Interface-engaged carbon fiber composite material as well as preparation method and application thereof

By constructing a multi-dimensional interface enhancement phase on the surface of carbon fiber and performing surface functional modification, chemical bonding is formed, the problem of interface failure of carbon fiber composite materials in deep-sea environment is solved, and its interface performance and high-pressure resistance are significantly improved to meet the deep-sea environment. long-lived service needs.

CN119019809APending Publication Date: 2024-11-26NINGBO INST OF MATERIALS TECH & ENG CHINESE ACAD OF SCI
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202310588786.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-23
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

The interface failure of carbon fiber composite materials in deep-sea environments due to high pressure, resulting in reduced macroscopic performance of the coating, and the interface between unmodified fibers and resins has stress concentration and crack propagation, affecting its service life in deep-sea environments.

Method used

The chemical vapor deposition method is used to construct multi-dimensional interface reinforced phases such as carbon nanospheres, carbon nanowires, and carbon nanosheets on the surface of carbon fibers, and the amino groups are introduced to form chemical bonds with the resin through surface functionalization modification to achieve interface meshing and chemical bonding. synergistic enhancement.

Benefits of technology

It significantly improves the interface shear strength and erosion resistance of carbon fiber composite materials, reduces the risks of interface cracking and crack propagation, and keeps it without failure for 240 hours under the high pressure of 5,000 meters of deep sea, meeting the long-life service requirements of the deep sea environment. .

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119019809A_ABST
    Figure CN119019809A_ABST
Patent Text Reader

Abstract

The invention discloses an interface-engaged carbon fiber composite material as well as a preparation method and application thereof. The preparation method comprises the following steps: constructing an interface reinforced phase on the surface of carbon fiber in situ by adopting a chemical vapor deposition method to obtain interface reinforced phase carbon fiber; performing surface functional modification on the interface reinforced phase carbon fibers to obtain modified carbon fibers; and uniformly mixing the modified carbon fiber with resin, and curing to obtain the interface-engaged carbon fiber composite material. The method provided by the invention is suitable for improving the interface performance of the carbon fiber composite material, so that the mechanical property, the erosion resistance, the deep sea high pressure resistance, the radiation resistance and the like of the fiber reinforced composite material are improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of carbon fiber reinforced composite materials for deep sea environment service, and specifically relates to an interface meshing carbon fiber composite material and a preparation method and application thereof. Background Art

[0002] In deep sea environment, high pressure significantly increases the penetration rate of corrosive media, hydrostatic pressure accelerates the diffusion rate of water and other corrosive media in the coating, the saturated water absorption rate of the coating increases, and high hydrostatic pressure causes stress concentration and crack propagation at the interface between unmodified fiber and resin. The peeling failure of the interface greatly reduces the macroscopic properties of the coating. The corrosion products accumulate at the metal / coating interface, significantly reducing the wet adhesion of the coating and causing bubbling of the coating. In addition, the high pressure in the deep sea promotes the corrosion and wear of the coating. Carbon fiber and its composite materials have excellent mechanical properties, heat resistance, corrosion resistance, impact resistance and other properties and are widely used in aerospace, military, rail transportation and other fields. With my country's scientific exploration of the 10,000-meter deep sea and the future demand for deep-sea resource drilling, the service performance of deep-sea protective materials has been put forward higher requirements and new challenges. The interface failure problem of carbon fiber reinforced composite coatings in extreme deep-sea environments is a key scientific issue affecting its long-life safe service. With its excellent mechanical properties and chemical stability, carbon fiber reinforced composite materials have shown great application potential in the field of corrosion protection of metal materials in deep-sea environments. However, the surface of untreated carbon fiber is smooth and has few active functional groups, which makes carbon fiber composites prone to failure forms such as interface cracking and fiber pullout under the influence of multiple factors in extreme environments, and stress concentration is formed in the interface area of ​​carbon fiber composites, which greatly reduces the impact resistance of the composites and seriously affects the performance of carbon fiber. The interface failure problem has become a key scientific issue for carbon fiber composites in the marine environment. Therefore, constructing carbon fiber composites with synergistic enhancement of interface meshing and chemical bonding is an important topic in the current research on the interface of carbon fiber reinforced composites. The in-situ construction of multi-dimensional interface reinforcement phases of carbon nanospheres, carbon nanowires, and carbon nanosheets on the surface of carbon fibers by chemical vapor deposition can effectively make the stress evenly transferred and dispersed, and the interface gradient modulus can effectively play a role in strengthening and toughening. At present, most of the research can improve the interface performance of composite materials to a certain extent through simple surface modification or constructing an interface layer on the fiber surface through sizing agents. However, since a new interface is introduced at the interface and the strength and performance of the interface layer cause new problems such as failure of the interface layer under extreme marine environments, the improvement of its interface performance is limited. It is urgent to design a carbon fiber reinforced composite material with strong interface bonding to meet its excellent mechanical properties, erosion resistance, deep sea high pressure resistance, and radiation resistance requirements under extreme marine environments. Summary of the invention

[0003] The main purpose of the present invention is to provide an interface-engaged carbon fiber composite material and a preparation method and use thereof, so as to overcome the shortcomings of the prior art.

[0004] In order to achieve the above-mentioned invention object, the technical solution adopted by the present invention includes:

[0005] An embodiment of the present invention provides a method for preparing an interface-engaged carbon fiber composite material, which comprises:

[0006] The interface reinforcement phase is constructed in situ on the surface of the carbon fiber by chemical vapor deposition to obtain the interface reinforcement phase carbon fiber; wherein the interface reinforcement phase includes any one of carbon nanospheres, carbon nanowires, and carbon nanosheets, or a combination of two or more thereof;

[0007] Performing surface functional modification on the interface reinforcement phase carbon fiber to obtain modified carbon fiber;

[0008] And, the modified carbon fiber is evenly mixed with resin and cured to obtain an interface-engaged carbon fiber composite material.

[0009] The embodiment of the present invention also provides an interface-engaged carbon fiber composite material obtained by the aforementioned preparation method, wherein a mechanically engaged strong bonding interface is formed between the interface reinforcement phase in the carbon fiber composite material and the resin, and a chemically bonded strengthening structure is formed between the modified carbon fiber and the resin.

[0010] The embodiment of the present invention also provides the use of the aforementioned interface-engaged carbon fiber composite material in the protection of mechanical parts in a deep-sea high-pressure environment.

[0011] The embodiment of the present invention also provides a method for improving the interface performance of carbon fiber composite materials by using interface meshing reinforcement, which comprises:

[0012] The interface reinforcement phase is constructed in situ on the surface of the carbon fiber by chemical vapor deposition to obtain the interface reinforcement phase carbon fiber; wherein the interface reinforcement phase includes any one of carbon nanospheres, carbon nanowires, and carbon nanosheets, or a combination of two or more thereof;

[0013] Performing surface functional modification on the interface reinforcement phase carbon fiber to obtain modified carbon fiber;

[0014] Furthermore, the modified carbon fiber and the resin are uniformly mixed and cured, thereby improving the interface performance of the carbon fiber composite material.

[0015] Compared with the prior art, the present invention has the following beneficial effects:

[0016] (1) The interfacial meshing strengthening effect in the carbon fiber composite material of the present invention is achieved by in-situ construction of a multi-dimensional interfacial reinforcement phase of carbon nanospheres, carbon nanowires and carbon nanosheets on the surface of the carbon fiber, thereby forming a very strong interfacial meshing strengthening effect at the interface between the carbon fiber and the resin;

[0017] (2) The present invention forms a chemical bonding strengthening effect at the interface between the carbon fiber and the resin through surface modification, and introduces amino groups by chemically modifying the surface of the carbon fiber on which the interface reinforcement phase grows, so as to form a chemical bonding strengthening effect with the resin; at the same time, the interface meshing and chemical bonding synergistically enhance the interface performance between the carbon fiber and the resin, forming a multi-level gradient modulus interface strengthening effect, which can evenly transmit and disperse stress, and improve interface compatibility, interface shear strength and interface toughness matching;

[0018] (3) The synergistic effect of the interface meshing strengthening and chemical bonding strengthening of the carbon fiber composite material in the present invention significantly improves the macroscopic performance of the carbon fiber composite material, and its interface shear strength can reach up to 110MPa, and the erosion volume is reduced by 91.4%. When the interface between the carbon fiber and the resin is exposed to a high pressure of 5,000 meters in the simulated deep sea for 240 hours, the interface does not produce failure forms such as cracking and crack extension;

[0019] (4) The method provided by the present invention is suitable for improving the interface properties of carbon fiber composite materials, thereby improving the mechanical properties, erosion resistance, deep-sea high pressure resistance, radiation resistance and other properties of fiber-reinforced composite materials. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments recorded in the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0021] Figure 1 is a SEM image of the carbon fiber growing the interface reinforcement phase in Example 1 of the present invention;

[0022] Figure 2 This is a morphology diagram of the interface between carbon fiber and resin of the carbon fiber reinforced composite material in Example 1 of the present invention after being subjected to a simulated deep sea environment of 5000 meters for 240 hours;

[0023] Figure 3 is a morphology diagram of the interface between carbon fiber and resin of the carbon fiber reinforced composite material in Example 1 of the present invention after an erosion test;

[0024] Figure 4This is a morphology diagram of the interface between carbon fiber and resin of the carbon fiber reinforced composite material in Comparative Example 1 of the present invention after 240 hours in a simulated deep sea environment of 5000 meters;

[0025] Figure 5 is a morphology diagram of the interface between carbon fiber and resin of the carbon fiber reinforced composite material in Comparative Example 1 of the present invention after an erosion test;

[0026] Figure 6 This is a morphology diagram of the interface between carbon fiber and resin of the carbon fiber reinforced composite material in Comparative Example 2 of the present invention after 240 hours in a simulated deep sea environment of 5000 meters;

[0027] Figure 7 is a morphology diagram of the interface between carbon fiber and resin of the carbon fiber reinforced composite material in Comparative Example 2 of the present invention after an erosion test;

[0028] Figure 8 This is a morphology diagram of the interface between carbon fiber and resin of the carbon fiber reinforced composite material in Comparative Example 3 of the present invention after 240 hours in a simulated deep sea environment of 5000 meters;

[0029] Fig. 9 This is a morphology diagram of the interface between carbon fiber and resin of the carbon fiber reinforced composite material in Comparative Example 2 of the present invention after an erosion test. DETAILED DESCRIPTION

[0030] In view of the defects of the prior art, the inventor of this case has proposed the technical solution of the present invention after long-term research and extensive practice. The technical solution of the present invention will be described clearly and completely below. Obviously, the described embodiments are part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0031] Specifically, as one aspect of the technical solution of the present invention, a method for preparing an interface-engaged carbon fiber composite material includes:

[0032] The interface reinforcement phase is constructed in situ on the surface of the carbon fiber by chemical vapor deposition to obtain the interface reinforcement phase carbon fiber; wherein the interface reinforcement phase includes any one of carbon nanospheres, carbon nanowires, and carbon nanosheets, or a combination of two or more thereof;

[0033] Performing surface functional modification on the interface reinforcement phase carbon fiber to obtain modified carbon fiber;

[0034] And, the modified carbon fiber is evenly mixed with resin and cured to obtain an interface-engaged carbon fiber composite material.

[0035] In some preferred embodiments, the interface reinforcement phase is a multi-dimensional interface reinforcement phase.

[0036] In some preferred embodiments, when the chemical vapor deposition method is used to in-situ construct the interface reinforcement phase, the carbon source gas used includes methane and / or acetylene, the temperature is 800-1100°C, the flow ratio of the carbon source gas to hydrogen is (1-3): (3-1), and the deposition time is 0.1-5.0h.

[0037] In some preferred embodiments, the preparation method includes: performing functionalization treatment on the interface reinforcement phase carbon fiber by any one or more of acid washing, alkali washing or oxidation to obtain functionalized interface reinforcement phase carbon fiber; wherein the functionalization treatment at least makes the surface of the interface reinforcement phase carbon fiber contain carboxyl and / or hydroxyl groups.

[0038] In some preferred embodiments, the preparation method comprises: using any one or a combination of two or more of terminal amino hyperbranched polymers, polysilazane with side chain amino groups, amino acid derivatives with side chain amino groups, polypropylene imine triamine dendrimers, tetraaminophthalocyanine, and polydopamine with side chain amino groups to covalently modify the functionalized interface reinforcement phase carbon fiber to obtain the modified carbon fiber.

[0039] Furthermore, the amino-terminated hyperbranched polymer is NH2-HBP.

[0040] Furthermore, the polysilazane with side chain amino groups is -[R1R2Si-NR3]-, wherein R1 is CH3, R2 is CH2CH2NH2, and R3 is CH3.

[0041] Furthermore, the amino acid derivative of the side chain amino group is NH2(CH2)5NHCOC=CCOOH.

[0042] Furthermore, the modification treatment at least causes the surface of the functionalized interfacial reinforcement phase carbon fiber to contain amino groups.

[0043] In some preferred embodiments, the carbon fiber includes any one of carbon fiber powder, chopped carbon fiber, and carbon fiber cloth, or a combination of two or more thereof, and is not limited thereto.

[0044] In some preferred embodiments, the resin includes one of waterborne epoxy resin, polyurethane, polyurea, and silicone resin, but is not limited thereto.

[0045] Another aspect of an embodiment of the present invention also provides an interface-engaged carbon fiber composite material obtained by the aforementioned preparation method, wherein a mechanically engaged strong bonding interface is formed between the interface reinforcement phase in the carbon fiber composite material and the resin, and a chemically bonded strengthening structure is formed between the modified carbon fiber and the resin.

[0046] Another aspect of the embodiments of the present invention further provides use of the aforementioned interface-engaged carbon fiber composite material in extreme marine environments.

[0047] For example, it exhibits excellent mechanical properties and resistance to erosion and wear in the wave splash zone and water level change zone, exhibits excellent corrosion resistance and mechanical properties in the atmosphere, exhibits excellent deep-sea high-pressure resistance in the deep-sea environment, and exhibits anti-radiation performance in the irradiation environment.

[0048] Another aspect of the embodiments of the present invention further provides a method for improving the interface performance of carbon fiber composite materials by using interface meshing reinforcement, which comprises:

[0049] The interface reinforcement phase is constructed in situ on the surface of the carbon fiber by chemical vapor deposition to obtain the interface reinforcement phase carbon fiber; wherein the interface reinforcement phase includes any one of carbon nanospheres, carbon nanowires, and carbon nanosheets, or a combination of two or more thereof;

[0050] Performing surface functional modification on the interface reinforcement phase carbon fiber to obtain modified carbon fiber;

[0051] Furthermore, the modified carbon fiber and the resin are uniformly mixed and cured, thereby improving the interface performance of the carbon fiber composite material.

[0052] In some preferred embodiments, the interface reinforcement phase is a multi-dimensional interface reinforcement phase.

[0053] In some preferred embodiments, when the chemical vapor deposition method is used to in-situ construct the interface reinforcement phase, the carbon source gas used includes methane and / or acetylene, the temperature is 800-1100°C, the flow ratio of the carbon source gas to hydrogen is (1-3): (3-1), and the deposition time is 0.1-5.0h.

[0054] In some preferred embodiments, the method includes: performing functionalization treatment on the interface reinforcement phase carbon fiber by any one or more of acid washing, alkali washing or oxidation to obtain functionalized interface reinforcement phase carbon fiber; wherein the functionalization treatment at least makes the surface of the interface reinforcement phase carbon fiber contain carboxyl and / or hydroxyl groups.

[0055] In some preferred embodiments, the method comprises: using any one or a combination of two or more of terminal amino hyperbranched polymers, polysilazane with side chain amino groups, amino acid derivatives with side chain amino groups, polypropylene imine triamine dendrimers, tetraaminophthalocyanine, and polydopamine with side chain amino groups to covalently modify the functionalized interface reinforcement phase carbon fiber to obtain the modified carbon fiber.

[0056] Furthermore, the amino-terminated hyperbranched polymer is NH2-HBP.

[0057] Furthermore, the polysilazane with side chain amino groups is -[R1R2Si-NR3]-, wherein R1 is CH3, R2 is CH2CH2NH2, and R3 is CH3.

[0058] Furthermore, the amino acid derivative of the side chain amino group is NH2(CH2)5NHCOC=CCOOH.

[0059] Furthermore, the modification treatment at least causes the surface of the functionalized interfacial reinforcement phase carbon fiber to contain amino groups.

[0060] In some preferred embodiments, the carbon fiber includes any one of carbon fiber powder, chopped carbon fiber, and carbon fiber cloth, or a combination of two or more thereof, and is not limited thereto.

[0061] In some preferred embodiments, the resin includes one of waterborne epoxy resin, polyurethane, polyurea, and silicone resin, but is not limited thereto.

[0062] In some more specific embodiments, the method of improving the interface performance of carbon fiber composite materials by using interface meshing reinforcement in the present invention includes:

[0063] (1) using chemical vapor deposition to in situ construct one or more multi-dimensional interface reinforcement phases such as carbon nanospheres, carbon nanowires, and carbon nanosheets on the surface of carbon fibers;

[0064] (2) The surface of the carbon fiber of the growth interface reinforcement phase is functionalized, that is, the original carbon fiber is functionalized, that is, the surface of the carbon fiber is rich in functional groups such as carboxyl and hydroxyl groups by one or more of acid washing, alkali washing and oxidation, and then the carbon fiber is functionalized by using one or more of terminal amino hyperbranched polymer (NH2-HBP), side chain amino polysilazane [-[R1R2Si-NR3]-, (R1:CH3), (R2:CH2CH2NH2), (R3:CH3)], side chain amino amino acid derivative (NH2(CH2)5NHCOC=CCOOH), polypropylene imine triamine dendrimer, tetraaminophthalocyanine, side chain amino polydopamine to modify the carbon fiber, so that the surface of the modified carbon fiber is rich in active groups;

[0065] (3) The carbon fibers that have grown an interface reinforcement phase and have been surface functionalized are added to the resin, dispersed evenly, and cured to obtain an interface-engaged carbon fiber reinforced composite material (i.e., the aforementioned "interface-engaged carbon fiber composite material").

[0066] Furthermore, the surface of the carbon fiber after the functional modification treatment in step (2) contains abundant amino groups, which can react with the resin to form chemical bonds.

[0067] Furthermore, the carbon fibers grown in step (3) after the interface reinforcement phase is grown and the surface is functionalized and modified are added to the resin to form a uniformly dispersed structure. These uniformly dispersed structures can greatly reduce defects such as cracks and pores in the fiber-reinforced composite material.

[0068] Furthermore, chemical vapor deposition can grow the interface reinforcement phase on the surface of carbon fiber powder, chopped carbon fiber and carbon fiber cloth.

[0069] Furthermore, the interface reinforcement phase is firmly bonded to the carbon fiber, and a mechanically meshing strong bonding interface is formed between the carbon fiber growing the interface reinforcement phase and the resin. The mechanical meshing effect between the interface reinforcement phase and the resin can improve the interface performance between the carbon fiber and the resin.

[0070] Furthermore, after the functional modification of the carbon fiber surface, it can react with the resin to form a chemical bond, and the type of the chemical bond is related to the type of functional group and the type of resin. The chemical bond can further improve the interface performance between the carbon fiber and the resin.

[0071] Furthermore, the interface reinforcement phase grown on the surface of the carbon fiber forms an interface meshing reinforcement with the resin, and the chemical bond between the surface and the resin forms a chemical bonding reinforcement after the surface functionalization modification, thereby comprehensively improving the macroscopic properties of the carbon fiber composite material by means of the synergistic effect of the interface meshing reinforcement and the chemical bonding reinforcement.

[0072] The carbon fiber surface treatment method of the present invention can greatly improve the interface performance between the carbon fiber and the resin, so that the modified carbon fiber reinforced resin composite coating has excellent mechanical properties, erosion resistance, deep sea high pressure resistance, radiation resistance and other properties.

[0073] The present invention constructs carbon nanospheres, carbon nanowires, and carbon nanosheets in situ on the fiber surface. The spherical structure, nanowires, and sheet structure of these interface reinforcement phases are mechanically meshed with epoxy resin, so that after the resin matrix is ​​cured, the interface reinforcement phase is embedded in the resin matrix to form a mechanical meshing interface structure, and then the amino group is introduced by surface modification to form a ring-opening reaction with the epoxy resin to form chemical bonding reinforcement. Due to the huge difference in storage modulus between carbon fiber and resin, common problems such as stress concentration and crack propagation occur at the interface between fiber and resin. After constructing the interface reinforcement phase and functional modification, the storage modulus between the fiber, the interface reinforcement phase, and the resin matrix forms a multi-level gradient transition, so that stress can be transferred from the resin matrix to the fiber, and energy is dissipated and cracks are deflected at the interface. The interface compatibility, interface shear strength, and interface toughness matching of carbon fiber and resin are improved by the synergistic effect of interface meshing reinforcement and chemical bonding reinforcement. The physical and chemical synergistic effect at the interface makes the carbon fiber and the resin form a whole, forming a reinforcement effect similar to no interface. In the present invention, a multi-dimensional interface reinforcement phase can be constructed in situ on the surface of the carbon fiber by the method of chemical vapor deposition, and then the carbon fiber with the grown interface reinforcement phase is surface modified to introduce amino groups, thereby improving the interface performance between the carbon fiber and the resin by virtue of the synergistic effect of interface reinforcement and chemical bonding reinforcement.

[0074] In some more specific embodiments, the method of improving the interface performance of carbon fiber composite materials by using interface meshing reinforcement in the present invention includes:

[0075] 1. In-situ growth of multi-dimensional interface enhancement phase:

[0076] (1) Select 500 mesh carbon fiber powder, remove the sizing agent and other impurities on the surface of the carbon fiber before growing the multi-dimensional interface reinforcement phase, use acid washing and alkali washing methods to finally clean the carbon fiber to neutrality, and dry it to obtain a carbon fiber raw material with a clean surface and no impurities.

[0077] (2) One or more multi-dimensional interface reinforcement phases such as carbon nanospheres, carbon nanowires, and carbon nanosheets are in situ constructed on the surface of carbon fiber powder by chemical vapor deposition. The chemical vapor deposition process adopts a segmented growth process. First, a mixed gas of hydrogen and nitrogen is introduced for pretreatment; then, the carbon source introduced during the growth stage is methane, the temperature during the growth stage is 800-1100°C, and the ratio of the carbon source gas flow rate to the nitrogen gas flow rate is 1:3; after the growth is completed, nitrogen is continued to be introduced as a protective atmosphere, and the total deposition time is 4 hours.

[0078] By regulating the chemical vapor deposition process parameters, one or more of the multi-dimensional interface reinforcement phases such as carbon nanospheres, carbon nanowires, and carbon nanosheets can be grown in situ on the carbon fiber surface. The grown interface reinforcement phase forms a mechanical meshing interface reinforcement effect with the resin.

[0079] 2. Surface modification to introduce amino groups:

[0080] The carbon fiber with the interface reinforcement phase is subjected to surface functional modification. First, the carbon fiber with the interface reinforcement phase is subjected to hydroxylation treatment so that the surface of the carbon fiber has abundant hydroxyl groups. Then, one or more of terminal amino hyperbranched polymer (NH2-HBP), polysilazane with side chain amino group [-[R1R2Si-NR3]-, (R1:CH3), (R2:CH2CH2NH2), (R3:CH3)], amino acid derivative with side chain amino group (NH2(CH2)5NHCOC=CCOOH), polypropylene imine triamine dendrimer, tetraaminophthalocyanine, and polydopamine with side chain amino group are used to perform functional modification on the carbon fiber after hydroxylation treatment. The surface of the carbon fiber after functional modification treatment contains abundant amino groups, which can react with the epoxy group of epoxy resin to form chemical bonding.

[0081] 3. Preparation of carbon fiber reinforced composite materials:

[0082] The carbon fibers that have grown the interface reinforcement phase and surface functionalization are added to the resin and dispersed evenly and cured to obtain the interface meshing reinforced carbon fiber reinforced composite material. The evenly dispersed carbon fibers can greatly reduce defects such as cracks and pores in the composite material.

[0083] In some more specific embodiments, the method of improving the interface performance of carbon fiber composite materials by using interface meshing reinforcement in the present invention includes:

[0084] 1. In-situ growth of multi-dimensional interface enhancement phase:

[0085] (1) Chopped carbon fibers are selected as raw materials. Before growing a multi-dimensional interface reinforcement phase, the sizing agent and other impurities on the surface of the carbon fibers are removed by acid washing and alkali washing. After desizing, the bundled carbon fibers are separated into single filaments or bundles with smaller diameters, so that after subsequent surface modification, the chopped carbon fibers can be efficiently and evenly dispersed in the resin without agglomeration. Finally, the carbon fibers are washed to neutrality and dried to obtain a carbon fiber raw material with a clean surface and no impurities.

[0086] (2) One or more multi-dimensional interface reinforcement phases such as carbon nanospheres, carbon nanowires, and carbon nanosheets are in situ constructed on the surface of chopped carbon fibers by chemical vapor deposition. The chemical vapor deposition process adopts a segmented growth process. First, a mixed gas of hydrogen and nitrogen is introduced for pretreatment; then, the carbon source introduced during the growth stage is methane, the temperature during the growth stage is 900-1100°C, and the ratio of the carbon source gas flow rate to the nitrogen gas flow rate is 1:4; after the growth is completed, nitrogen is continued to be introduced as a protective atmosphere, and the total deposition time is 5 hours.

[0087] By regulating the chemical vapor deposition process parameters, one or more of the multi-dimensional interface reinforcement phases such as carbon nanospheres, carbon nanowires, and carbon nanosheets can be grown in situ on the carbon fiber surface. The grown interface reinforcement phase forms a mechanical meshing interface reinforcement effect with the resin.

[0088] 2. Surface modification to introduce amino groups:

[0089] The carbon fiber with the interface reinforcement phase is subjected to surface functional modification. First, the carbon fiber with the interface reinforcement phase is subjected to oxidation treatment so that the surface of the carbon fiber has abundant hydroxyl and carboxyl groups. Then, one or more of terminal amino hyperbranched polymer (NH2-HBP), polysilazane with side chain amino group [-[R1R2Si-NR3]-, (R1:CH3), (R2:CH2CH2NH2), (R3:CH3)], amino acid derivative with side chain amino group (NH2(CH2)5NHCOC=CCOOH), polypropylene imine triamine dendrimer, tetraaminophthalocyanine, and polydopamine with side chain amino group are used to perform functional modification on the carbon fiber after hydroxylation treatment. The surface of the carbon fiber after functional modification treatment contains abundant amino groups, which can react with the epoxy group of epoxy resin to form chemical bonding.

[0090] 3. Preparation of carbon fiber reinforced composite materials:

[0091] The chopped carbon fibers after the growth of the interface reinforcement phase and the surface functionalization modification are added to the resin and dispersed evenly and cured to obtain the interface meshing reinforced carbon fiber reinforced composite material. The evenly dispersed carbon fibers can greatly reduce defects such as cracks and pores in the composite material.

[0092] In some more specific embodiments, the method of improving the interface performance of carbon fiber composite materials by using interface meshing reinforcement in the present invention includes:

[0093] 1. In-situ growth of multi-dimensional interface enhancement phase:

[0094] (1) Carbon fiber cloth is selected as the raw material. Before growing the multi-dimensional interface reinforcement phase, the adhesive and other impurities on the surface of the carbon fiber are removed by acid washing and alkali washing. The bundled carbon fiber tows are separated after treatment, and then the carbon fiber is washed to neutrality and dried to obtain a carbon fiber raw material with a clean surface and no impurities.

[0095] (2) One or more multi-dimensional interface reinforcement phases such as carbon nanospheres, carbon nanowires, and carbon nanosheets are in situ constructed on the surface of chopped carbon fibers by chemical vapor deposition. The chemical vapor deposition process adopts a segmented growth process, firstly, nitrogen is introduced for pretreatment; then, acetylene is introduced as the carbon source during the growth stage, the temperature during the growth stage is 1000-1100°C, the ratio of the carbon source gas flow rate to the nitrogen gas flow rate is 1:3, and the deposition time is 3 hours; after the growth is completed, nitrogen is continued to be introduced as a protective atmosphere.

[0096] By regulating the chemical vapor deposition process parameters, one or more of the multi-dimensional interface reinforcement phases such as carbon nanospheres, carbon nanowires, and carbon nanosheets can be grown in situ on the carbon fiber surface. The grown interface reinforcement phase forms a mechanical meshing interface reinforcement effect with the resin.

[0097] 2. Surface modification to introduce amino groups:

[0098] The carbon fiber with the interface reinforcement phase is subjected to surface functional modification. First, the carbon fiber with the interface reinforcement phase is subjected to acid washing treatment so that the surface of the carbon fiber has abundant carboxyl groups. Then, one or more of terminal amino hyperbranched polymer (NH2-HBP), polysilazane with side chain amino group [-[R1R2Si-NR3]-, (R1: CH3), (R2: CH2CH2NH2), (R3: CH3)], amino acid derivative with side chain amino group (NH2(CH2)5NHCOC=CCOOH), polypropylene imine triamine dendrimer, tetraaminophthalocyanine, and polydopamine with side chain amino group are used to perform functional modification on the carbon fiber after hydroxylation treatment. The surface of the carbon fiber after functional modification treatment contains abundant amino groups, and these amino groups can react with the epoxy group of epoxy resin to form chemical bonding.

[0099] 3. Preparation of carbon fiber reinforced composite materials:

[0100] The carbon fiber cloth after growth of interface reinforcement phase and surface functionalization modification is immersed in resin, and then a certain thickness of resin is formed on the surface of the fiber cloth. After curing, an interface meshing reinforced carbon fiber reinforced composite material is obtained.

[0101] In some more specific embodiments, the method of improving the interface performance of carbon fiber composite materials by using interface meshing reinforcement in the present invention includes:

[0102] 1. In-situ growth of multi-dimensional interface enhancement phase:

[0103] (1) Carbon fiber powder and carbon fiber cloth are selected as raw materials. Before growing the multi-dimensional interface reinforcement phase, the sizing agent, adhesive and other impurities on the surface of the carbon fiber are removed by acid washing and alkali washing. The carbon fiber is then washed to neutrality and dried to obtain a carbon fiber raw material with a clean surface and no impurities.

[0104] (2) One or more multi-dimensional interface reinforcement phases such as carbon nanospheres, carbon nanowires, and carbon nanosheets are in situ constructed on the surface of carbon fiber powder and carbon fiber cloth by chemical vapor deposition. The chemical vapor deposition process adopts a segmented growth process, firstly, nitrogen is introduced for pretreatment; then, the carbon source introduced in the growth stage is methane, the temperature in the growth stage is 900-1100°C, and the ratio of the carbon source gas flow rate to the nitrogen gas flow rate is 1:4; after the growth is completed, nitrogen is continued to be introduced as a protective atmosphere, and the total deposition time is 3-4 hours.

[0105] By regulating the chemical vapor deposition process parameters, one or more of the multi-dimensional interface reinforcement phases such as carbon nanospheres, carbon nanowires, and carbon nanosheets can be grown in situ on the carbon fiber surface. The grown interface reinforcement phase forms a mechanical meshing interface reinforcement effect with the resin.

[0106] 2. Surface modification to introduce amino groups:

[0107] The carbon fiber powder and carbon fiber cloth with the interfacial reinforcement phase are respectively subjected to surface functional modification. First, the carbon fiber powder and carbon fiber cloth with the interfacial reinforcement phase are subjected to acid washing treatment so that the carbon fiber surface has abundant hydroxyl and carboxyl groups. Then, one or more of terminal amino hyperbranched polymer (NH2-HBP), polysilazane with side chain amino group [-[R1R2Si-NR3]-, (R1:CH3), (R2:CH2CH2NH2), (R3:CH3)], amino acid derivative with side chain amino group (NH2(CH2)5NHCOC=CCOOH), polypropylene imine triamine dendrimer, tetraaminophthalocyanine, and polydopamine with side chain amino group are used to functionally modify the carbon fiber after hydroxylation treatment. The surface of the carbon fiber after functional modification treatment contains abundant amino groups, which can react with the epoxy group of epoxy resin to form chemical bonding.

[0108] 3. Preparation of carbon fiber reinforced composite materials:

[0109] First, the carbon fiber powder after the growth interface reinforcement phase and surface functionalization modification is added to the epoxy resin and dispersed evenly to obtain a carbon fiber modified resin composite material. The evenly dispersed carbon fiber can greatly reduce defects such as cracks and pores in the resin.

[0110] Then the carbon fiber cloth is immersed in the epoxy resin modified by carbon fiber powder, and then a certain thickness of carbon fiber modified epoxy resin is formed on the surface of the fiber cloth. After curing, an interface meshing reinforced carbon fiber reinforced composite material is obtained, so that the resin inside the surface of the carbon fiber cloth also contains uniformly dispersed interface modified carbon fiber powder material. A carbon fiber reinforced epoxy composite material with excellent comprehensive performance is obtained by compounding the carbon fiber powder modified epoxy resin with the interface reinforced carbon fiber cloth.

[0111] The interface reinforcement phase is firmly bonded to the carbon fiber, and a mechanical meshing type strong bonding interface is formed between the carbon fiber growing the interface reinforcement phase and the resin. The mechanical meshing effect between the interface reinforcement phase and the resin can improve the interface performance between the carbon fiber and the resin. The functional modified molecules on the surface of the carbon fiber can react with the resin to form a chemical bond. The type of chemical bond is related to the type of functional molecules and the type of resin. The chemical bond can further improve the interface performance between the carbon fiber and the resin.

[0112] The interface reinforcement phase grown on the surface of carbon fiber forms interface meshing reinforcement with the resin, and the chemical bond between the surface and the resin forms chemical bonding reinforcement after surface functionalization modification. The synergistic effect of interface meshing reinforcement and chemical bonding reinforcement can comprehensively improve the macroscopic properties of carbon fiber composites.

[0113] After surface functional modification, the interfacial compatibility between carbon fiber and resin is enhanced, so the carbon fiber and resin form a whole at the interface, and no interface defects such as weak interfacial bonding and zero volume defects will occur. This also makes the interface between carbon fiber and resin meet the service requirements in extreme marine environments.

[0114] The technical solution of the present invention is further described in detail below in conjunction with several preferred embodiments. This embodiment is implemented on the premise of the technical solution of the invention, and a detailed implementation method and specific operation process are given, but the protection scope of the present invention is not limited to the following embodiments.

[0115] Unless otherwise specified, the experimental materials used in the following examples can be purchased from conventional biochemical reagent companies.

[0116] Example 1

[0117] 1. In-situ growth of multi-dimensional interface enhancement phase:

[0118] (1) Select 500 mesh carbon fiber powder, remove the sizing agent and other impurities on the surface of the carbon fiber before growing the multidimensional interface reinforcement phase, and carry out pickling treatment in a 20 g / L hydrochloric acid solution. The magnetic stirring speed is 400 r / min, the temperature is 60 ° C, and the pickling time is 3 hours. After pickling, use a large amount of deionized water to wash the carbon fiber to neutrality, and dry it in an environment of 80 ° C for 2 hours to obtain a carbon fiber raw material with a clean surface and no impurities.

[0119] (2) Carbon nanospheres were constructed in situ on the surface of carbon fiber powder by chemical vapor deposition. A segmented growth process was used in the chemical vapor deposition process. First, a mixed gas of hydrogen and argon was introduced for pretreatment. Then, methane was introduced as the carbon source during the growth stage. The temperature during the growth stage was 1000°C. The ratio of the carbon source gas flow rate to the hydrogen gas flow rate was 1:10. After the growth was completed, nitrogen was introduced as a protective atmosphere. The total deposition time was 4 hours.

[0120] By adjusting the chemical vapor deposition process parameters, carbon nanospheres with uniform size and regular shape can be grown in situ on the carbon fiber surface to enhance the interface. Figure 1 As shown, it can be found that the carbon nanospheres are concentrically structured carbon spheres, and multiple layers of parallel and continuous carbon layers are grown on the surface of the carbon fiber where no carbon spheres are grown. Since the growth of the carbon layer can repair the defects on the surface of the carbon fiber, the in-situ grown carbon nanospheres are firmly bonded to the carbon fiber and form a mechanically meshing interface strengthening effect with the resin.

[0121] 2. Surface modification to introduce amino groups:

[0122] The carbon fiber with the growth interface reinforcement phase was subjected to surface functionalization modification. First, the carbon fiber with the growth interface reinforcement phase was functionalized with a mixed solution of sulfuric acid and nitric acid and treated at 65°C for 15 minutes, so that the carbon fiber surface had abundant hydroxyl and carboxyl groups. Then, polysilazane with side chain amino groups was used to functionalize the carbon fiber after the functionalization treatment. The surface of the carbon fiber after the functionalization modification treatment contained abundant amino groups. When the surface functionalized carbon fiber was added to the epoxy resin E51, the abundant amino groups on the surface of the carbon fiber could react with the epoxy groups of the epoxy resin to form a chemical bonding reaction.

[0123] 3. Preparation of carbon fiber reinforced composite materials:

[0124] The carbon fibers that have grown the interface reinforcement phase and surface functionalization are added to the resin and dispersed evenly and cured to obtain the interface meshing reinforced carbon fiber reinforced composite material. The evenly dispersed carbon fibers can greatly reduce defects such as cracks and pores in the composite material.

[0125] The interface reinforcement phase is firmly bonded to the carbon fiber, and a mechanical meshing type strong bonding interface is formed between the carbon fiber growing the interface reinforcement phase and the resin. The mechanical meshing effect between the interface reinforcement phase and the resin can improve the interface performance between the carbon fiber and the resin. The functional modified molecules on the surface of the carbon fiber can react with the resin to form a chemical bond. The type of chemical bond is related to the type of functional molecules and the type of resin. The chemical bond can further improve the interface performance between the carbon fiber and the resin.

[0126] The interface reinforcement phase grown on the surface of carbon fiber forms an interface meshing reinforcement with the resin, and the chemical bond between the surface and the resin forms a chemical bonding reinforcement after surface functionalization modification. The macroscopic performance of carbon fiber composite materials is comprehensively improved by the synergistic effect of interface meshing reinforcement and chemical bonding reinforcement. The micro-bead debonding experiment measured the interface shear strength between carbon fiber and epoxy resin to reach 110MPa, and the multiphase flow erosion experiment measured the erosion volume of the interface meshing reinforced carbon fiber reinforced epoxy composite material to reduce by 91.4%. The carbon fiber composite material was brittle fractured by liquid nitrogen to expose the interface between carbon fiber and epoxy resin. The composite material after brittle fracture was immersed in a simulated deep sea high pressure of 5,000 meters for 240 hours. After taking it out, the interface between carbon fiber and epoxy resin was observed under a scanning electron microscope. It was found that there was no failure form such as interface cracking and crack extension at the interface, indicating that the interface meshing reinforced carbon fiber reinforced composite material has excellent high pressure resistance.

[0127] The morphology of the interface between the carbon fiber and the resin of the carbon fiber reinforced composite material in this embodiment after 240 hours in a simulated deep sea environment of 5000 meters is as follows: Figure 2 As shown in the figure, the interface morphology of carbon fiber and resin of carbon fiber reinforced composite material after erosion test is shown in the figure. Figure 3 shown.

[0128] After surface functional modification, the interfacial compatibility between carbon fiber and resin is enhanced, so the carbon fiber and resin form a whole at the interface, and no interface defects such as weak interfacial bonding and zero volume defects will occur. This also makes the interface between carbon fiber and resin meet the service requirements in extreme marine environments.

[0129] Example 2

[0130] 1. In-situ growth of multi-dimensional interface enhancement phase:

[0131] (1) Chopped carbon fiber is selected as raw material, and the sizing agent and other impurities on the surface of the carbon fiber are removed before growing the multi-dimensional interface reinforcement phase. The carbon fiber is pickled in a 10g / L sulfuric acid and nitric acid solution, with a magnetic stirring speed of 400r / min, a temperature of 70°C, and a pickling time of half an hour. After pickling, the carbon fiber is washed with a large amount of deionized water until it is neutral, and dried in an environment of 60°C for 2 hours to obtain a carbon fiber raw material with a clean surface and no impurities. After treatment, the bundled carbon fiber is separated into monofilaments or bundles with smaller diameters, so that the chopped carbon fiber can be efficiently and evenly dispersed in the resin after subsequent surface modification without agglomeration.

[0132] (2) The carbon nanowires were constructed in situ on the surface of carbon fiber powder by chemical vapor deposition. The chemical vapor deposition process used a segmented growth process. First, a mixed gas of hydrogen and argon was introduced for pretreatment; then, methane and hydrogen were introduced in a ratio of 1:10 during the growth phase. The temperature of the growth phase was 900°C and the deposition time was 1 hour. After the growth was completed, nitrogen was introduced as a protective atmosphere.

[0133] By regulating the chemical vapor deposition process parameters, the carbon nanowires can be grown in situ on the carbon fiber surface. The interface reinforcement phase has a relatively uniform length and is densely arranged. Scanning electron microscopy shows that the carbon nanowires are radial on the carbon fiber surface. The in situ grown carbon nanowires are firmly bonded to the carbon fiber and form a mechanically meshed interface reinforcement effect with the resin.

[0134] 2. Surface modification to introduce amino groups:

[0135] The carbon fiber with the grown interface reinforcement phase is surface functionalized. First, the carbon fiber with the grown interface reinforcement phase is functionalized with dilute sulfuric acid at 75°C for 12 minutes to make the surface of the carbon fiber have abundant hydroxyl and carboxyl groups. Then, the functionalized carbon fiber is functionalized with an amino acid derivative with a side chain amino group at 50°C for 8 hours. The surface of the functionalized carbon fiber contains abundant amino groups. The surface functionalized carbon fiber is added to a water-based epoxy resin. The abundant amino groups on the surface of the carbon fiber can react with the epoxy groups of the epoxy resin to form a chemical bonding reaction.

[0136] 3. Preparation of carbon fiber reinforced composite materials:

[0137] The carbon fibers that have grown the interface reinforcement phase and surface functionalization are added to the resin and dispersed evenly and cured to obtain the interface meshing reinforced carbon fiber reinforced composite material. The evenly dispersed carbon fibers can greatly reduce defects such as cracks and pores in the composite material.

[0138] The interface reinforcement phase is firmly bonded to the carbon fiber, and a mechanical meshing type strong bonding interface is formed between the carbon fiber growing the interface reinforcement phase and the resin. The mechanical meshing effect between the interface reinforcement phase and the resin can improve the interface performance between the carbon fiber and the resin. The functional modified molecules on the surface of the carbon fiber can react with the resin to form a chemical bond. The type of chemical bond is related to the type of functional molecules and the type of resin. The chemical bond can further improve the interface performance between the carbon fiber and the resin.

[0139] The interface reinforcement phase grown on the surface of carbon fiber forms an interface meshing reinforcement with the resin, and the chemical bond between the surface and the resin forms a chemical bonding reinforcement after surface functionalization modification. The synergistic effect of interface meshing reinforcement and chemical bonding reinforcement comprehensively improves the macroscopic performance of carbon fiber composite materials. The micro-bead debonding experiment measured the interface shear strength between carbon fiber and epoxy resin to reach 102MPa. The multiphase flow erosion experiment measured the erosion volume of the interface meshing reinforced carbon fiber reinforced epoxy composite material to be reduced by 86%. The carbon fiber composite material was brittle fractured with liquid nitrogen to expose the interface between the carbon fiber and the epoxy resin. The composite material after brittle fracture was immersed in 30MPa high pressure for 240 hours. After taking it out, the interface between the carbon fiber and the epoxy resin was observed under a scanning electron microscope. It was found that there was no failure form such as interface cracking and crack extension at the interface, indicating that the interface meshing reinforced carbon fiber reinforced composite material has excellent high pressure resistance.

[0140] After surface functional modification, the interfacial compatibility between carbon fiber and resin is enhanced, so the carbon fiber and resin form a whole at the interface, and no interface defects such as weak interfacial bonding and zero volume defects will occur. This also makes the interface between carbon fiber and resin meet the service requirements in extreme marine environments.

[0141] Example 3

[0142] 1. In-situ growth of multi-dimensional interface enhancement phase:

[0143] (1) Carbon fiber cloth was selected as the raw material, and the sizing agent and other impurities on the surface of the carbon fiber were removed before growing the multidimensional interface reinforcement phase. The carbon fiber was pickled in a 10 g / L sulfuric acid and nitric acid solution, with a magnetic stirring speed of 400 r / min, a temperature of 75 °C, and a pickling time of 15 min. After pickling, the carbon fiber was washed with a large amount of deionized water until it was neutral, and dried at 50 °C for 150 min. The bundled carbon fiber tows were separated after treatment to obtain a carbon fiber raw material with a clean surface and no impurities.

[0144] (2) Carbon nanospheres were constructed in situ on the surface of carbon fiber powder by chemical vapor deposition. The chemical vapor deposition process used a segmented growth process. First, a mixed gas of hydrogen and argon was introduced for pretreatment. Then, the carbon source in the growth stage was acetylene, the temperature in the growth stage was 1100°C, the ratio of the carbon source gas flow rate to the nitrogen gas flow rate was 1:3, and the deposition time was 3 hours. After the growth was completed, nitrogen was continued to be introduced as a protective atmosphere.

[0145] By adjusting the chemical vapor deposition process parameters, the carbon nanospheres can be grown in situ on the carbon fiber surface. The length of the interface reinforcement phase is relatively consistent and densely arranged. Scanning electron microscopy shows that the carbon nanospheres are radial on the carbon fiber surface. The in situ grown carbon nanospheres are firmly bonded to the carbon fiber and form a mechanical meshing interface reinforcement effect with the resin.

[0146] 2. Surface modification to introduce amino groups:

[0147] The carbon fiber with the grown interface reinforcement phase is surface functionalized. First, the carbon fiber with the grown interface reinforcement phase is functionalized with dilute sulfuric acid at 65°C for 20 minutes to make the surface of the carbon fiber have abundant hydroxyl and carboxyl groups. Then, the functionalized carbon fiber is functionalized with an amino acid derivative with a side chain amino group at 65°C for 5 hours. The surface of the functionalized carbon fiber contains abundant amino groups. The surface functionalized carbon fiber is added to a water-based epoxy resin. The abundant amino groups on the surface of the carbon fiber can react with the epoxy groups of the epoxy resin to form a chemical bonding reaction.

[0148] 3. Preparation of carbon fiber reinforced composite materials:

[0149] The carbon fibers that have grown the interface reinforcement phase and surface functionalization are added to the resin and dispersed evenly and cured to obtain the interface meshing reinforced carbon fiber reinforced composite material. The evenly dispersed carbon fibers can greatly reduce defects such as cracks and pores in the composite material.

[0150] The interface reinforcement phase is firmly bonded to the carbon fiber, and a mechanical meshing type strong bonding interface is formed between the carbon fiber growing the interface reinforcement phase and the resin. The mechanical meshing effect between the interface reinforcement phase and the resin can improve the interface performance between the carbon fiber and the resin. The functional modified molecules on the surface of the carbon fiber can react with the resin to form a chemical bond. The type of chemical bond is related to the type of functional molecules and the type of resin. The chemical bond can further improve the interface performance between the carbon fiber and the resin.

[0151] The interface reinforcement phase grown on the surface of carbon fiber forms an interface meshing reinforcement with the resin, and the chemical bond between the surface and the resin forms a chemical bonding reinforcement after surface functionalization modification. The synergistic effect of interface meshing reinforcement and chemical bonding reinforcement comprehensively improves the macroscopic performance of carbon fiber composite materials. The micro-bead debonding experiment measured the interface shear strength between carbon fiber and epoxy resin to reach 105MPa. The multiphase flow erosion experiment measured the erosion volume of the interface meshing strengthened carbon fiber reinforced epoxy composite material to be reduced by 88%. The carbon fiber composite material was brittle fractured with liquid nitrogen to expose the interface between the carbon fiber and the epoxy resin. The composite material after brittle fracture was immersed in 30MPa high pressure for 480 hours. After taking it out, the interface between carbon fiber and epoxy resin was observed under a scanning electron microscope. It was found that there was no failure form such as interface cracking and crack extension at the interface, indicating that the interface meshing strengthened carbon fiber reinforced composite material has excellent high pressure resistance.

[0152] After surface functional modification, the interfacial compatibility between carbon fiber and resin is enhanced, so the carbon fiber and resin form a whole at the interface, and no interface defects such as weak interfacial bonding and zero volume defects will occur. This also makes the interface between carbon fiber and resin meet the service requirements in extreme marine environments.

[0153] Comparative Example 1

[0154] Preparation of carbon fiber reinforced composites:

[0155] The unmodified original carbon fiber is added to the resin, dispersed evenly and cured to obtain a carbon fiber composite material. The carbon fiber can enhance the mechanical properties of the composite material.

[0156] Since there are almost no active groups on the surface of unmodified carbon fiber, the interface between the epoxy resin and the epoxy resin is only bound by van der Waals force and a small amount of hydrogen bonding, showing very poor interfacial properties, and cannot exert the excellent mechanical properties of carbon fiber. And when the content of carbon fiber increases, it is difficult for the carbon fiber to be evenly dispersed in the resin, resulting in carbon fiber agglomeration. This is a defect that has a great impact on the performance of the composite material for resin composite materials, causing stress concentration and enrichment of corrosive media, thereby greatly reducing the comprehensive performance of the composite material.

[0157] The microbead debonding experiment measured the interface shear strength between the unmodified carbon fiber and the epoxy resin to be between 50-60MPa, with an average value of 56MPa. The multiphase flow erosion experiment measured that the erosion volume of the unmodified carbon fiber reinforced epoxy composite material was larger. The same erosion time was consistent with the complete peeling of the coating from the metal substrate surface, and obvious corrosion appeared on the metal substrate surface. In addition, the carbon fiber composite material was brittlely fractured using liquid nitrogen to expose the interface between the carbon fiber and the epoxy resin. The composite material after brittle fracture was immersed in a simulated 5,000-meter deep-sea environment (50MPa high pressure) for 240 hours. After being taken out, the interface between the carbon fiber and the epoxy resin was observed under a scanning electron microscope, and failure forms such as obvious cracking and crack propagation were found at the interface, indicating that the interface performance of the unmodified carbon fiber and the resin is poor and cannot meet the long-term service requirements in deep-sea environments. The morphology of the interface between the carbon fiber and the resin of the carbon fiber reinforced composite material in this comparative example after 240 hours of simulating a deep-sea environment of 5,000 meters is shown in the following figure. Figure 4 As shown in the figure, the interface morphology of carbon fiber and resin of carbon fiber reinforced composite material after erosion test is shown in the figure. Figure 5 shown.

[0158] Since the surface has not been functionally modified, the interface compatibility between the carbon fiber and the resin is poor, so the carbon fiber and the resin are poorly bonded at the interface, resulting in weak interface bonding or interface defects. This makes the interface between the carbon fiber and the resin prone to interface failure under simulated deep-sea extreme environment service conditions, and thus cannot meet the long-life surface safety service requirements in deep-sea environments.

[0159] Comparative Example 2

[0160] 1. Surface modification to introduce amino groups:

[0161] The carbon fiber with the growth interface reinforcement phase was subjected to surface functionalization modification. First, the carbon fiber with the growth interface reinforcement phase was functionalized with a mixed solution of sulfuric acid and nitric acid and treated at 65°C for 15 minutes, so that the carbon fiber surface had abundant hydroxyl and carboxyl groups. Then, polysilazane with side chain amino groups was used to functionalize the carbon fiber after the functionalization treatment. The surface of the carbon fiber after the functionalization modification treatment contained abundant amino groups. When the surface functionalized carbon fiber was added to the epoxy resin E51, the abundant amino groups on the surface of the carbon fiber could react with the epoxy groups of the epoxy resin to form a chemical bonding reaction.

[0162] 2. Preparation of carbon fiber reinforced composite materials:

[0163] The surface functionalized carbon fiber is added to the resin for uniform dispersion and solidification to obtain a carbon fiber reinforced composite material. The uniformly dispersed carbon fiber can greatly reduce defects such as cracks and pores in the composite material.

[0164] The functional modified molecules on the surface of the carbon fiber can react with the resin to form chemical bonds. The type of chemical bonds is related to the type of functional molecules and the type of resin. The chemical bonds can further improve the interface performance between the carbon fiber and the resin.

[0165] After the surface of carbon fiber is functionalized and modified, the chemical bond between the carbon fiber and the resin is formed to strengthen the chemical bonding. With the help of chemical bonding strengthening, the macroscopic performance of carbon fiber composite materials can be effectively improved. The micro-bead debonding experiment measured the interface shear strength between carbon fiber and epoxy resin to reach 70-85MPa, and the multiphase flow erosion experiment measured the interface meshing strengthening carbon fiber reinforced epoxy composite material erosion volume reduced by 67%-74%, the carbon fiber composite material was brittle fractured by liquid nitrogen, so that the interface between carbon fiber and epoxy resin was exposed, and the composite material after brittle fracture was soaked for 240 hours under a high pressure of 5000 meters in the simulated deep sea, and the interface between carbon fiber and epoxy resin was observed under a scanning electron microscope after being taken out, and it was found that some fiber and resin interfaces had interface cracking and crack extension and other failure forms, indicating that the surface modified carbon fiber reinforced composite material has good high pressure resistance, but its high pressure resistance is poor compared with the carbon fiber reinforced composite material with interface meshing strengthening and chemical bonding synergistic enhancement in Example 1.

[0166] The morphology of the interface between the carbon fiber and the resin in the carbon fiber reinforced composite material in this comparative example after 240 hours in a simulated deep sea environment of 5000 meters is as follows Figure 6 As shown in the figure, the interface morphology of carbon fiber and resin of carbon fiber reinforced composite material after erosion test is shown in the figure. Figure 7 shown.

[0167] After surface functional modification, the interfacial compatibility between carbon fiber and resin is enhanced, so the interface between carbon fiber and resin can effectively transfer stress, and the interfacial bonding performance is significantly improved compared with unmodified carbon fiber composites. However, due to the high pressure in the deep sea, carbon fiber reinforced coating materials with only surface functional modification still cannot meet the service requirements in extreme marine environments.

[0168] Comparative Example 3

[0169] 1. In-situ growth of multi-dimensional interface enhancement phase:

[0170] (1) Select 500 mesh carbon fiber powder, remove the sizing agent and other impurities on the surface of the carbon fiber before growing the multidimensional interface reinforcement phase, and carry out pickling treatment in a 20 g / L hydrochloric acid solution. The magnetic stirring speed is 400 r / min, the temperature is 60 ° C, and the pickling time is 3 hours. After pickling, use a large amount of deionized water to wash the carbon fiber to neutrality, and dry it in an environment of 80 ° C for 2 hours to obtain a carbon fiber raw material with a clean surface and no impurities.

[0171] (2) Carbon nanospheres were constructed in situ on the surface of carbon fiber powder by chemical vapor deposition. A segmented growth process was used in the chemical vapor deposition process. First, a mixed gas of hydrogen and argon was introduced for pretreatment. Then, methane was introduced as the carbon source during the growth stage. The temperature during the growth stage was 1000°C. The ratio of the carbon source gas flow rate to the hydrogen gas flow rate was 1:10. After the growth was completed, nitrogen was introduced as a protective atmosphere. The total deposition time was 4 hours.

[0172] By regulating the process parameters of chemical vapor deposition, the carbon nanospheres with uniform size and regular shape can be grown in situ on the surface of carbon fiber to enhance the interface. Scanning electron microscopy shows that the carbon nanospheres are concentrically structured carbon spheres, and multiple layers of parallel and continuous carbon layers grow on the surface of carbon fiber without carbon spheres. Since the growth of carbon layers can repair the defects on the surface of carbon fiber, the in-situ grown carbon nanospheres are firmly bonded to the carbon fiber and form a mechanically meshed interface with the resin to strengthen the meshing effect.

[0173] 2. Preparation of carbon fiber reinforced composite materials:

[0174] The carbon fiber with the interfacial reinforcement phase is added to the resin and dispersed evenly and cured to obtain a carbon fiber reinforced composite material. The evenly dispersed carbon fiber with the interfacial reinforcement phase can significantly improve the interfacial bonding strength of the composite material, thereby showing excellent mechanical properties.

[0175] The interface reinforcement phase is firmly bonded to the carbon fiber, and a mechanically meshing strong bonding interface is formed between the carbon fiber growing the interface reinforcement phase and the resin. The mechanical meshing effect between the interface reinforcement phase and the resin can improve the interface performance between the carbon fiber and the resin.

[0176] The interface reinforcement phase grown on the surface of carbon fiber forms an interface meshing reinforcement with the resin. The macroscopic properties of carbon fiber composites can be significantly improved by means of the interface meshing reinforcement effect. The microbead debonding experiment measured the interfacial shear strength between the carbon fiber and the epoxy resin to reach 80-90MPa, and the multiphase flow erosion experiment measured the erosion volume of the interface meshing strengthened carbon fiber reinforced epoxy composite material to reduce by 70%-85%. The carbon fiber composite material was brittle fractured by liquid nitrogen to expose the interface between the carbon fiber and the epoxy resin. The composite material after brittle fracture was immersed in a simulated deep sea high pressure of 5000 meters for 240 hours. After being taken out, the interface between the carbon fiber and the epoxy resin was observed under a scanning electron microscope, and failure forms such as interface cracking and crack propagation appeared at the interface. This shows that although the interface meshing strengthening can improve the bonding strength between the carbon fiber and the resin, since the carbon fiber and the resin at the interface are still physically bonded, mainly through the van der Waals force, stress concentration occurs at the interface of the composite material under strong high pressure, and the crack propagates along the interface between the fiber and the resin, so that the composite material exhibits the characteristics of strong and brittle at the interface, and its high pressure resistance is poorer than that of the carbon fiber reinforced composite material synergistically enhanced by interface meshing strengthening and chemical bonding in Example 1.

[0177] The morphology of the interface between the carbon fiber and the resin in the carbon fiber reinforced composite material in this comparative example after 240 hours in a simulated deep sea environment of 5000 meters is as follows Figure 8 As shown in the figure, the interface morphology of carbon fiber and resin of carbon fiber reinforced composite material after erosion test is shown in the figure. Fig. 9 shown.

[0178] Since the surface has not been functionally modified, the interface compatibility between the carbon fiber and the resin is poor, resulting in weak interface bonding or interface defects. This makes the interface between the carbon fiber and the resin prone to interface failure under simulated deep-sea extreme environment service conditions, thus failing to meet the long-life surface safety service requirements in deep-sea environments.

[0179] In general, by comparing the embodiments and the comparative examples, surface modification and growth of interface reinforcement phase can improve the interface performance and macroscopic properties such as mechanical properties and high pressure resistance of carbon fiber reinforced composite materials to a certain extent. However, for carbon fiber composite materials that are only surface modified, their interface shear strength is low, and cracks and expansion appear on the interface under the action of deep sea high pressure; for carbon fiber composite materials that grow interface reinforcement phase but are not surface modified, although the interface meshing effect significantly improves the interface shear strength, due to the poor surface active functional groups of carbon fiber, the interface bonding performance with the resin is poor, and the interface stress concentration is prone to occur under the action of deep sea high pressure, so that cracks spread along the fiber and resin interface. It can be concluded that only by surface modification or growth of interface reinforcement phase, it is still impossible to obtain a carbon fiber reinforced composite material with excellent interface performance in a deep sea environment. It is necessary to grow an interface reinforcement phase and perform surface functionalization modification in combination, that is, to improve the interface performance of the carbon fiber reinforced epoxy composite coating by means of the synergistic effect of interface meshing reinforcement and chemical bonding reinforcement, so that it has a series of excellent properties such as excellent mechanical properties, deep sea high pressure resistance and radiation resistance, so that it can meet the long-life safe service in a deep sea high pressure environment.

[0180] In addition, the inventors of this case also referred to the aforementioned embodiments and conducted experiments with other raw materials, process operations, and process conditions described in this specification, and obtained relatively ideal results.

[0181] It should be understood that the technical solution of the present invention is not limited to the above-mentioned specific implementation cases. Any technical deformation made according to the technical solution of the present invention without departing from the scope of protection of the purpose of the present invention and the claims shall fall within the protection scope of the present invention.

Claims

1. A method for preparing an interface-engaged carbon fiber composite material, characterized in that include: The interface reinforcement phase is constructed in situ on the surface of the carbon fiber by chemical vapor deposition to obtain the interface reinforcement phase carbon fiber; wherein the interface reinforcement phase includes any one of carbon nanospheres, carbon nanowires, and carbon nanosheets, or a combination of two or more thereof; Performing surface functional modification on the interface reinforcement phase carbon fiber to obtain modified carbon fiber; And, the modified carbon fiber is evenly mixed with resin and cured to obtain an interface-engaged carbon fiber composite material.

2. The preparation method according to claim 1, characterized in that: The interface reinforcement phase is a multi-dimensional interface reinforcement phase.

3. The preparation method according to claim 1, characterized in that: When the chemical vapor deposition method is used to in-situ construct the interface enhancement phase, the carbon source gas used includes methane and / or acetylene, the temperature is 800-1100°C, the flow ratio of the carbon source gas to hydrogen is (1-3): (3-1), and the deposition time is 0.1-5.0h.

4. The preparation method according to claim 1, characterized in that include: The interface reinforcement phase carbon fiber is subjected to functionalization treatment by any one or more of acid washing, alkali washing or oxidation to obtain functionalized interface reinforcement phase carbon fiber; wherein the functionalization treatment at least makes the surface of the interface reinforcement phase carbon fiber contain carboxyl and / or hydroxyl groups.

5. The preparation method according to claim 4, characterized in that include: The functionalized interface reinforcement phase carbon fiber is covalently modified by using any one of terminal amino hyperbranched polymers, polysilazane with side chain amino groups, amino acid derivatives with side chain amino groups, polypropylene imine triamine dendrimers, tetraaminophthalocyanine, and polydopamine with side chain amino groups, or a combination of two or more thereof, to obtain the modified carbon fiber.

6. The preparation method according to claim 5, characterized in that: The modification treatment at least makes the surface of the functionalized interfacial reinforcement phase carbon fiber contain amino groups.

7. The preparation method according to claim 1, characterized in that: The carbon fiber includes any one or a combination of two or more of carbon fiber powder, chopped carbon fiber, and carbon fiber cloth; And / or, the resin includes any one or a combination of two or more of water-based epoxy resin, polyurethane, polyurea, and silicone resin.

8. The interfacially meshed carbon fiber composite material obtained by the preparation method according to any one of claims 1 to 7, characterized in that: A mechanically meshing strong bonding interface is formed between the interface reinforcement phase in the carbon fiber composite material and the resin, and a chemically bonded strengthening structure is formed between the modified carbon fiber and the resin.

9. Use of the interfacially meshed carbon fiber composite material according to claim 8 in the protection of mechanical parts in deep sea high pressure environments.

10. A method for improving the interface performance of carbon fiber composite materials by using interface meshing reinforcement, characterized in that include: The interface reinforcement phase is constructed in situ on the surface of the carbon fiber by chemical vapor deposition to obtain the interface reinforcement phase carbon fiber; wherein the interface reinforcement phase includes any one of carbon nanospheres, carbon nanowires, and carbon nanosheets, or a combination of two or more thereof; Performing surface functional modification on the interface reinforcement phase carbon fiber to obtain modified carbon fiber; Furthermore, the modified carbon fiber and the resin are uniformly mixed and cured, thereby improving the interface performance of the carbon fiber composite material.

Citation Information

Patent Citations

  • Method for performing amino functionalizing on carbon fiber surface

    CN105113260A

  • Novel pressure-resistant cabin body made from carbon fiber macromolecular composite materials and manufacturing technology of novel pressure-resistant cabin body

    CN105620693A

  • Corrosion-resistance and wear-resistance coating layer containing carbon fibers and preparation method thereof

    CN107858624A

  • Method for repairing modified carbon fiber surface, and application thereof

    CN111851068A

  • Method for synchronously modifying surface and interface of carbon fiber through electrophoretic deposition-electropolymerization and carbon fiber composite material thereof

    CN114032669A