the original structure and performance of the material and preventing moisture and dust from entering the interior of the cable to cause a fire. In addition, alginate is used to introduce metal elements into the polyorganosiloxane network, thereby improving the mechanical properties of the polyorganosiloxane. At the same time, when eroded by flames, the decomposition of polyorganosiloxane and alginate will absorb part of the heat, and the products generated by the decomposition of alginate will synergize with amorphous SiO2 to form a dense ceramic layer, which prevents the internal cable from contacting with external oxygen and flames, thereby preventing the flame from spreading further and achieving a flame retardant effect. The new cable sheath material prepared by the present invention can self-repair by repolymerizing the dynamic disulfide bonds in the polyorganosiloxane network, thereby maintaining the original structure and performance of the material and preventing moisture and dust from entering the interior of the cable and causing a fire. In addition, alginate is used to introduce metal elements into the polyorganosiloxane network, thereby improving the mechanical properties of the polyorganosiloxane. At the same time, when eroded by flames, the decomposition of polyorganosiloxane and alginate will absorb part of the heat, and the products generated by the decomposition of alginate will synergize with amorphous SiO2 to form a dense ceramic layer, which prevents the internal cable from contacting with external oxygen and flames, thereby preventing the flame from spreading further and achieving a flame retardant effect. The new cable sheath material prepared by the present invention can self-repair by repolymerizing the dynamic disulfide bonds in the polyorganosiloxane network, thereby preventing the cable from contacting with external oxygen and flames and preventing the flame from spreading further, thereby achieving a flame retardant effect. The new cable sheath material prepared by the present invention can self-repair by repolymerizing the dynamic disulfide bonds in the DETAILED DESCRIPTION

[0027] The present invention is described in detail below in conjunction with specific implementation modes.

[0028] A method for preparing a novel cable sheath material is specifically implemented according to the following steps:

[0029] Step 1, preparation of carboxyl-terminated polyorganosiloxane

[0030] Acid anhydride is added to the amino-terminated polyorganosiloxane, and the mixture is stirred for 1 h to 2 h using a stirring paddle at 5000 r / min to 8000 r / min to obtain a carboxyl-terminated polyorganosiloxane, wherein the amino-terminated polyorganosiloxane is any one of amino-terminated silicone oil, amino-terminated polydimethylsiloxane, silicone wax polyether aminopolysiloxane, and amino-terminated polyethylene glycol silane, and the acid anhydride is any one of acetic anhydride, phthalic anhydride, maleic anhydride, and maleic anhydride, and the molar mass ratio of the acid anhydride to the amino-terminated polyorganosiloxane is 0.75 to 1.5.

[0031] Step 2: Preparation of sulfurized carboxyl-terminated polyorganosiloxane

[0032] A photoinitiator is added to the carboxyl-terminated polyorganosiloxane prepared in step 1, and a monomer containing a disulfide bond is added after stirring for 1 h to 2 h with a stirring paddle at 5000 r / min to 8000 r / min, and UV ultraviolet rays with a wavelength of 300 nm to 400 nm are irradiated for 2 h to 4 h for grafting to obtain a sulfurized carboxyl-terminated polyorganosiloxane, wherein the photoinitiator is any one of xanthone, benzophenone, hydrogen peroxide, α-carboxyl ketone, and α-amino ketone, and the monomer containing a disulfide bond is any one of diphenylamine disulfide, sulfur disulfide, dodecanethiophosphoric acid, diphenyl disulfide, dimethyl disulfide, and diallyl disulfide, the mass ratio of the carboxyl-terminated polyorganosiloxane to the photoinitiator is 10 to 20, and the molar mass ratio of the carboxyl-terminated polyorganosiloxane to the disulfide bond monomer is 1.1 to 1.

[0033] Step 3, Preparation of Alginate

[0034] The composite metal salt and alginic acid are mixed in an anhydrous ethanol solution in a mass ratio of 0.1 to 0.2 at a stirring rate of 700 r / min to 900 r / min for 30 min to 60 min until the pH value of the solution is 6 to 8, and then placed in a vacuum drying oven at 30°C to 50°C and dried for 24 h to 48 h to obtain alginate powder, wherein the composite metal salt is any one of (MgCl2 and Mg(OH)2), (CaCl2 and Ca(OH)2), and (ZnCl2 and Zn(OH)2), and the composite metal salt includes 70% to 90% of the strong base and 10% to 30% of the corresponding metal salt in terms of mass percentage, the sum of the above components is 100%, and the mass fraction of the solute in the anhydrous ethanol is 10wt.% to 20wt.%.

[0035] Step 4, prepare wet gel

[0036] Add the alginate powder prepared in step 3 to the sulfurized terminal carboxyl polyorganosiloxane in step 2, and stir with a stirring paddle at 5000 r / min to 8000 r / min for 2 h to 4 h until sufficient reaction to obtain a wet gel, wherein the mass ratio of the sulfurized terminal carboxyl polyorganosiloxane to the alginate is 0.5 to 2, the organic solvent is any one of tetrahydrofuran, cyclohexane, toluene, and chloroform, and the mass ratio of the solute to the organic solvent is 10 to 20.

[0037] Step 5: Drying and curing

[0038] The wet gel prepared in step 4 is placed in a drying oven at 60-100° C. for drying and curing for 3-5 hours to obtain a new cable sheath material.

[0039] The present invention selects to use polyorganosiloxane as the matrix of the cable sheath material. When eroded by flame, the polyorganosiloxane on the side close to the fire source decomposes to generate an amorphous SiO2 ceramic layer, which isolates the internal material from the external flame and oxygen, thereby achieving the purpose of flame retardancy. At the same time, alginate is introduced into the polyorganosiloxane. The presence of metal elements in alginate can improve the mechanical properties of the sheath to a certain extent. In addition, when the sheath is eroded by flame, the residue generated by the decomposition of alginate can synergize with amorphous SiO2 to form a dense ceramic layer, further improving the flame retardant effect. In the process of outdoor cable equipment, the cable sheath may be damaged by various tools. The dynamic disulfide bond is introduced into the polyorganosiloxane network, relying on the reversible fracture and formation of the dynamic disulfide bond, to ensure that the sheath can achieve self-repair after being damaged, thereby preventing moisture and dust and other substances from entering the cable, causing cable insulation breakdown and causing fire.

[0040] The new cable sheath material prepared by the present invention can self-repair by repolymerization of the dynamic disulfide bonds in the polyorganosiloxane network after the cable sheath is damaged by rocks and sharp tools, thereby maintaining the original structure and performance of the material; in addition, alginate is used to introduce metal elements into the polyorganosiloxane network to improve the mechanical properties of the polyorganosiloxane, and when eroded by flames, the products generated by the decomposition of alginate will synergize with amorphous SiO2 to form a dense ceramic layer, thereby preventing the flame from spreading further and achieving a flame retardant effect.

[0041] Example 1 Preparation of MG 2+ —PDMS cable sheath material

[0042] First, 3.65 g of maleic anhydride was added to 4.86 g of amino-terminated polydimethylsiloxane, and then stirred for 1 hour with a stirring paddle at 5000 r / min to obtain carboxyl-terminated polydimethylsiloxane; then 0.85 g of xanthone was added to the mixed solution, and stirred for 1 hour with a stirring paddle at 5000 r / min, and then 3.74 g of diphenylamine disulfide was added, and UV ultraviolet rays with a wavelength of 300 nm were irradiated for 2 hours to obtain sulfurized carboxyl-terminated polydimethylsiloxane;

[0043] 0.59 g Mg(OH)2, 0.25 g MgCl2 and 8.43 g alginic acid were dissolved in 90 ml anhydrous ethanol, and stirred on a magnetic stirrer at 700 r / min until the pH value of the solution was 6. Finally, the solution was placed in a vacuum drying oven at 30°C and dried for 24 h to obtain alginate powder.

[0044] 3.49 g of sulfurized terminal carboxyl polydimethylsiloxane and 6.97 g of alginate powder were dissolved in 0.7 g of tetrahydrofuran, and stirred with a stirring paddle at 5000 r / min for 2 h until fully reacted to obtain a wet gel; the prepared wet gel was then placed in a drying oven at 60°C for drying and curing for 3 h to obtain a new cable sheath material.

[0045] Example 2 Preparation of CA 2+ —AWPESO cable sheath material

[0046] First, 0.43 g of phthalic anhydride was added to 5.78 g of silicone wax polyether aminopolysiloxane, and then stirred for 2 hours with a stirring paddle at 7000 r / min to obtain carboxyl-terminated silicone wax polyether aminopolysiloxane; then 0.39 g of benzophenone was added to the mixed solution, and stirred for 2 hours with a stirring paddle at 7000 r / min, and then 0.094 g of dimethyl disulfide was added, and UV ultraviolet rays with a wavelength of 350 nm were irradiated for 3 hours to obtain vulcanized carboxyl-terminated silicone wax polyether aminopolysiloxane;

[0047] 0.74 g of Ca(OH)2, 0.19 g of CaCl2 and 4.62 g of alginic acid were dissolved in 30 ml of anhydrous ethanol, and stirred on a magnetic stirrer at 800 r / min until the pH of the solution was 7. Finally, the solution was placed in a vacuum drying oven at 40°C and dried for 36 h to obtain alginate powder.

[0048] 4.56 g of sulfurized terminal carboxyl silicone wax polyether aminopolysiloxane and 4.56 g of alginate powder were dissolved in 0.46 g of cyclohexane, and stirred with a stirring paddle at 6000 r / min for 3 h until fully reacted to obtain a wet gel; the prepared wet gel was then placed in a drying oven at 70°C for 4 h to dry and cure to obtain a new cable sheath material.

[0049] Example 3 Preparation of ZN 2+ —MPEG cable sheath material

[0050] First, 0.96 g of maleic anhydride was added to 6.56 g of amino-terminated polyethylene glycol silane, and then stirred for 2 h with a stirring paddle at 8000 r / min to obtain carboxyl-terminated polyethylene glycol silane; then 0.33 g of α-amino ketone was added to the mixed solution, and stirred for 1.5 h with a stirring paddle at 8000 r / min, and then 1.48 g of diphenyl disulfide was added, and UV ultraviolet rays with a wavelength of 400 nm were irradiated for 4 h to obtain sulfurized carboxyl-terminated polyethylene glycol silane;

[0051] 0.99 g Zn(OH)2, 0.11 g ZnCl2 and 5.5 g alginate were dissolved in 40 ml anhydrous ethanol and stirred on a magnetic stirrer at 900 r / min until the pH value of the solution was 8. Finally, the solution was placed in a vacuum drying oven at 50°C and dried for 48 h to obtain alginate powder.

[0052] 5.78 g of sulfurized end-carboxyl polyethylene glycol silane and 2.89 g of alginate powder were dissolved in 0.44 g of toluene, and stirred with a stirring paddle at 7000 r / min for 4 hours until fully reacted to obtain a wet gel; the prepared wet gel was then placed in a drying oven at 100°C for drying and curing for 5 hours to obtain a new cable sheath material.

[0053] Example 4 Preparation of CA 2+ —PDMS composite aerogel

[0054] First, 1.38 g of acetic anhydride was added to 4.71 g of amino-terminated polydimethylsiloxane, and then stirred for 1 h with a stirring paddle at 7000 r / min to obtain carboxyl-terminated polydimethylsiloxane; then 0.47 g of benzophenone was added to the mixed solution, and stirred for 2 h with a stirring paddle at 7000 r / min, and then 1.80 g of diallyl disulfide was added, and UV ultraviolet rays with a wavelength of 300 nm were irradiated for 4 h to obtain sulfurized carboxyl-terminated polydimethylsiloxane;

[0055] 0.74 g of Ca(OH)2, 0.32 g of CaCl2 and 5.3 g of alginic acid were dissolved in 80 ml of anhydrous ethanol, and stirred on a magnetic stirrer at 900 r / min until the pH of the solution was 7. Finally, the solution was placed in a vacuum drying oven at 50°C and dried for 48 h to obtain alginate powder.

[0056] 5.35 g of sulfurized end-carboxyl polydimethylsiloxane and 2.68 g of alginate powder were dissolved in 0.8 g of chloroform, and stirred with a stirring paddle at 8000 r / min for 3 h until fully reacted to obtain a wet gel; the prepared wet gel was then placed in a drying oven at 80°C for 4 h to dry and cure to obtain a new cable sheath material.

[0057] Table 1 is a comparison of the mechanical and self-healing properties of the new cable sheath materials in Examples 1-4. As can be seen from Table 1, in terms of mechanical properties, the addition of alginate to the polyorganosiloxane network, thereby introducing metal elements, improves the mechanical properties of polyorganosiloxane to a certain extent, and when subjected to flame erosion, the decomposition products of alginate and the amorphous SiO2 produced by the decomposition of polyorganosiloxane synergistically form a dense ceramic layer, which can isolate external flames and oxygen and improve the flame retardant properties of the material. At the same time, from the comparison of the tensile strength after 24h repair and the tensile strength of the material before damage, the tensile properties of the material after self-repair only show a slight decrease, proving that the introduction of dynamic disulfide bonds can improve the self-healing properties of the sheath material.

[0058] Table 1 Mechanical and self-repairing properties of the new cable sheath materials in Examples 1-4

[0059]

[0060]

[0061] The above-mentioned embodiments only express the specific implementation of the present invention, and the description thereof is relatively specific and detailed, but it cannot be understood as limiting the scope of the invention patent. It should be pointed out that for ordinary technicians in this field, several modifications and improvements can be made without departing from the concept of the present invention, which all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be based on the attached claims.

Claims

1. A method for preparing a new type of cable sheath material, characterized in that: Follow the steps below to implement it: Step 1, preparation of carboxyl-terminated polyorganosiloxane Adding acid anhydride to the amino-terminated polyorganosiloxane, and obtaining the carboxyl-terminated polyorganosiloxane after the reaction is complete; Step 2: Preparation of sulfurized carboxyl-terminated polyorganosiloxane Adding a photoinitiator to the carboxyl-terminated polyorganosiloxane prepared in step 1, mixing evenly, and then adding a monomer containing a disulfide bond to carry out grafting under UV irradiation to obtain a sulfurized carboxyl-terminated polyorganosiloxane; Step 3, Preparation of Alginate The alginic acid and the composite metal salt are stirred and reacted in an anhydrous ethanol solution until the pH of the solution is neutral, and then placed in a vacuum drying oven for drying to obtain alginate powder; Step 4, prepare wet gel Adding the alginate powder prepared in step 3 to the sulfurized carboxyl-terminated polyorganosiloxane in step 2, stirring with the aid of an organic solvent until the reaction is fully achieved to obtain a wet gel; Step 5: Drying and curing The wet gel prepared in step 4 is placed in a drying oven for drying and solidification to obtain a new cable sheath material.

2. The method for preparing a novel cable sheath material according to claim 1, characterized in that: In step 1, the amino-terminated polyorganosiloxane is any one of amino-terminated silicone oil, amino-terminated polydimethylsiloxane, silicone wax polyether aminopolysiloxane, and amino-terminated polyethylene glycol silane, the acid anhydride is any one of acetic anhydride, phthalic anhydride, maleic anhydride, and maleic anhydride, the molar mass ratio of the acid anhydride to the amino-terminated polyorganosiloxane is 0.75 to 1.5, the stirring speed of the stirring paddle is 5000 r / min to 8000 r / min, and the stirring time is 1 h to 2 h.

3. The method for preparing a novel cable sheath material according to claim 1, characterized in that: In step 2, the photoinitiator is any one of xanthone, benzophenone, hydrogen peroxide, α-carboxyl ketone, and α-amino ketone, the monomer containing a disulfide bond is any one of diphenylamine disulfide, sulfur disulfide, dodecanethiophosphoric acid, diphenyl disulfide, dimethyl disulfide, and diallyl disulfide, the UV ultraviolet wavelength is 300nm~400nm, the illumination time is 2h~4h, the mass ratio of the terminal carboxyl polyorganosiloxane to the photoinitiator is 10~20, the molar mass ratio of the terminal carboxyl polyorganosiloxane to the disulfide bond monomer is 1.1~1, the stirring speed of the stirring paddle is 5000r / min~8000r / min, and the stirring time is 1h~2h.

4. The method for preparing a novel cable sheath material according to claim 1, characterized in that: In step 3, the composite metal salt is any one of MgCl2 and Mg(OH)2, CaCl2 and Ca(OH)2, ZnCl2 and Zn(OH)2, the mass ratio of the composite metal salt to alginic acid is 0.1-0.2, the mass fraction of the solute in anhydrous ethanol is 10wt.%-20wt.%, the solution pH is 6-8, the stirring rate is 700r / min-900r / min, the stirring time is 30min-60min, the drying temperature is 30°C-50°C, and the drying time is 24h-48h.

5. The method for preparing a novel cable sheath material according to claim 4, characterized in that: The composite metal salt comprises 70% to 90% of a strong base and 10% to 30% of a corresponding metal salt in terms of mass percentage, and the sum of the above components is 100%.

6. The method for preparing a novel cable sheath material according to claim 1, characterized in that: In step 4, the mass ratio of the sulfurized terminal carboxyl polyorganosiloxane to the alginate is 0.5 to 2, the organic solvent is any one of tetrahydrofuran, cyclohexane, toluene, and chloroform, the mass ratio of the solute to the organic solvent is 10 to 20, the stirring speed of the stirring paddle is 5000 r / min to 8000 r / min, and the stirring time is 2 h to 4 h.

7. The method for preparing a novel cable sheath material according to claim 1, characterized in that: The wet gel in step 5 is placed in a drying oven at 60-100° C. for 3-5 hours.

8. A new type of cable sheath, characterized in that: A cable sheath material prepared by the preparation method described in any one of claims 1 to 7.