Modified polyvinyl alcohol water-soluble film with redeposition resistance and preparation method of modified polyvinyl alcohol water-soluble film

By chemical crosslinking in polyvinyl alcohol water-soluble film, the cross-linked network structure is formed, and the performance and single function of polyvinyl alcohol water-soluble film in humid environments is solved, and the resistance to redeposition and color-proof performance is improved. , suitable for diversified and high-performance applications.

CN119019798APending Publication Date: 2024-11-26GUANGZHOU FANDAO NETWORK TECH CO LTD
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
CN202411179649.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-27
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

Polyvinyl alcohol water-soluble films are prone to absorb water in humid environments, resulting in degradation of performance, and have a single function, which cannot meet the requirements of high gas barrier properties and mechanical properties, and lack the anti-redeposition function.

Method used

By chemically reacting the hydroxyl groups in the PVA chain with compounds containing two or more functional groups, a crosslinked network structure is formed, which reduces hydrophilic groups, enhances the chemical crosslinked structure, and improves the film's anti-redeposition and anti-color properties.

Benefits of technology

It effectively reduces the solubility of the membrane in water, improves the resistance to redeposition and color-proof properties, and makes the membrane more diversified and functional in practical applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119019798A_ABST
    Figure CN119019798A_ABST
Patent Text Reader

Abstract

The invention provides a modified polyvinyl alcohol water-soluble film with redeposition resistance and a preparation method of the modified polyvinyl alcohol water-soluble film. The modified polyvinyl alcohol water-soluble film composition with redeposition resistance comprises the following components in percentage by weight: 5-18% of polyvinyl alcohol; 0.5%-2.5% of a surfactant; 3%-11% of a plasticizer; 0.1%-2.5% of a release agent; 1%-10% of a cross-linking agent; 0.05%-0.2% of a defoaming agent; 0.005% of a bitter agent; and the balance water. According to the invention, hydrophilic hydroxyl groups on a PVA molecular chain are reduced through a chemical reaction, and a formed chemical crosslinking structure can prevent the membrane from being dissolved in water, so that the swelling degree of the PVA membrane in water is reduced. And the problem of single function of the PVA water-soluble film is solved, so that the PVA water-soluble film has redeposition resistance and cross color resistance, and is more diversified and functionalized in practical application.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of water-soluble high molecular polymers, and in particular to a modified polyvinyl alcohol water-soluble film with anti-redeposition properties and a preparation method thereof. Background Art

[0002] Polyvinyl alcohol (PVA) is a water-soluble high molecular polymer obtained by the alcoholysis of vinyl acetate polymerization. Using polyvinyl alcohol resin to prepare films is a new direction in the application of polyvinyl alcohol resin. The films prepared from PVA have excellent oxygen barrier properties, solvent resistance, antistatic properties, high mechanical properties, etc. In addition, they are water-soluble and biodegradable.

[0003] In recent years, water-soluble polyvinyl alcohol film, as a novel and green packaging material that is biodegradable, safe and convenient to use, has been widely used in the packaging of various products, such as pesticides, detergents, water treatment agents, etc. The water-soluble film prepared by polyvinyl alcohol is used to seal and package a unit amount of laundry beads, pesticides, dyes and other products. When used, the packaged products can be directly put into water in the form of packaging, and the packaged contents are dissolved in water through the film and dispersed in water. The advantages of this unit quantitative packaging are that it does not come into direct contact with the contents when used, the packaged contents are quantitative, and the measurement procedures are omitted when used; and the packaging can be dissolved in water, which also reduces garbage disposal.

[0004] However, polyvinyl alcohol water-soluble film has some defects, mainly manifested in that the PVA water-soluble film without special treatment is easy to absorb water in a humid environment, resulting in a decrease in performance. This is because the PVA structure contains a large number of hydrophilic groups (-OH), which causes the film to easily absorb water and swell, thereby affecting its gas barrier properties and mechanical properties. This limits its application in situations where high gas barrier properties and mechanical properties are required.

[0005] In addition, currently PVA water-soluble film can only play the role of packaging isolation, with relatively simple functionality, and cannot give diversified applications to packaging materials.

[0006] At present, there are few reports on the modification function of the polyvinyl alcohol water-soluble film composition with anti-redeposition, so the research on its anti-redeposition function is of great significance. Summary of the invention

[0007] In view of the shortcomings of the above-mentioned prior art, the purpose of the present invention is to provide a modified polyvinyl alcohol water-soluble film with anti-redeposition properties. The film is matched with a selected special polyvinyl alcohol to make the hydroxyl groups in the PVA chain more active, and chemically react with compounds containing two or more functional groups such as carboxyl groups, aldehyde groups, isocyanate groups, etc., so that a cross-linked network structure is formed between the PVA molecular chains; this method not only reduces the hydrophilic hydroxyl groups on the PVA molecular chains through chemical reactions, but also the formed chemical cross-linked structure can prevent the film from dissolving in water and reduce the swelling degree of the PVA film in water; and it solves the problem of single functionalization of the PVA water-soluble film, so that it has anti-redeposition properties and anti-color transfer properties, and is more diversified and functional in practical applications.

[0008] The present invention is achieved through the following technical solutions.

[0009] The present invention discloses a modified polyvinyl alcohol water-soluble film with anti-redeposition properties, which comprises the following components in terms of weight percentage:

[0010]

[0011] Wherein, the polyvinyl alcohol is selected from one or more of PVA1788, PVA1792, and PVA2588.

[0012] The plasticizer is selected from one or more of propylene glycol, sorbitol, glycerol, polyethylene glycol, and ethylene glycol.

[0013] The surfactant is selected from sodium lauryl sulfate.

[0014] The release agent is selected from one or more of dimethyl silicone oil, Tween-20, and Tween-80.

[0015] The cross-linking agent is selected from compounds containing two or more functional groups such as carboxyl groups, aldehyde groups, isocyanate groups, etc., and is selected from glutaraldehyde, toluene diisocyanate, urea, (3-chloro-2-hydroxypropyl) trimethylammonium chloride, glycolic acid, lactic acid, malic acid, citric acid, tartaric acid, mandelic acid, gluconic acid, mucic acid, oxalic acid, boric acid, and mixtures thereof.

[0016] The defoaming agent is selected from one or more of the defoaming agent 740A and the defoaming agent 444.

[0017] Unless otherwise specified, the above-mentioned raw materials are conventional commercially available products.

[0018] Furthermore, the cross-linking agent is selected from one or more of urea, citric acid, glutaraldehyde, oxalic acid, boric acid, (3-chloro-2-hydroxypropyl)trimethylammonium chloride and mixtures thereof.

[0019] Furthermore, the cross-linking agent is selected from one or more of citric acid, glutaraldehyde, and (3-chloro-2-hydroxypropyl)trimethylammonium chloride.

[0020] Furthermore, the modified polyvinyl alcohol water-soluble film composition with anti-redeposition properties of the present invention comprises the following formula components in percentage by weight:

[0021] Phase A surfactant, release agent: 0.5-2% sodium dodecyl sulfate, 0.2-0.5% Tween-80;

[0022] Phase B polyvinyl alcohol: 13-17.5% PVA1788, 0-3% PVA2588, 0-3% PVA1792;

[0023] Phase C plasticizer: 3-5% glycerol, 0-8% propylene glycol;

[0024] Phase D crosslinking agent, defoaming agent, bittering agent: 0.5% (3-chloro-2-hydroxypropyl) trimethylammonium chloride, 0-2% citric acid, 0-1% glutaraldehyde, 0.1% defoaming agent, 0.005% bittering agent.

[0025] Furthermore, the modified polyvinyl alcohol water-soluble film composition with anti-redeposition of the present invention comprises the following formula components in percentage by weight:

[0026] Phase A surfactant, release agent: 1.5% sodium dodecyl sulfate, 0.3% Tween-80;

[0027] Phase B polyvinyl alcohol: 15% PVA1788, 3% PVA2588;

[0028] Plasticizer of phase C: 3% glycerol;

[0029] Phase D crosslinking agent, defoaming agent, bittering agent: 0.5% (3-chloro-2-hydroxypropyl) trimethylammonium chloride, 2% citric acid, 1% glutaraldehyde, 0.1% defoaming agent, 0.005% bittering agent.

[0030] The present invention also provides a method for preparing a modified polyvinyl alcohol water-soluble film composition having anti-redeposition properties, comprising the following steps:

[0031] Step S1: mixing water, the surfactant, and the release agent to prepare a first mixture;

[0032] Step S2: heating the first mixed material and the polyvinyl alcohol to 90° C. to disperse and dissolve them uniformly, thereby preparing a second mixed material;

[0033] Step S3: uniformly mixing the second mixed material and the plasticizer to prepare a third mixed material;

[0034] Step S4: the third mixed material, the cross-linking agent and the bittering agent are mixed at 90° C. for 1 hour until they are uniform, to prepare a fourth mixed material, a defoaming agent is added, and the mixture is allowed to stand for 24 hours after defoaming to obtain a polyvinyl alcohol aqueous solution masterbatch;

[0035] Step S5: Set the parameters of the flat plate coating machine to coating speed: 6 mm / s, coating thickness: 80 um, temperature 90° C., and drying time 20 min.

[0036] The polyvinyl alcohol aqueous solution masterbatch was slowly and evenly drooled on the glass plate of the flat coater, the solution was flatly pushed by a coating scraper, dried at a set temperature, and peeled off from the glass plate to obtain a PVA film with a thickness of 80 um.

[0037] The beneficial effects of the present invention are:

[0038] 1) The membrane of the present invention is matched with a selected special polyvinyl alcohol, and the hydroxyl groups in the PVA chain are relatively active, and chemically react with compounds containing two or more functional groups such as carboxyl groups, aldehyde groups, isocyanate groups, etc., so that a cross-linked network structure is formed between the PVA molecular chains;

[0039] 2) The method of the present invention not only reduces the hydrophilic hydroxyl groups on the PVA molecular chain through chemical reaction, but also forms a chemical cross-linking structure that can prevent the film from dissolving in water and reduce the swelling degree of the PVA film in water; and solves the problem of single functionalization of the PVA water-soluble film, so that it has anti-redeposition performance and anti-color transfer performance, and is more diversified and functionalized in practical applications. BRIEF DESCRIPTION OF THE DRAWINGS

[0040] Figure 1 Shown is the modified polyvinyl alcohol water-soluble film with anti-redeposition properties according to Example 2 of the present invention.

[0041] Figure 2 Shown is the anti-color bleed performance graph of the efficacy test example. DETAILED DESCRIPTION

[0042] The present invention provides a modified polyvinyl alcohol water-soluble film with anti-redeposition properties and a preparation method thereof. The specific raw material combinations and proportions include but are not limited to the embodiments of the present invention.

[0043] The invention provides a ratio and preparation process of a modified polyvinyl alcohol water-soluble film with anti-redeposition properties.

[0044] The main production methods of water-soluble polyvinyl alcohol film are solution casting and melt extrusion. The method adopted by the present invention is: solution casting, which is to dissolve polyvinyl alcohol in water to make a dilute solution. In order to improve its processing performance, some additives such as plasticizers, crosslinking agents, release agents, etc. are generally added. Then, it is cast from the gap on a flat plate and heated and dried to form a film.

[0045] Water-soluble films are made water-soluble by using polyvinyl alcohol, which is extremely sensitive to water. There are a large number of water-soluble hydroxyl groups in polyvinyl alcohol. Polyvinyl alcohol is generally obtained by hydrolysis of polyvinyl acetate, and its solubility is changed by controlling the hydrolysis of polyvinyl acetate.

[0046] The water solubility of polyvinyl alcohol film at different temperatures is related to the alcoholysis degree of polyvinyl alcohol. PVA with an alcoholysis degree in the range of 75% to 88% has the best water solubility and can be dissolved in cold water at 0 to 30°C; PVA with an alcoholysis degree in the range of 95% to 97% has poor water solubility and can be dissolved in warm water at 40 to 60°C; and PVA with an alcoholysis degree of more than 99% (the so-called completely alcoholysed PVA) has very poor water solubility and can only be dissolved in hot water above 70°C.

[0047] Therefore, the above-mentioned water-soluble PVA film is usually processed from a PVA resin with an alcoholysis degree of about 88%, while the preparation of a water-resistant PVA film generally requires the use of a completely alcoholysed PVA resin with an alcoholysis degree of more than 99% as a raw material.

[0048] The hydroxyl groups in the PVA chain are relatively active and can easily react chemically with compounds containing two or more functional groups such as carboxyl groups, aldehyde groups, isocyanate groups, etc., to form a cross-linked network structure between the PVA molecular chains. The chemical cross-linking method not only reduces the hydrophilic hydroxyl groups on the PVA molecular chain through chemical reactions, but also forms a chemical cross-linking structure that can prevent the film from dissolving in water and reduce the swelling degree of the PVA film in water.

[0049] By adding one or two of citric acid and cationic quaternary ammonium salt crosslinking agents into the polyvinyl alcohol masterbatch, the water-soluble film is modified so that its water resistance is significantly improved; moreover, it has anti-redeposition performance and anti-color transfer performance.

[0050] The modified polyvinyl alcohol water-soluble film composition with anti-redeposition properties and the preparation method thereof are further described in detail below in conjunction with specific examples. The raw materials used in the following examples are all commercially available products unless otherwise specified.

[0051] Examples 1-5

[0052] This embodiment provides a modified polyvinyl alcohol water-soluble film composition with anti-redeposition properties. The weight percentages of the components of the polyvinyl alcohol water-soluble film masterbatch are shown in Table 1 below.

[0053] The preparation method is as follows:

[0054] 1) Clean and disinfect the equipment and weighing tools and keep them ready for use;

[0055] 2) First, accurately weigh a certain amount of the raw material surfactant and release agent of phase A and dissolve them in a beaker;

[0056] 3) Place the beaker in a constant temperature water bath and stir and heat, weigh a certain amount of phase B polyvinyl alcohol, slowly add the polyvinyl alcohol into the beaker while stirring, and heat to 90° C. while stirring to allow the polyvinyl alcohol to fully swell and disperse evenly;

[0057] 4) Weigh a certain amount of C-phase plasticizer and slowly pour it into the beaker;

[0058] 5) Add phase D raw materials, stir at a constant temperature of 90°C for 1 hour to fully dissolve the polyvinyl alcohol until the solution is uniform and transparent, add defoamer, stir at this temperature for 30 minutes, evacuate, cool the material, and let it stand for 24 hours after the material is tested to be qualified;

[0059] 6) Set the parameters of the flat plate coater to coating speed: 6mm / s, coating thickness: 80um, temperature 90℃, and drying time 20min. Slowly and evenly pour the PVA solution onto the glass plate of the flat plate coater, push the solution flat with a coating scraper, dry it at the set temperature, and peel it off from the glass plate to obtain a PVA film with a thickness of 80um.

[0060] Comparative Example 1-2

[0061] This comparative example provides a modified polyvinyl alcohol water-soluble film composition with anti-redeposition properties. The weight percentages of the components of the polyvinyl alcohol water-soluble film masterbatch are shown in Table 1 below.

[0062] The preparation method is as follows:

[0063] 1) Clean and disinfect the equipment and weighing tools and keep them ready for use;

[0064] 2) First, accurately weigh a certain amount of raw surfactant of phase A and dissolve it in a beaker;

[0065] 3) Place the beaker in a constant temperature water bath and stir and heat, weigh a certain amount of phase B polyvinyl alcohol, slowly add the polyvinyl alcohol into the beaker while stirring, and heat to 90° C. while stirring to allow the polyvinyl alcohol to fully swell and disperse evenly;

[0066] 4) Weigh a certain amount of C-phase plasticizer and slowly pour it into the beaker;

[0067] 5) Add phase D raw materials, stir at a constant temperature of 90°C for 1 hour to fully dissolve the polyvinyl alcohol until the solution is uniform and transparent, add defoamer, stir at this temperature for 30 minutes, evacuate, cool the material, and let it stand for 24 hours after the material is tested to be qualified;

[0068] 6) Set the parameters of the flat plate coater to coating speed: 6mm / s, coating thickness: 80um, temperature 90℃, and drying time 20min. Slowly and evenly pour the PVA solution onto the glass plate of the flat plate coater, push the solution flat with a coating scraper, dry it at the set temperature, and peel it off from the glass plate to obtain a PVA film with a thickness of 80um.

[0069] Table 1 Polyvinyl alcohol water-soluble film masterbatch formula

[0070]

[0071] Example 2: Modified polyvinyl alcohol water-soluble film with anti-redeposition properties Figure 1 shown.

[0072] The following are the contents of the efficacy test examples.

[0073] Polyvinyl alcohol water-soluble film performance test

[0074] ①Tensile test:

[0075] Refer to "GB / T 1040.3-2006 Determination of tensile properties of plastics Part 3: Test conditions for films and sheets".

[0076] Preparation before the experiment: electric tensile testing machine, scissors, samples, specimen size template, etc.

[0077] Sampling: Some properties of water-soluble films may vary with different directions within the film plane (anisotropy). In this case, two groups of samples should be prepared with their main axes parallel and perpendicular to the film orientation direction respectively (i.e., transverse sampling and longitudinal sampling). After sampling, any samples with obvious defects on the cut edges should be removed.

[0078] Experimental steps: The samples were placed at a temperature of 25°C and a humidity of 50% RH for 24 hours before testing.

[0079] Cut at least 10 15cm×1.5cm long strips (i.e. Type 2 specimens), measure the thickness, set the gauge length to 50mm, and the tensile speed to 200mm / min. After breaking, record the elongation at break and tensile strength, and take the average value. (Some film materials have a high elongation when they break, which may exceed the travel limit of the testing machine. In this case, the initial distance between the clamps can be reduced to 50mm) (Type 2 specimens are preferred for testing).

[0080] ② Film water solubility: 1000mL of water, magnetic stirring vortex about 30mm, 25℃ water temperature, water-soluble film size 40mm*40mm.

[0081] ③ Anti-redeposition performance: Refer to GBT 13174-2021 Determination of detergency and cyclic washing performance of detergents for clothing. In a decontamination test machine, at the specified temperature and washing time, use water of a certain hardness to prepare a detergent solution of a certain concentration, add a certain amount of dirty liquid, and wash a certain number of white cotton cloth pieces.

[0082] After taking out and drying, repeat the washing process for a specified number of times (usually more than 20 times), and evaluate the appearance (roughness) and softness of the washed white cotton cloth by sensory evaluation, and measure the deposited ash (burning method) and whiteness retention (calculated from the whiteness before and after washing). Compare these criteria to evaluate the anti-stain redeposition ability of the detergent.

[0083] ④Anti-color cross-talk performance:

[0084] Add 300g of hard water (250mg / kg) into a bucket, accurately weigh 0.50g of direct dye (pre-configured 0.1% aqueous solution), add 10g of standard laundry detergent (in the test experiment, add 0.3g of the corresponding water-soluble film), stir to dissolve, put in 3 pieces of 5cm×5cm JB00 standard white cloth to soak, wash at 25℃, 120rpm for 5min, rinse with tap water once, dry in a constant temperature drying oven at 48℃ for 30min, take pictures and compare to record the anti-color bleeding effect.

[0085] The experimental results are shown in Table 2 and Figure 1 shown.

[0086] Table 2 Test result record

[0087]

[0088] Table 2 and Figure 1 The results show:

[0089] ① Examples 1-5 used crosslinking agents such as lemon, glutaraldehyde and (3-chloro-2-hydroxypropyl) trimethylammonium chloride. Compared with Comparative Examples 1-2, the transverse and longitudinal tensile strengths and tensile fracture rates of the examples were greater than those of the comparative examples, indicating that the tensile properties were significantly improved. The fundamental reason is that the addition of the crosslinking agent reduces the hydrophilic hydroxyl groups on the PVA molecular chain, forming a network structure and enhancing the tensile properties;

[0090] ② Examples 1-5 used crosslinking agents such as lemon, glutaraldehyde and (3-chloro-2-hydroxypropyl) trimethylammonium chloride. Compared with Comparative Examples 1-2, the whiteness ratio of the examples was greater than that of the comparative examples, indicating that the water-soluble film of the examples can reduce the probability of stains being deposited on the fabric again, showing excellent anti-redeposition; Figure 2 The dyeing condition of the embodiment is lower than that of the comparative example, indicating that the water-soluble film of the embodiment can reduce the adsorption of pigments onto the fabric, showing excellent anti-color transfer performance;

[0091] ③ Examples 1-5 used cross-linking agents such as lemon, glutaraldehyde and (3-chloro-2-hydroxypropyl) trimethylammonium chloride. Compared with Comparative Examples 1-2, the complete dissolution time of the examples in water was greater than that of the comparative examples, indicating that the cross-linking of the hydroxyl groups of the water-soluble film of the examples reduced the speed of contact dissolution of water molecules, thereby significantly improving the water resistance.

[0092] The above description is only a preferred embodiment of the present invention and does not limit the present invention in any form. Therefore, any simple modification, equivalent change and modification made to the above embodiment according to the technical essence of the present invention without departing from the technical solution of the present invention still fall within the scope of the technical solution of the present invention.

Claims

1. A modified polyvinyl alcohol water-soluble film having anti-redeposition properties, comprising the following components in weight percentage: The polyvinyl alcohol is selected from one or more of PVA1788, PVA1792, and PVA2588; The plasticizer is selected from one or more of propylene glycol, sorbitol, glycerol, polyethylene glycol, and ethylene glycol; The surfactant is selected from sodium lauryl sulfate; The release agent is selected from one or more of dimethyl silicone oil, Tween-20, and Tween-80; The cross-linking agent is selected from compounds containing two or more functional groups such as carboxyl groups, aldehyde groups, isocyanate groups, etc., and is selected from glutaraldehyde, toluene diisocyanate, urea, (3-chloro-2-hydroxypropyl) trimethylammonium chloride, glycolic acid, lactic acid, malic acid, citric acid, tartaric acid, mandelic acid, gluconic acid, mucic acid, oxalic acid, boric acid, and mixtures thereof; The defoaming agent is selected from one or more of the defoaming agent 740A and the defoaming agent 444.

2. The modified polyvinyl alcohol water-soluble film having anti-redeposition properties as claimed in claim 1, characterized in that: The cross-linking agent is selected from one or more of urea, citric acid, glutaraldehyde, oxalic acid, boric acid, (3-chloro-2-hydroxypropyl)trimethylammonium chloride and mixtures thereof.

3. The modified polyvinyl alcohol water-soluble film having anti-redeposition properties as claimed in claim 1, characterized in that: The formula contains the following weight percentage ingredients: Phase A surfactant, release agent: 0.5-2% sodium dodecyl sulfate, 0.2-0.5% Tween-80; Phase B polyvinyl alcohol: 13-17.5% PVA1788, 0-3% PVA2588, 0-3% PVA1792; Phase C plasticizer: 3-5% glycerol, 0-8% propylene glycol; Phase D crosslinking agent, defoaming agent, bittering agent: 0.5% (3-chloro-2-hydroxypropyl) trimethylammonium chloride, 0-2% citric acid, 0-1% glutaraldehyde, 0.1% defoaming agent, 0.005% bittering agent.

4. The modified polyvinyl alcohol water-soluble film having anti-redeposition properties as claimed in claim 3, characterized in that: The formula contains the following weight percentage ingredients: Phase A surfactant, release agent: 1.5% sodium dodecyl sulfate, 0.3% Tween-80; Phase B polyvinyl alcohol: 15% PVA1788, 3% PVA2588; Plasticizer of phase C: 3% glycerol; Phase D crosslinking agent, defoaming agent, bittering agent: 0.5% (3-chloro-2-hydroxypropyl) trimethylammonium chloride, 2% citric acid, 1% glutaraldehyde, 0.1% defoaming agent, 0.005% bittering agent.

5. The method for preparing the modified polyvinyl alcohol water-soluble film having anti-redeposition properties according to any one of claims 1 to 3, characterized in that: The steps include: Step S1: mixing water, the surfactant, and the release agent to prepare a first mixture; Step S2: heating the first mixed material and the polyvinyl alcohol to 90° C. to disperse and dissolve them uniformly, thereby preparing a second mixed material; Step S3: uniformly mixing the second mixed material and the plasticizer to prepare a third mixed material; Step S4: the third mixed material, the cross-linking agent and the bittering agent are mixed at 90° C. for 1 hour until they are uniform, to prepare a fourth mixed material, a defoaming agent is added, and the mixture is allowed to stand for 24 hours after defoaming to obtain a polyvinyl alcohol aqueous solution masterbatch; Step S5: coating with a flat plate coater.

6. The method for preparing the modified polyvinyl alcohol water-soluble film having anti-redeposition properties as claimed in claim 5, characterized in that: In step S5, the flat plate coating machine is set with the following parameters: coating speed: 6 mm / s, coating thickness: 80 um, temperature: 90° C., and drying time: 20 min.

7. The method for preparing the modified polyvinyl alcohol water-soluble film having anti-redeposition properties according to claim 5, characterized in that: Step S5 also includes: The polyvinyl alcohol aqueous solution masterbatch was slowly and evenly drooled on the glass plate of the flat coater, the solution was flatly pushed by a coating scraper, dried at a set temperature, and peeled off from the glass plate to obtain a PVA film with a thickness of 80 um.

Citation Information

Patent Citations

  • Preparation method of gelatin / poli vinyl alcohol (PVA) composite films crosslinked with glutaraldehyde solution

    CN102585265A

  • Manufacturing method of water-resistant polyvinyl alcohol film

    CN103059486A

  • Middle-temperature water-soluble film, preparing method and refined filtration equipment

    CN106589723A

  • Normal-temperature-used water-soluble film and preparation method thereof, and fine filtration device

    CN106589724A

  • Water-soluble bag and application thereof

    CN108504010A