Preparation method of packaging hose with high barrier property
By using modified high-density polyethylene and ethylene-vinyl alcohol copolymer materials in the hose, and preparing microgel fillers and injection molding technology in combination with electrospraying method, the problem of poor shoulder barrier performance of existing hose is solved, and the problem of achieving the goal of achieving Efficient barrier performance and simplified processing process meet the needs of high barrier packaging hoses.
Patent Information
- Application Number
- CN202411135817.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-19
- Publication Date
- 2024-11-26
AI Technical Summary
The existing hoses have poor shoulder barrier performance, making it difficult to effectively prevent failure or deterioration of volatile substances or strong permeability substances. At the same time, the processing process of composite sheets is cumbersome.
Modified high-density polyethylene, intermediate layer ethylene-vinyl alcohol copolymer and lower layer modified high-density polyethylene material are used to prepare microgel fillers by electrospraying, and mold them in combination with the extrusion screw distributor of the injection molding machine to form High barrier material pipe shoulders and pipe body improve barrier performance and peel strength.
It significantly improves the transmission rate of oxygen and water vapor, enhances the intermolecular force, improves the barrier performance, simplifies the processing process, improves the peel strength, and meets the needs of high-barrier performance packaging hoses.
Smart Images

Figure BDA0004999399140000151
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of hoses, and in particular to a method for preparing a packaging hose with high barrier performance. Background Art
[0002] A hose is usually composed of a shoulder, a cap and a body. The bodies of existing hoses on the market are mostly made of materials with high barrier properties, thereby preventing substances from volatilizing or leaking.
[0003] Chinese patent CN114379158B discloses a waterproof paper-plastic composite hose and a preparation method thereof, wherein the composite hose comprises a tube cap, a tube shoulder and a tube body; the tube cap is made of modified polypropylene and is injection molded by an injection molding machine; the tube shoulder is made of modified high-density polyethylene and is injection molded by an injection molding machine; the tube body is made of a composite sheet by an extrusion composite process, and the composite sheet comprises a first PE layer, a first adhesive layer, a special paper layer, a second adhesive layer and a second PE layer from the outside to the inside; the composite has high composite strength and good waterproof performance, and can be widely used in various liquid product packaging.
[0004] In the above patent, the tube body is composed of a composite sheet with good waterproof performance, and the tube shoulder is composed of a layer of modified high-density polyethylene material. The barrier performance of the tube shoulder is poor. When it is loaded with some volatile substances, highly permeable substances, or substances that are easy to deteriorate and oxidize, it is easy to cause such substances to become ineffective or deteriorate. In addition, the composite sheet in the above patent is composed of five layers of materials. The first PE layer, the first adhesive layer, the second adhesive layer and the second PE layer need to be extruded separately and then compounded together, and the processing flow is relatively cumbersome.
[0005] Based on this, the present invention designs a method for preparing a packaging hose with high barrier performance to solve the above problems. Summary of the invention
[0006] In view of the above-mentioned shortcomings of the prior art, the present invention provides a method for preparing a packaging hose with high barrier performance.
[0007] To achieve the above objectives, the present invention is implemented through the following technical solutions:
[0008] A method for preparing a high barrier performance packaging hose, comprising a tube body, a tube shoulder and a tube cap;
[0009] The tube cap is made of modified polycarbonate, and the tube shoulder and tube body are made of high barrier material;
[0010] The high barrier material is composed of an upper layer of modified high-density polyethylene, a middle layer of ethylene-vinyl alcohol copolymer, and a lower layer of modified high-density polyethylene;
[0011] The method for preparing the upper layer modified high-density polyethylene and the lower layer modified high-density polyethylene comprises the following steps:
[0012] Step 1, preparing filler;
[0013] A. Preparation of mixed solution:
[0014] Dissolving lignin in lithium bromide trihydrate to obtain a lignin solution, and blending the sodium silicate solution with the lignin solution to obtain a mixed solution;
[0015] B. The mixed liquid is squeezed through the needle at a certain flow rate, and a voltage is applied at the needle tip. When the voltage exceeds a critical value, the liquid at the needle tip overcomes the surface tension to form a micron-sized droplet-shaped charged jet.
[0016] C. Rapidly evaporate the droplets at high temperature and collect the remaining powder to obtain microgel;
[0017] Step 2: Preheat the melting furnace and add high-density polyethylene, heat and melt it, and stir it evenly;
[0018] Step 3, adding thermoplastic phenolic resin as a modifier into a melting furnace, heating and stirring;
[0019] Step 4: slowly add the microgel as filler into the melting furnace, stirring while adding, to obtain a viscous modified high-density polyethylene, and keep it warm for later use;
[0020] Step 5: preparing the tube cap;
[0021] Step 6: co-injection-molding the modified high-density polyethylene and ethylene-vinyl alcohol copolymer through a distributor of an extrusion screw of an injection molding machine to obtain a tube shoulder and a tube body with the middle layer being the ethylene-vinyl alcohol copolymer and the upper and lower layers being both the modified high-density polyethylene;
[0022] Step 7: Weld the tube shoulder to the tube body; then weld the tube cap to the tube shoulder; and prepare a high barrier performance packaging hose.
[0023] Furthermore, in step one, step A is specifically as follows: dissolving 5-8 parts of lignin in 40-60 parts of lithium bromide trihydrate to obtain a lignin solution, and blending 15-30 parts of a Na2SiO3 9H2O aqueous solution with the lignin solution to obtain a mixed solution.
[0024] Furthermore, in step one, step B is specifically as follows: the mixed liquid is extruded through the needle at a flow rate of 0.8-0.9 mL / h, a voltage of 35-40 kV is applied at the needle tip, and the receiving distance is 140-150 mm; when the voltage exceeds the critical value, the liquid at the needle tip overcomes the surface tension to form a micron-sized droplet-shaped charged jet.
[0025] Furthermore, in step 1, the diameter of the microgel is 2.5-3.8 μm.
[0026] Furthermore, in step 2, the melting furnace is preheated for 5-10 minutes and then 90-100 parts of high-density polyethylene are added.
[0027] Furthermore, in step 2, the heating temperature is 180-240°C, and the mixture is stirred for 15-20 minutes after melting;
[0028] Furthermore, step three is specifically as follows: adding 25-36 parts of thermoplastic phenolic resin as a modifier into the melting furnace three times, each time with an interval of 5 minutes, and after adding, heating by 10° C. and stirring for 30-40 minutes.
[0029] Furthermore, step four is specifically as follows: slowly add 18-21 parts of microgel as filler into the melting furnace, add it for 20-25 minutes, stir while adding, to obtain viscous modified high-density polyethylene, and keep it warm for later use.
[0030] Furthermore, in step five, the mass ratio of polycarbonate and the modifier maleic anhydride grafted polypropylene is: (45-52): (21-33).
[0031] Furthermore, in step five, the heating temperature is 170-220°C.
[0032] Compared with the prior art, the present invention has the following beneficial effects:
[0033] 1. The high-barrier packaging hose prepared by the present invention has excellent barrier properties and low oxygen and water vapor transmission rates. This is because the small-diameter microgel filler is evenly dispersed in the high-density polyethylene, thereby achieving improved barrier properties; and the larger groups such as the benzene ring in the phenolic resin and the hydrogen bonding of the phenolic hydroxyl group increase the intermolecular force, thereby improving the bonding strength between the phenolic resin and the high-density polyethylene, thereby reducing the molecular gap and further improving the barrier properties.
[0034] 2. The present invention obtains the tube shoulder and the tube body at one time by co-injection molding through the distributor of the extrusion screw of the injection molding machine, so that the peeling strength is significantly improved. DETAILED DESCRIPTION
[0035] In order to make the purpose, technical solution and advantages of the embodiments of the present invention clearer, the technical solution in the embodiments of the present invention will be clearly and completely described in combination with the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0036] Embodiment 1
[0037] This embodiment provides a method for preparing a high-barrier performance packaging hose, comprising a tube body, a tube shoulder fixedly connected to the tube body, and a tube cap fixedly connected to the tube shoulder;
[0038] The tube cap is made of modified polycarbonate, and the tube shoulder and tube body are made of high barrier material;
[0039] The high barrier material is composed of an upper layer of modified high-density polyethylene, a middle layer of ethylene-vinyl alcohol copolymer, and a lower layer of modified high-density polyethylene;
[0040] The method for preparing the upper layer modified high-density polyethylene and the lower layer modified high-density polyethylene comprises the following steps:
[0041] Step 1, preparing filler;
[0042] A. Preparation of mixed solution:
[0043] 8 kg of lignin was dissolved in 60 kg of lithium bromide trihydrate to obtain a lignin solution, and 30 kg of Na2SiO3 9H2O aqueous solution was mixed with the lignin solution to obtain a mixed solution;
[0044] B. The mixed liquid is squeezed through the needle at a flow rate of 0.9 mL / h, and a voltage of 40 kV is applied at the needle tip. The receiving distance is 150 mm. When the voltage exceeds the critical value, the liquid at the needle tip overcomes the surface tension to form a micron-sized droplet-shaped charged jet.
[0045] C. After the droplets are evaporated quickly at high temperature, the remaining powder is collected to obtain a microgel with a diameter of 3.8 μm;
[0046] Step 2: Preheat the melting furnace for 10 minutes, add 100 kg of high-density polyethylene, heat to 240°C, melt and stir for 20 minutes;
[0047] Step 3: Add 36 kg of thermoplastic phenolic resin as a modifier into the melting furnace three times, each time with an interval of 5 minutes, raise the temperature by 10°C and stir for 40 minutes;
[0048] Step 4: slowly add 21 kg of microgel as filler into the melting furnace for 25 minutes, stirring while adding, to obtain a viscous modified high-density polyethylene, and keep it warm for later use;
[0049] Step 5: After fully mixing 52 kg of polycarbonate and 33 kg of maleic anhydride grafted polypropylene as a modifier, heat to 220°C to melt, and pour into a mold to obtain a tube cap;
[0050] Step 6: co-injection-molding the modified high-density polyethylene and ethylene-vinyl alcohol copolymer through a distributor of an extrusion screw of an injection molding machine to obtain a tube shoulder and a tube body with the middle layer being the ethylene-vinyl alcohol copolymer and the upper and lower layers being both the modified high-density polyethylene;
[0051] Step 7: Weld the tube shoulder to the tube body; then weld the tube cap to the tube shoulder; and prepare a high barrier performance packaging hose.
[0052] The high barrier performance packaging hose prepared in Example 1 was tested according to GB / T 2411-1980 "Plastic Shore Hardness Test Method", and the hardness (HD) was 58, which met the basic performance requirements of the packaging hose.
[0053] Embodiment 2
[0054] This embodiment provides a method for preparing a high-barrier performance packaging hose, comprising a tube body, a tube shoulder fixedly connected to the tube body, and a tube cap fixedly connected to the tube shoulder;
[0055] The tube cap is made of modified polycarbonate, and the tube shoulder and tube body are made of high barrier material;
[0056] The high barrier material is composed of an upper layer of modified high-density polyethylene, a middle layer of ethylene-vinyl alcohol copolymer, and a lower layer of modified high-density polyethylene;
[0057] The method for preparing the upper layer modified high-density polyethylene and the lower layer modified high-density polyethylene comprises the following steps:
[0058] Step 1, preparing filler;
[0059] A. Preparation of mixed solution:
[0060] 5 kg of lignin was dissolved in 40 kg of lithium bromide trihydrate to obtain a lignin solution, and 15 kg of Na2SiO3 9H2O aqueous solution was mixed with the lignin solution to obtain a mixed solution;
[0061] B. The mixed liquid is squeezed through the needle at a flow rate of 0.8 mL / h, and a voltage of 35 kV is applied at the needle tip. The receiving distance is 140 mm. When the voltage exceeds the critical value, the liquid at the needle tip overcomes the surface tension to form a micron-sized droplet-shaped charged jet.
[0062] C. After the droplets are evaporated rapidly at high temperature, the remaining powder is collected to obtain a microgel with a diameter of 2.5 μm;
[0063] Step 2: Preheat the melting furnace for 5 minutes, add 90 kg of high-density polyethylene, heat to 180°C and melt, then stir for 15 minutes;
[0064] Step 3: Add 25 kg of thermoplastic phenolic resin as a modifier into the melting furnace three times, each time with an interval of 5 minutes, and heat up by 10°C and stir for 30 minutes;
[0065] Step 4: slowly add 18 kg of microgel as filler into the melting furnace for 20 minutes, stirring while adding, to obtain a viscous modified high-density polyethylene, and keep it warm for later use;
[0066] Step 5: After fully mixing 45 kg of polycarbonate and 21 kg of maleic anhydride grafted polypropylene as a modifier, heat to 170°C to melt, and pour into a mold to obtain a tube cap;
[0067] Step 6: co-injection-molding the modified high-density polyethylene and ethylene-vinyl alcohol copolymer through a distributor of an extrusion screw of an injection molding machine to obtain a tube shoulder and a tube body with the middle layer being the ethylene-vinyl alcohol copolymer and the upper and lower layers being both the modified high-density polyethylene;
[0068] Step 7: Weld the tube shoulder to the tube body; then weld the tube cap to the tube shoulder; and prepare a high barrier performance packaging hose.
[0069] Embodiment 3
[0070] This embodiment provides a method for preparing a high-barrier performance packaging hose, comprising a tube body, a tube shoulder fixedly connected to the tube body, and a tube cap fixedly connected to the tube shoulder;
[0071] The tube cap is made of modified polycarbonate, and the tube shoulder and tube body are made of high barrier material;
[0072] The high barrier material is composed of an upper layer of modified high-density polyethylene, a middle layer of ethylene-vinyl alcohol copolymer, and a lower layer of modified high-density polyethylene;
[0073] The method for preparing the upper layer modified high-density polyethylene and the lower layer modified high-density polyethylene comprises the following steps:
[0074] Step 1, preparing filler;
[0075] A. Preparation of mixed solution:
[0076] 6 kg of lignin was dissolved in 48 kg of lithium bromide trihydrate to obtain a lignin solution, and 25 kg of Na2SiO3 9H2O aqueous solution was mixed with the lignin solution to obtain a mixed solution;
[0077] B. The mixed liquid is squeezed through the needle at a flow rate of 0.83 mL / h, and a voltage of 37 kV is applied at the needle tip; the receiving distance is 146 mm; when the voltage exceeds the critical value, the liquid at the needle tip overcomes the surface tension to form a micron-sized droplet-shaped charged jet;
[0078] C. After the droplets are evaporated rapidly at high temperature, the remaining powder is collected to obtain microgels with a diameter of 2.5-3.8 μm;
[0079] Step 2: Preheat the melting furnace for 6 minutes, add 98 kg of high-density polyethylene, heat to 210°C and melt, then stir for 16 minutes;
[0080] Step 3: Add 34 kg of thermoplastic phenolic resin as a modifier into the melting furnace three times, each time with an interval of 5 minutes, and heat up to 10°C and stir for 31 minutes;
[0081] Step 4: slowly add 20 kg of microgel as filler into the melting furnace for 22 minutes, stirring while adding, to obtain a viscous modified high-density polyethylene, and keep it warm for later use;
[0082] Step 5: After fully mixing 50 kg of polycarbonate and 28 kg of maleic anhydride grafted polypropylene as a modifier, heat to 200° C. to melt, and pour into a mold to obtain a tube cap;
[0083] Step 6: co-injection-molding the modified high-density polyethylene and ethylene-vinyl alcohol copolymer through a distributor of an extrusion screw of an injection molding machine to obtain a tube shoulder and a tube body with the middle layer being the ethylene-vinyl alcohol copolymer and the upper and lower layers being both the modified high-density polyethylene;
[0084] Step 7: Weld the tube shoulder to the tube body; then weld the tube cap to the tube shoulder; and prepare a high barrier performance packaging hose.
[0085] Embodiment 4
[0086] This embodiment provides a method for preparing a high-barrier performance packaging hose, comprising a tube body, a tube shoulder fixedly connected to the tube body, and a tube cap fixedly connected to the tube shoulder;
[0087] The tube cap is made of modified polycarbonate, and the tube shoulder and tube body are made of high barrier material;
[0088] The high barrier material is composed of an upper layer of modified high-density polyethylene, a middle layer of ethylene-vinyl alcohol copolymer, and a lower layer of modified high-density polyethylene;
[0089] The method for preparing the upper layer modified high-density polyethylene and the lower layer modified high-density polyethylene comprises the following steps:
[0090] Step 1, preparing filler;
[0091] A. Preparation of mixed solution:
[0092] 7 kg of lignin was dissolved in 45 kg of lithium bromide trihydrate to obtain a lignin solution, and 18 kg of Na2SiO3 9H2O aqueous solution was mixed with the lignin solution to obtain a mixed solution;
[0093] B. The mixed liquid is squeezed out through the needle at a flow rate of 0.81 mL / h, and a voltage of 39 kV is applied at the needle tip; the receiving distance is 148 mm; when the voltage exceeds the critical value, the liquid at the needle tip overcomes the surface tension to form a micron-sized droplet-shaped charged jet;
[0094] C. After the droplets are evaporated quickly at high temperature, the remaining powder is collected to obtain a microgel with a diameter of 2.8 μm;
[0095] Step 2: Preheat the melting furnace for 6 minutes, add 97 kg of high-density polyethylene, heat to 230°C and melt, then stir for 19 minutes;
[0096] Step 3: Add 27 kg of thermoplastic phenolic resin as a modifier into the melting furnace three times, each time with an interval of 5 minutes, and heat up by 10°C and stir for 34 minutes;
[0097] Step 4: slowly add 20 kg of microgel as filler into the melting furnace for 21 minutes, stirring while adding, to obtain a viscous modified high-density polyethylene, and keep it warm for later use;
[0098] Step 5: After fully mixing 50 kg of polycarbonate and 30 kg of maleic anhydride grafted polypropylene as a modifier, heat to 190° C. to melt, and pour into a mold to obtain a tube cap;
[0099] Step 6: co-injection-molding the modified high-density polyethylene and ethylene-vinyl alcohol copolymer through a distributor of an extrusion screw of an injection molding machine to obtain a tube shoulder and a tube body with the middle layer being the ethylene-vinyl alcohol copolymer and the upper and lower layers being both the modified high-density polyethylene;
[0100] Step 7: Weld the tube shoulder to the tube body; then weld the tube cap to the tube shoulder; and prepare a high barrier performance packaging hose.
[0101] Embodiment 5
[0102] This embodiment provides a method for preparing a high-barrier performance packaging hose, comprising a tube body, a tube shoulder fixedly connected to the tube body, and a tube cap fixedly connected to the tube shoulder;
[0103] The tube cap is made of modified polycarbonate, and the tube shoulder and tube body are made of high barrier material;
[0104] The high barrier material is composed of an upper layer of modified high-density polyethylene, a middle layer of ethylene-vinyl alcohol copolymer, and a lower layer of modified high-density polyethylene;
[0105] The method for preparing the upper layer modified high-density polyethylene and the lower layer modified high-density polyethylene comprises the following steps:
[0106] Step 1, preparing filler;
[0107] A. Preparation of mixed solution:
[0108] 6.9 kg of lignin was dissolved in 44 kg of lithium bromide trihydrate to obtain a lignin solution, and 22 kg of Na2SiO3 9H2O aqueous solution was mixed with the lignin solution to obtain a mixed solution;
[0109] B. The mixed liquid is squeezed through the needle at a flow rate of 0.88 mL / h, and a voltage of 39 kV is applied at the needle tip; the receiving distance is 145 mm; when the voltage exceeds the critical value, the liquid at the needle tip overcomes the surface tension to form a micron-sized droplet-shaped charged jet;
[0110] C. After the droplets are evaporated rapidly at high temperature, the remaining powder is collected to obtain a microgel with a diameter of 3.1 μm;
[0111] Step 2: Preheat the melting furnace for 7 minutes, add 94 kg of high-density polyethylene, heat to 210°C and melt, then stir for 17 minutes;
[0112] Step 3: Add 26 kg of thermoplastic phenolic resin as a modifier into the melting furnace three times, each time with an interval of 5 minutes, and heat up by 10°C and stir for 36 minutes;
[0113] Step 4: slowly add 19 kg of microgel as filler into the melting furnace for 24 minutes, stirring while adding, to obtain a viscous modified high-density polyethylene, and keep it warm for later use;
[0114] Step 5: After fully mixing 46 kg of polycarbonate and 26 kg of maleic anhydride grafted polypropylene as a modifier, heat to 185°C to melt, and pour into a mold to obtain a tube cap;
[0115] Step 6: co-injection-molding the modified high-density polyethylene and ethylene-vinyl alcohol copolymer through a distributor of an extrusion screw of an injection molding machine to obtain a tube shoulder and a tube body with the middle layer being the ethylene-vinyl alcohol copolymer and the upper and lower layers being both the modified high-density polyethylene;
[0116] Step 7: Weld the tube shoulder to the tube body; then weld the tube cap to the tube shoulder; and prepare a high barrier performance packaging hose.
[0117] Embodiment 6
[0118] This embodiment provides a method for preparing a high-barrier performance packaging hose, comprising a tube body, a tube shoulder fixedly connected to the tube body, and a tube cap fixedly connected to the tube shoulder;
[0119] The tube cap is made of modified polycarbonate, and the tube shoulder and tube body are made of high barrier material;
[0120] The high barrier material is composed of an upper layer of modified high-density polyethylene, a middle layer of ethylene-vinyl alcohol copolymer, and a lower layer of modified high-density polyethylene;
[0121] The method for preparing the upper layer modified high-density polyethylene and the lower layer modified high-density polyethylene comprises the following steps:
[0122] Step 1, preparing filler;
[0123] A. Preparation of mixed solution:
[0124] 6 kg of lignin was dissolved in 47 kg of lithium bromide trihydrate to obtain a lignin solution, and 19 kg of Na2SiO3 9H2O aqueous solution was mixed with the lignin solution to obtain a mixed solution;
[0125] B. The mixed liquid is squeezed through the needle at a flow rate of 0.84 mL / h, and a voltage of 38 kV is applied at the needle tip; the receiving distance is 149 mm; when the voltage exceeds the critical value, the liquid at the needle tip overcomes the surface tension to form a micron-sized droplet-shaped charged jet;
[0126] C. After the droplets are evaporated rapidly at high temperature, the remaining powder is collected to obtain a microgel with a diameter of 3.3 μm;
[0127] Step 2: Preheat the melting furnace for 6 minutes, add 99 kg of high-density polyethylene, heat to 220°C and melt, then stir for 16 minutes;
[0128] Step 3: Add 31 kg of thermoplastic phenolic resin as a modifier into the melting furnace three times, each time with an interval of 5 minutes, raise the temperature by 10°C and stir for 33 minutes;
[0129] Step 4: slowly add 20 kg of microgel as filler into the melting furnace for 22 minutes, stirring while adding, to obtain a viscous modified high-density polyethylene, and keep it warm for later use;
[0130] Step 5: After fully mixing 50 kg of polycarbonate and 28 kg of maleic anhydride grafted polypropylene as a modifier, heat to 210° C. to melt, and pour into a mold to obtain a tube cap;
[0131] Step 6: co-injection-molding the modified high-density polyethylene and ethylene-vinyl alcohol copolymer through a distributor of an extrusion screw of an injection molding machine to obtain a tube shoulder and a tube body with the middle layer being the ethylene-vinyl alcohol copolymer and the upper and lower layers being both the modified high-density polyethylene;
[0132] Step 7: Weld the tube shoulder to the tube body; then weld the tube cap to the tube shoulder; and prepare a high barrier performance packaging hose.
[0133] Comparative Example 1
[0134] The difference from Example 6 is that step B in step 1 is missing.
[0135] This embodiment provides a method for preparing a high-barrier performance packaging hose, comprising a tube body, a tube shoulder fixedly connected to the tube body, and a tube cap fixedly connected to the tube shoulder;
[0136] The tube cap is made of modified polycarbonate, and the tube shoulder and tube body are made of high barrier material;
[0137] The high barrier material is composed of an upper layer of modified high-density polyethylene, a middle layer of ethylene-vinyl alcohol copolymer, and a lower layer of modified high-density polyethylene;
[0138] The method for preparing the upper layer modified high-density polyethylene and the lower layer modified high-density polyethylene comprises the following steps:
[0139] Step 1, preparing filler;
[0140] A. Preparation of mixed solution:
[0141] 6 kg of lignin was dissolved in 47 kg of lithium bromide trihydrate to obtain a lignin solution, and 19 kg of Na2SiO3 9H2O aqueous solution was mixed with the lignin solution to obtain a mixed solution;
[0142] C. After the mixed solution is evaporated rapidly at high temperature, the remaining powder is collected to obtain a microgel with a diameter of 3.3 μm;
[0143] Step 2: Preheat the melting furnace for 6 minutes, add 99 kg of high-density polyethylene, heat to 220°C and melt, then stir for 16 minutes;
[0144] Step 3: Add 31 kg of thermoplastic phenolic resin as a modifier into the melting furnace three times, each time with an interval of 5 minutes, raise the temperature by 10°C and stir for 33 minutes;
[0145] Step 4: slowly add 20 kg of microgel as filler into the melting furnace for 22 minutes, stirring while adding, to obtain a viscous modified high-density polyethylene, and keep it warm for later use;
[0146] Step 5: After fully mixing 50 kg of polycarbonate and 28 kg of maleic anhydride grafted polypropylene as a modifier, heat to 210° C. to melt, and pour into a mold to obtain a tube cap;
[0147] Step 6: co-injection-molding the modified high-density polyethylene and ethylene-vinyl alcohol copolymer through a distributor of an extrusion screw of an injection molding machine to obtain a tube shoulder and a tube body with the middle layer being the ethylene-vinyl alcohol copolymer and the upper and lower layers being both the modified high-density polyethylene;
[0148] Step 7: Weld the tube shoulder to the tube body; then weld the tube cap to the tube shoulder; and prepare a high barrier performance packaging hose.
[0149] Comparative Example 2
[0150] The difference from Example 6 is that a raw material Na2SiO3 9H2O aqueous solution is missing in step 1.
[0151] This embodiment provides a method for preparing a high-barrier performance packaging hose, comprising a tube body, a tube shoulder fixedly connected to the tube body, and a tube cap fixedly connected to the tube shoulder;
[0152] The tube cap is made of modified polycarbonate, and the tube shoulder and tube body are made of high barrier material;
[0153] The high barrier material is composed of an upper layer of modified high-density polyethylene, a middle layer of ethylene-vinyl alcohol copolymer, and a lower layer of modified high-density polyethylene;
[0154] The method for preparing the upper layer modified high-density polyethylene and the lower layer modified high-density polyethylene comprises the following steps:
[0155] Step 1, preparing filler;
[0156] A. Preparation of mixed solution:
[0157] Dissolving 6 kg of lignin in 47 kg of lithium bromide trihydrate to obtain a lignin solution;
[0158] B. The lignin solution is extruded through the needle at a flow rate of 0.84 mL / h, and a voltage of 38 kV is applied at the needle tip; the receiving distance is 149 mm; when the voltage exceeds the critical value, the liquid at the needle tip overcomes the surface tension to form a micron-sized droplet-shaped charged jet;
[0159] C. After the droplets are evaporated rapidly at high temperature, the remaining powder is collected to obtain a microgel with a diameter of 3.3 μm;
[0160] Step 2: Preheat the melting furnace for 6 minutes, add 99 kg of high-density polyethylene, heat to 220°C and melt, then stir for 16 minutes;
[0161] Step 3: Add 31 kg of thermoplastic phenolic resin as a modifier into the melting furnace three times, each time with an interval of 5 minutes, raise the temperature by 10°C and stir for 33 minutes;
[0162] Step 4: slowly add 20 kg of microgel as filler into the melting furnace for 22 minutes, stirring while adding, to obtain a viscous modified high-density polyethylene, and keep it warm for later use;
[0163] Step 5: After fully mixing 50 kg of polycarbonate and 28 kg of maleic anhydride grafted polypropylene as a modifier, heat to 210° C. to melt, and pour into a mold to obtain a tube cap;
[0164] Step 6: co-injection-molding the modified high-density polyethylene and ethylene-vinyl alcohol copolymer through a distributor of an extrusion screw of an injection molding machine to obtain a tube shoulder and a tube body with the middle layer being the ethylene-vinyl alcohol copolymer and the upper and lower layers being both the modified high-density polyethylene;
[0165] Step 7: Weld the tube shoulder to the tube body; then weld the tube cap to the tube shoulder; and prepare a high barrier performance packaging hose.
[0166] Experimental Example 1
[0167] According to the standard of GB / T 1038.1-2022, oxygen permeability tests were performed on the tube shoulders prepared in Examples 1, 2, 3, 4, 5, and 6, the tube shoulders prepared in Comparative Example 1, and the tube shoulders prepared in Comparative Example 2, respectively. The oxygen permeability of the tube body under standard atmospheric pressure for 24 hours was tested, and the results were as follows:
[0168] Instrument: OX2 / 230 oxygen transmission rate tester;
[0169] According to the standard of GB / T 26253-2010, the water vapor transmission rate of each group of products was tested. The water permeability rate of the test tube body under standard atmospheric pressure for 24 hours was tested. The results are as follows:
[0170] Instrument: 3 / 33MA Vapor Permeability Tester;
[0171] According to the standard of GB / T 8808-1988, each group of products was subjected to peeling test, with the peeling angle of 90 degrees. The results are as follows:
[0172]
[0173] As can be seen from the above table, the high-barrier packaging hose prepared by the present invention has excellent barrier properties, and the oxygen and water vapor transmission rates are low. This is because the small-diameter microgel filler is evenly dispersed in the high-density polyethylene, thereby achieving improved barrier properties; and the larger groups such as the benzene ring in the phenolic resin and the hydrogen bonding of the phenolic hydroxyl group increase the intermolecular force, thereby improving the bonding strength between the phenolic resin and the high-density polyethylene, thereby reducing the molecular gap and further improving the barrier properties;
[0174] In addition, the present invention obtains the tube shoulder and the tube body at one time by co-injection molding through the distributor of the extrusion screw of the injection molding machine, so that the peeling strength is significantly improved.
[0175] The above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit the same. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that the technical solutions described in the aforementioned embodiments may still be modified, or some of the technical features may be replaced by equivalents. Such modifications or replacements will not cause the essence of the corresponding technical solutions to deviate from the spirit and scope of the technical solutions of the embodiments of the present invention.
Claims
1. A method for preparing a packaging hose with high barrier properties, characterized in that: Including pipe body, pipe shoulder and pipe cap; The tube cap is made of modified polycarbonate, and the tube shoulder and tube body are made of high barrier material; The high barrier material is composed of an upper layer of modified high-density polyethylene, a middle layer of ethylene-vinyl alcohol copolymer, and a lower layer of modified high-density polyethylene; The method for preparing the upper layer modified high-density polyethylene and the lower layer modified high-density polyethylene comprises the following steps: Step 1, preparing filler; A. Preparation of mixed solution: Dissolving lignin in lithium bromide trihydrate to obtain a lignin solution, and blending the sodium silicate solution with the lignin solution to obtain a mixed solution; B. The mixed liquid is squeezed through the needle at a certain flow rate, and a voltage is applied at the needle tip. When the voltage exceeds a critical value, the liquid at the needle tip overcomes the surface tension to form a micron-sized droplet-shaped charged jet. C. Rapidly evaporate the droplets at high temperature and collect the remaining powder to obtain microgel; Step 2: Preheat the melting furnace and add high-density polyethylene, heat and melt it, and stir it evenly; Step 3, adding thermoplastic phenolic resin as a modifier into a melting furnace, heating and stirring; Step 4: slowly add the microgel as filler into the melting furnace, stirring while adding, to obtain a viscous modified high-density polyethylene, and keep it warm for later use; Step 5: preparing the tube cap; Step 6: co-injection-molding the modified high-density polyethylene and ethylene-vinyl alcohol copolymer through a distributor of an extrusion screw of an injection molding machine to obtain a tube shoulder and a tube body with the middle layer being the ethylene-vinyl alcohol copolymer and the upper and lower layers being both the modified high-density polyethylene; Step 7: Weld the tube shoulder to the tube body; then weld the tube cap to the tube shoulder; and prepare a high barrier performance packaging hose.
2. The preparation method according to claim 1, characterized in that: In step one, step A is specifically as follows: dissolving 5-8 parts of lignin in 40-60 parts of lithium bromide trihydrate to obtain a lignin solution, and blending 15-30 parts of a Na2SiO3 9H2O aqueous solution with the lignin solution to obtain a mixed solution.
3. The preparation method according to claim 2, characterized in that: In step one, step B is specifically as follows: the mixed liquid is extruded through the needle at a flow rate of 0.8-0.9 mL / h, a voltage of 35-40 kV is applied at the needle tip, and the receiving distance is 140-150 mm; when the voltage exceeds the critical value, the liquid at the needle tip overcomes the surface tension to form a micron-sized droplet-shaped charged jet.
4. The preparation method according to claim 3, characterized in that: In step 1, the diameter of the microgel is 2.5-3.8 μm.
5. The preparation method according to claim 4, characterized in that: In step 2, the melting furnace is preheated for 5-10 minutes and then 90-100 parts of high-density polyethylene are added.
6. The preparation method according to claim 5, characterized in that: In step 2, the heating temperature is 180-240° C. and the mixture is stirred for 15-20 minutes after melting.
7. The preparation method according to claim 6, characterized in that: Step three is as follows: 25-36 parts of thermoplastic phenolic resin as a modifier are added to the melting furnace three times, with an interval of 5 minutes between each addition, and after the addition is completed, the temperature is raised by 10° C. and stirred for 30-40 minutes.
8. The preparation method according to claim 7, characterized in that: Step 4 is as follows: slowly add 18-21 parts of microgel as filler into the melting furnace, add it for 20-25 minutes, stir while adding, to obtain viscous modified high-density polyethylene, and keep it warm for later use.
9. The preparation method according to claim 8, characterized in that: In step 5, the mass ratio of polycarbonate and the modifier maleic anhydride grafted polypropylene is: (45-52): (21-33).
10. The preparation method according to claim 9, characterized in that: In step 5, the heating temperature is 170-220°C.
