High-temperature-resistant polyethylene material and preparation method thereof
By adding triazine-based flame retardant and nano-alumina to the polyethylene material, the problem of insufficient flame retardant and high-temperature resistance performance of polyethylene materials is solved, and better high-temperature resistance and flame retardant effects are achieved.
Patent Information
- Application Number
- CN202411288860.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-14
- Publication Date
- 2024-11-26
AI Technical Summary
The poor flame retardant and high temperature resistance of existing polyethylene materials limit their development in some applications.
High temperature-resistant polyethylene materials are prepared by melt-extruded triazine-based flame retardant, calcium carbonate, antioxidant 1076 and polyethylene resin in an extruder. The triazine-based flame retardant is obtained through reaction and used to use it at high temperatures. Decompose the acidic substances and non-combustible gases that produce flame retardant effects, and nano-alumina form carbonized heat insulation.
It significantly improves the flame retardant performance and high temperature resistance of the material, reduces the combustion speed and thermal conductivity, and enhances the fire resistance of the material.
Smart Images

Figure BDA0005043900320000071
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of polyethylene materials, in particular to a high-temperature resistant polyethylene material and a preparation method thereof. Background Art
[0002] Polyethylene materials are widely used in the manufacture of films, containers, pipes, monofilaments, wires and cables, daily necessities, etc. Polyethylene is odorless, non-toxic, feels like wax, has excellent low temperature resistance, and good chemical stability, but its flame retardant and high temperature resistance are poor, which limits its development. Therefore, how to avoid this phenomenon is the key to solving the problem. For example, patent CN116922892A discloses a high temperature resistant polyethylene bulletproof material and its preparation method. The invention only meets the 53 PU 100m bulletproof performance requirements through a lamination and lamination process, and enables the material to maintain good interlayer bonding at a high temperature of 100°C, but its flame retardant effect is not improved. Summary of the invention
[0003] 1. Technical issues to be resolved
[0004] In view of the deficiencies of the prior art, the present invention provides a high temperature resistant polyethylene material and a preparation method thereof, which has good flame retardancy and high temperature resistance.
[0005] (II) Technical solution
[0006] To achieve the above objectives, the present invention provides the following technical solution: a high temperature resistant polyethylene material, comprising the following components by weight: 80-100 parts by weight of polyethylene resin, 6-12 parts by weight of triazine-based flame retardant, 3-5 parts by weight of calcium carbonate, and 1-2 parts by weight of antioxidant 1076.
[0007] Preferably, the method of the triazine-based flame retardant is:
[0008] (1) adding tetrahydrofuran solvent and aniline to a reactor, cooling at -78°C to -80°C for 10-15 minutes, then continuously adding n-butyl lithium to the reactor, reacting at -75°C to -79°C for 5-8 hours, and obtaining lithium aniline after completion;
[0009] (2) Add lithium aniline and trichloronitrile to N,N-dimethylformamide solvent, stir and dissolve, continue to add triethylamine catalyst, react at 85-110° C. for 6-10 hours, and then distill under reduced pressure, filter, wash and dry to obtain intermediate 1;
[0010] (3) ultrasonically dispersing nano-alumina into a mixed solution of anhydrous ethanol and deionized water, mixing evenly, adding γ-aminopropyltriethoxysilane, reacting at 75-80° C. for 10-14 h, centrifuging, washing, and drying to obtain amino-alumina;
[0011] (4) Add the amino aluminum oxide and the intermediate 1 into N,N-dimethylformamide solvent, stir evenly, then add pyridine catalyst thereto, react at 85-100° C. for 5-8 hours, and then perform rotary distillation, wash and dry to obtain a triazine-based flame retardant.
[0012] Preferably, the mass ratio of aniline to n-butyl lithium in (1) is 1:1.1-1.3.
[0013] Preferably, the mass ratio of lithium aniline, trichloronitrile and triethylamine catalyst in (2) is 0.8-1.2:1:0.01-0.03.
[0014] Preferably, the mass ratio of nano-alumina to γ-aminopropyltriethoxysilane in (3) is 1:2.1-4.6.
[0015] Preferably, the mass ratio of the amino aluminum oxide, the intermediate 1, and the pyridine catalyst in (4) is 1.3-1.5:1:0.02-0.04.
[0016] Preferably, the preparation method of the high temperature resistant polyethylene material is: polyethylene resin, triazine-based flame retardant, calcium carbonate, and antioxidant 1076 are sequentially added into an extruder for melt extrusion, and the temperatures from the extruder die to the die head are 140°C, 150°C, 175°C, 190°C, 190°C, 195°C, 195°C, and 185°C respectively, and granulation is performed to obtain the high temperature resistant polyethylene material.
[0017] (III) Beneficial technical effects
[0018] The invention obtains the high temperature resistant polyethylene material by sequentially adding polyethylene resin, triazine-based flame retardant, calcium carbonate and antioxidant 1076 into an extruder for melt extrusion and granulation.
[0019] Aniline and n-butyl lithium are reacted to obtain lithium aniline, and nitrogen-hydrogen bonds in lithium aniline and chlorine in trichloronitrile are subjected to substitution reaction to obtain intermediate 1, and nano-alumina and γ-aminopropyltriethoxysilane are reacted to obtain amino alumina, and amino groups in the amino alumina and chlorine in intermediate 1 are subjected to substitution reaction to obtain a triazine-based flame retardant.
[0020] The triazine group in the triazine-based flame retardant has good high temperature resistance. The phosphorus element will decompose into phosphoric acid, metaphosphoric acid and even polymetaphosphoric acid when heated. These acidic substances can promote the dehydration of polymer materials and form carbonized products, thereby achieving a flame retardant effect. The nitrogen element decomposes at high temperatures to produce non-flammable gases such as ammonia and nitrogen. These gases dilute the oxygen and combustible gas concentrations in the air, reduce the combustion rate, and achieve a flame retardant effect. The nano-alumina therein can promote the formation of a solid carbonized layer on the surface of the polymer at high temperatures. This carbon layer has a low thermal conductivity and can effectively isolate external heat and oxygen from entering the underlying material, thereby achieving a flame retardant effect. At the same time, the nano-alumina itself also has good high temperature resistance. DETAILED DESCRIPTION
[0021] Example 1
[0022] (1) adding tetrahydrofuran solvent and aniline to a reactor, cooling at -78°C for 10 minutes, and then continuously adding n-butyl lithium to the reactor, wherein the mass ratio of aniline to n-butyl lithium is 1:1.1, reacting at -75°C for 5 hours, and obtaining lithium aniline after completion;
[0023] (2) Add lithium aniline and trichloronitrile to N,N-dimethylformamide solvent, stir to dissolve, and continue to add triethylamine catalyst, wherein the mass ratio of lithium aniline, trichloronitrile and triethylamine catalyst is 0.8:1:0.01, react at 85° C. for 6 hours, and then distill under reduced pressure, filter, wash and dry to obtain intermediate 1;
[0024] (3) ultrasonically dispersing nano-alumina into a mixed solution of anhydrous ethanol and deionized water, mixing evenly, adding γ-aminopropyltriethoxysilane, wherein the mass ratio of nano-alumina to γ-aminopropyltriethoxysilane is 1:2.1, reacting at 75° C. for 10 h, centrifuging, washing, and drying after the reaction to obtain amino-alumina;
[0025] (4) adding ammoniated aluminum oxide and intermediate 1 to N,N-dimethylformamide solvent, stirring evenly, and then adding pyridine catalyst thereto, wherein the mass ratio of ammoniated aluminum oxide, intermediate 1, and pyridine catalyst is 1.3:1:0.02, reacting at 85° C. for 5 h, and then rotary distilling, washing, and drying to obtain a triazine-based flame retardant;
[0026] (5) 80 parts by weight of polyethylene resin, 6 parts by weight of triazine-based flame retardant, 3 parts by weight of calcium carbonate and 1 part by weight of antioxidant 1076 are sequentially added into an extruder for melt extrusion. The temperatures from the extruder die to the die head are 140°C, 150°C, 175°C, 190°C, 190°C, 195°C, 195°C and 185°C respectively. Granulation is performed to obtain a high temperature resistant polyethylene material.
[0027] Example 2
[0028] (1) adding tetrahydrofuran solvent and aniline to a reactor, cooling at -80°C for 15 minutes, and then continuously adding n-butyl lithium to the reactor, wherein the mass ratio of aniline to n-butyl lithium is 1:1.3, reacting at -79°C for 8 hours, and obtaining lithium aniline after completion;
[0029] (2) Add lithium aniline and trichloronitrile to N,N-dimethylformamide solvent, stir to dissolve, and continue to add triethylamine catalyst, wherein the mass ratio of lithium aniline, trichloronitrile and triethylamine catalyst is 1.2:1:0.03, react at 110° C. for 10 h, and then distill under reduced pressure, filter, wash and dry to obtain intermediate 1;
[0030] (3) ultrasonically dispersing nano-alumina into a mixed solution of anhydrous ethanol and deionized water, mixing evenly, adding γ-aminopropyltriethoxysilane, wherein the mass ratio of nano-alumina to γ-aminopropyltriethoxysilane is 1:4.6, reacting at 80° C. for 14 h, centrifuging, washing, and drying after the reaction to obtain amino-alumina;
[0031] (4) adding the aminated aluminum oxide and the intermediate 1 to an N,N-dimethylformamide solvent, stirring evenly, and then adding a pyridine catalyst thereto, wherein the mass ratio of the aminated aluminum oxide, the intermediate 1, and the pyridine catalyst is 1.5:1:0.04, reacting at 100° C. for 8 hours, and then rotary distilling, washing, and drying to obtain a triazine-based flame retardant;
[0032] (5) 100 parts by weight of polyethylene resin, 12 parts by weight of triazine-based flame retardant, 5 parts by weight of calcium carbonate and 2 parts by weight of antioxidant 1076 are sequentially added into an extruder for melt extrusion. The temperatures from the die to the head of the extruder are 140°C, 150°C, 175°C, 190°C, 190°C, 195°C, 195°C and 185°C respectively. Granulation is performed to obtain a high temperature resistant polyethylene material.
[0033] Example 3
[0034] (1) adding tetrahydrofuran solvent and aniline to a reactor, cooling at -79°C for 12.5 minutes, and then continuously adding n-butyl lithium to the reactor, wherein the mass ratio of aniline to n-butyl lithium is 1:1.2, reacting at -76°C for 6.5 hours, and obtaining lithium aniline after completion;
[0035] (2) Add lithium aniline and trichloronitrile to N,N-dimethylformamide solvent, stir to dissolve, and continue to add triethylamine catalyst, wherein the mass ratio of lithium aniline, trichloronitrile and triethylamine catalyst is 1.0:1:0.023, react at 97° C. for 8 h, and then distill under reduced pressure, filter, wash and dry to obtain intermediate 1;
[0036] (3) ultrasonically dispersing nano-alumina into a mixed solution of anhydrous ethanol and deionized water, mixing well, adding γ-aminopropyltriethoxysilane, wherein the mass ratio of nano-alumina to γ-aminopropyltriethoxysilane is 1:2.35, reacting at 77° C. for 12 h, centrifuging, washing, and drying after the reaction to obtain amino-alumina;
[0037] (4) adding ammoniated aluminum oxide and intermediate 1 to N,N-dimethylformamide solvent, stirring evenly, and then adding pyridine catalyst thereto, wherein the mass ratio of ammoniated aluminum oxide, intermediate 1, and pyridine catalyst is 1.4:1:0.03, reacting at 92° C. for 6.5 hours, and then rotary distilling, washing, and drying to obtain a triazine-based flame retardant;
[0038] (5) 90 parts by weight of polyethylene resin, 9 parts by weight of triazine-based flame retardant, 4 parts by weight of calcium carbonate and 1.5 parts by weight of antioxidant 1076 are sequentially added into an extruder for melt extrusion. The temperatures from the extruder die to the die head are 140°C, 150°C, 175°C, 190°C, 190°C, 195°C, 195°C and 185°C respectively. Granulation is performed to obtain a high temperature resistant polyethylene material.
[0039] Example 4
[0040] (1) adding tetrahydrofuran solvent and aniline to a reactor, cooling at -78°C for 10 minutes, and then continuously adding n-butyl lithium to the reactor, wherein the mass ratio of aniline to n-butyl lithium is 1:1.1, reacting at -75°C for 5 hours, and obtaining lithium aniline after completion;
[0041] (2) Add lithium aniline and trichloronitrile to N,N-dimethylformamide solvent, stir to dissolve, and continue to add triethylamine catalyst, wherein the mass ratio of lithium aniline, trichloronitrile and triethylamine catalyst is 0.8:1:0.01, react at 85° C. for 6 hours, and then distill under reduced pressure, filter, wash and dry to obtain intermediate 1;
[0042] (3) ultrasonically dispersing nano-alumina into a mixed solution of anhydrous ethanol and deionized water, mixing evenly, adding γ-aminopropyltriethoxysilane, wherein the mass ratio of nano-alumina to γ-aminopropyltriethoxysilane is 1:4.6, reacting at 80° C. for 14 h, centrifuging, washing, and drying after the reaction to obtain amino-alumina;
[0043] (4) adding the aminated aluminum oxide and the intermediate 1 to an N,N-dimethylformamide solvent, stirring evenly, and then adding a pyridine catalyst thereto, wherein the mass ratio of the aminated aluminum oxide, the intermediate 1, and the pyridine catalyst is 1.5:1:0.04, reacting at 100° C. for 8 hours, and then rotary distilling, washing, and drying to obtain a triazine-based flame retardant;
[0044] (5) 90 parts by weight of polyethylene resin, 9 parts by weight of triazine-based flame retardant, 4 parts by weight of calcium carbonate and 1.5 parts by weight of antioxidant 1076 are sequentially added into an extruder for melt extrusion. The temperatures from the extruder die to the die head are 140°C, 150°C, 175°C, 190°C, 190°C, 195°C, 195°C and 185°C respectively. Granulation is performed to obtain a high temperature resistant polyethylene material.
[0045] Comparative Example 1
[0046] Compared with Example 4, this comparative example is characterized in that no triazine-based flame retardant is added.
[0047] The thermal properties of the high temperature resistant polyethylene material were tested by a thermogravimetric analyzer in a nitrogen atmosphere, with a heating rate of 25°C / min and a maximum temperature of 800°C. The limiting oxygen index of the material was tested using an oxygen index meter, and the combustion grade of the material was tested using a horizontal vertical combustion instrument. The test results are shown in Table 1.
[0048] Table 1: High temperature resistance test and flame retardancy test.
[0049]
[0050] It can be seen from Table 1 that Examples 1-4 of the present invention have better flame retardancy than Comparative Example 1, and the temperatures of 20% and 50% mass loss in Comparative Example 1 are lower than those in Examples 1-4, indicating that the high temperature resistant polyethylene material of the present invention has better high temperature resistance effect.
[0051] The preferred embodiments of the present invention disclosed above are only used to help illustrate the present invention. The preferred embodiments do not describe all the details in detail, nor do they limit the invention to the specific implementation methods described. Obviously, many modifications and changes can be made according to the content of this specification. This specification selects and specifically describes these embodiments in order to better explain the principles and practical applications of the present invention, so that those skilled in the art can understand and use the present invention well. The present invention is limited only by the claims and their full scope and equivalents.
Claims
1. A high temperature resistant polyethylene material, It is characterized in that The invention comprises the following components by weight: 80-100 parts by weight of polyethylene resin, 6-12 parts by weight of triazine-based flame retardant, 3-5 parts by weight of calcium carbonate and 1-2 parts by weight of antioxidant 1076.
2. The high temperature resistant polyethylene material according to claim 1, It is characterized in that The method of the triazine-based flame retardant is: (1) adding tetrahydrofuran solvent and aniline to a reactor, cooling at -78°C to -80°C for 10-15 minutes, then continuously adding n-butyl lithium to the reactor, reacting at -75°C to -79°C for 5-8 hours, and obtaining lithium aniline after completion; (2) Add lithium aniline and trichloronitrile to N,N-dimethylformamide solvent, stir and dissolve, continue to add triethylamine catalyst, react at 85-110° C. for 6-10 hours, and then distill under reduced pressure, filter, wash and dry to obtain intermediate 1; (3) ultrasonically dispersing nano-alumina into a mixed solution of anhydrous ethanol and deionized water, mixing evenly, adding γ-aminopropyltriethoxysilane, reacting at 75-80° C. for 10-14 h, centrifuging, washing, and drying to obtain amino-alumina; (4) Add the amino aluminum oxide and the intermediate 1 into N,N-dimethylformamide solvent, stir evenly, then add pyridine catalyst thereto, react at 85-100° C. for 5-8 hours, and then perform rotary distillation, wash and dry to obtain a triazine-based flame retardant.
3. The high temperature resistant polyethylene material according to claim 1, It is characterized in that The mass ratio of aniline to n-butyl lithium in (1) is 1:1.1-1.
3.
4. The high temperature resistant polyethylene material according to claim 1, It is characterized in that The mass ratio of lithium aniline, trichloronitrile and triethylamine catalyst in (2) is 0.8-1.2:1:0.01-0.
03.
5. The high temperature resistant polyethylene material according to claim 1, It is characterized in that The mass ratio of nano-alumina to γ-aminopropyltriethoxysilane in (3) is 1:2.1-4.
6.
6. The high temperature resistant polyethylene material according to claim 1, It is characterized in that The mass ratio of the amino aluminum oxide, the intermediate 1, and the pyridine catalyst in (4) is 1.3-1.5:1:0.02-0.
04.
7. A method for preparing the high temperature resistant polyethylene material according to any one of claims 1 to 6, It is characterized in that The preparation method of the high temperature resistant polyethylene material is: polyethylene resin, triazine-based flame retardant, calcium carbonate, and antioxidant 1076 are sequentially added into an extruder for melt extrusion, the temperature from the extruder die to the die head is sequentially 140°C, 150°C, 175°C, 190°C, 190°C, 195°C, 195°C, and 185°C, granulation is performed to obtain the high temperature resistant polyethylene material.