Preparation method of antibacterial modified thermoplastic polyurethane elastomer
By mixing montmorillonite and guanidine-containing halamine phenylphosphate with thermoplastic polyurethane elastomer, antibacterially modified thermoplastic polyurethane elastomer is prepared, which solves the problem of poor antibacterial performance of existing thermoplastic polyurethane elastomers and achieves excellent Antibacterial and flame retardant properties.
Patent Information
- Application Number
- CN202410903549.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-08
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2044-07-08
AI Technical Summary
The existing thermoplastic polyurethane elastomers have poor antibacterial properties, which limits their application in certain fields.
By mixing montmorillonite and guanidine-containing halide phenylphosphate with thermoplastic polyurethane elastomer, after extrusion and granulation, an antibacterial modified thermoplastic polyurethane elastomer is prepared, and the biguanidine and dihalide amine structures are used to enhance Antibacterial properties, and the reaction of phosphorus and nitrogen elements form a dense carbon layer and flame-retardant gas, enhancing the flame retardant performance.
The antibacterial and flame retardant properties of thermoplastic polyurethane elastomers are significantly improved, forming a dense carbon layer and flame-retardant gas, enhancing the fire and bacterial resistance of the material.
Smart Images

Figure CN119019834A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of polyurethane, in particular to a method for preparing an antibacterial modified thermoplastic polyurethane elastomer. Background Art
[0002] Polyurethane refers to a type of polymer containing a large number of repeated carbamate groups in the molecular chain structure. Thermoplastic polyurethane elastomer, referred to as TPU, is a new type of synthetic material between rubber and plastic. It is mainly made of isocyanate, polyol and chain extender through polymerization reaction. It has excellent mechanical properties and wear resistance, and is widely used in transportation, agricultural production, construction and building materials. However, its antibacterial properties are poor, which limits its application in some fields.
[0003] Montmorillonite is a natural silicate mineral with excellent thermal stability, adsorption, impact resistance and other properties, and is widely used in adsorbents, catalysts and other fields. For example, the patent application publication number is CN109134821A, which discloses a flame retardant thermoplastic polyurethane elastomer and a preparation method thereof. The invention uses polytetramethylene ether glycol, organic montmorillonite, mixed flame retardant and the like as raw materials, and the prepared thermoplastic polyurethane elastomer has excellent flame retardant properties, but does not improve the antibacterial properties of the polyurethane elastomer. Summary of the invention
[0004] 1. Technical issues to be solved
[0005] In view of the deficiencies of the prior art, the present invention provides a method for preparing an antibacterial modified thermoplastic polyurethane elastomer. The prepared thermoplastic polyurethane elastomer has excellent antibacterial and flame retardant properties.
[0006] (II) Technical solution
[0007] A method for preparing an antibacterial modified thermoplastic polyurethane elastomer, the preparation method is as follows:
[0008] Thermoplastic polyurethane elastomer, montmorillonite, and guanidine-containing halogenamine phenyl phosphate are added to a high-speed mixer and mixed evenly. The mixture is added to a twin-screw extruder, extruded into granules, and finally placed in a flat vulcanizer at 180° C. and 10 MPa for pressing to obtain an antibacterial modified thermoplastic polyurethane elastomer.
[0009] Preferably, the temperatures of the three zones of the twin-screw extruder are 170°C, 180°C and 175°C.
[0010] Preferably, the mass ratio of the thermoplastic polyurethane elastomer, montmorillonite and guanidine-containing halogenamine phenyl phosphate is 100:(15-30):(1-8).
[0011] Preferably, the preparation method of the guanidine-containing halogenamine phenyl phosphate is:
[0012] (1) 1-Hydroxymethyl-5,5-dimethylhydantoin is added to isopropanol solvent, stirred and dispersed, and then N-(2-hydroxyethyl)ethylenediamine is added thereto, and the reaction is carried out at 20-35° C. for 3-6 hours. After the reaction is completed, the reaction is carried out by vacuum distillation to obtain intermediate 1.
[0013] (2) Add cyanamide to isopropanol solvent, stir and disperse, add 2-5 mol / L hydrochloric acid to adjust the pH to 4-5, then add intermediate 1, react at 10-25° C. for 8-16 hours, and after the reaction is completed, distill under reduced pressure to obtain intermediate 2.
[0014] (3) Under nitrogen conditions, intermediate 2 is added to tetrahydrofuran solvent, stirred and dispersed, and then phenylphosphonic acid dichloride and triethylamine are added thereto. The temperature is raised to 60-70° C. and the reaction is carried out for 20-36 hours. After the reaction is completed, the mixture is filtered, rotary evaporated, washed with deionized water, and dried to obtain intermediate 3.
[0015] (4) Add the intermediate 3 to deionized water, stir and disperse, then add sodium hypochlorite, adjust the pH to 7-8 with 0.4 mol / L sulfuric acid, stir and react at 20-35° C. for 3-6 h. After the reaction is completed, centrifuge, wash with deionized water, and dry to obtain guanidine-containing halogenamine phenyl phosphate.
[0016] Preferably, in step (1), the molar ratio of 1-hydroxymethyl-5,5-dimethylhydantoin to N-(2-hydroxyethyl)ethylenediamine is 1:(1-1.2).
[0017] Preferably, in step (2), the molar ratio of cyanamide to intermediate 1 is (1-1.5):1.
[0018] Preferably, in step (3), the molar ratio of intermediate 2, phenylphosphonic dichloride and triethylamine is (2-3):1:(2.2-2.6).
[0019] Preferably, in step (4), the molar ratio of intermediate 3 to sodium hypochlorite is 1:(2.5-4).
[0020] (III) Beneficial technical effects
[0021] The invention uses 1-hydroxymethyl-5,5-dimethylhydantoin, N-(2-hydroxyethyl)ethylenediamine, cyanamide, phenylphosphonyl dichloride, sodium hypochlorite and the like as raw materials, and reacts to prepare guanidine-containing halogenamine phenyl phosphate. Montmorillonite and guanidine-containing halogenamine phenyl phosphate are added to a thermoplastic polyurethane elastomer, mixed evenly, extruded into granules, and pressed into shape to obtain an antibacterial modified thermoplastic polyurethane elastomer.
[0022] The guanidine-containing halogenamine phenyl phosphate prepared by a series of reactions of the present invention has a simple preparation method and a novel structure. Since it contains a biguanidine structure and a bihaloamine structure, it is added to a thermoplastic polyurethane elastomer, and its antibacterial effect is better than that of a single guanidine and haloamine structure. And since the guanidine-containing halogenamine phenyl phosphate contains more phosphorus and nitrogen elements, both of which are flame retardant elements, it is added to the thermoplastic polyurethane elastomer, and the phosphorus element is heated to produce strong dehydrating substances such as phosphoric acid and metaphosphoric acid, which can promote the dehydration of the material into carbon, and form a dense carbon layer on the surface of the material, isolating the material transport and the transfer of energy. The nitrogen element can be heated to produce a flame-retardant gas, dilute the content of the flammable gas in the air, and further improve the flame retardant properties of the material. The thermoplastic polyurethane elastomer prepared by the present invention has excellent antibacterial properties and flame retardant properties. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1 It is a preparation route for guanidine-containing halogenamine phenyl phosphate. DETAILED DESCRIPTION
[0024] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.
[0025] Example 1
[0026] (1) 0.1 mol of 1-hydroxymethyl-5,5-dimethylhydantoin was added to 200 mL of isopropanol solvent, and the mixture was dispersed by stirring. Then, 0.12 mol of N-(2-hydroxyethyl)ethylenediamine was added thereto, and the mixture was reacted at 25° C. for 4 h. After the reaction was completed, the mixture was distilled under reduced pressure to obtain Intermediate 1.
[0027] (2) 0.25 mol of cyanamide was added to 200 mL of isopropanol solvent, and the mixture was stirred and dispersed. 5 mol / L hydrochloric acid was added to adjust the pH to 5, and then 0.2 mol of intermediate 1 was added to the mixture. The mixture was reacted at 20° C. for 10 h. After the reaction was completed, the mixture was distilled under reduced pressure to obtain intermediate 2.
[0028] (3) Under nitrogen conditions, 0.35 mol of intermediate 2 was added to 200 mL of tetrahydrofuran solvent, stirred and dispersed, and then 0.15 mol of phenylphosphonic dichloride and 0.35 mol of triethylamine were added thereto. The temperature was raised to 65° C. and the reaction was carried out for 26 h. After the reaction was completed, the mixture was filtered, rotary evaporated, washed with deionized water, and dried to obtain intermediate 3.
[0029] (4) 40 mmol of the intermediate 3 was added to 100 mL of deionized water, stirred and dispersed, and then 160 mmol of sodium hypochlorite was added thereto. The pH was adjusted to 7 with 0.4 mol / L sulfuric acid. The mixture was stirred and reacted at 25° C. for 3 h. After the reaction was completed, the mixture was centrifuged, washed with deionized water, and dried to obtain a guanidine-containing halogenamine phenyl phosphate.
[0030] (5) 20 g of thermoplastic polyurethane elastomer, 4 g of montmorillonite, and 0.2 g of guanidine-containing halogenamine phenyl phosphate are added to a high-speed mixer and mixed evenly. The mixture is added to a twin-screw extruder and extruded into granules. The temperatures of the three zones of the twin-screw extruder are 170° C., 180° C., and 175° C. Finally, the mixture is placed in a flat vulcanizer at 180° C. and 10 MPa for pressing to obtain an antibacterial modified thermoplastic polyurethane elastomer.
[0031] Example 2
[0032] (1) 0.1 mol of 1-hydroxymethyl-5,5-dimethylhydantoin was added to 200 mL of isopropanol solvent, and the mixture was dispersed by stirring. Then, 0.1 mol of N-(2-hydroxyethyl)ethylenediamine was added thereto, and the mixture was reacted at 35° C. for 3 h. After the reaction was completed, the mixture was distilled under reduced pressure to obtain Intermediate 1.
[0033] (2) 0.25 mol of cyanamide was added to 200 mL of isopropanol solvent, and the mixture was stirred and dispersed. 3 mol / L hydrochloric acid was added to adjust the pH to 5, and then 0.2 mol of intermediate 1 was added to the mixture. The mixture was reacted at 15° C. for 10 h. After the reaction was completed, the mixture was distilled under reduced pressure to obtain intermediate 2.
[0034] (3) Under nitrogen conditions, 0.35 mol of intermediate 2 was added to 200 mL of tetrahydrofuran solvent, stirred and dispersed, and then 0.15 mol of phenylphosphonic acid dichloride and 0.35 mol of triethylamine were added thereto. The temperature was raised to 65° C. and the reaction was carried out for 25 h. After the reaction was completed, the mixture was filtered, rotary evaporated, washed with deionized water, and dried to obtain intermediate 3.
[0035] (4) 40 mmol of intermediate 3 was added to 100 mL of deionized water, stirred and dispersed, and then 150 mmol of sodium hypochlorite was added thereto. The pH was adjusted to 7 with 0.4 mol / L sulfuric acid. The mixture was stirred and reacted at 35° C. for 6 h. After the reaction was completed, the mixture was centrifuged, washed with deionized water, and dried to obtain guanidine-containing halogenamine phenyl phosphate.
[0036] (5) 20 g of thermoplastic polyurethane elastomer, 4 g of montmorillonite, and 0.5 g of guanidine-containing halogenamine phenyl phosphate are added to a high-speed mixer and mixed evenly. The mixture is added to a twin-screw extruder and extruded into granules. The temperatures of the three zones of the twin-screw extruder are 170° C., 180° C., and 175° C. Finally, the mixture is placed in a flat vulcanizer at 180° C. and 10 MPa for pressing to obtain an antibacterial modified thermoplastic polyurethane elastomer.
[0037] Example 3
[0038] (1) 0.1 mol of 1-hydroxymethyl-5,5-dimethylhydantoin was added to 200 mL of isopropanol solvent, and the mixture was dispersed by stirring. Then, 0.11 mol of N-(2-hydroxyethyl)ethylenediamine was added thereto, and the mixture was reacted at 20° C. for 6 h. After the reaction was completed, the mixture was distilled under reduced pressure to obtain Intermediate 1.
[0039] (2) 0.2 mol of cyanamide was added to 200 mL of isopropanol solvent, and the mixture was dispersed by stirring. 4 mol / L hydrochloric acid was added to adjust the pH to 5, and then 0.2 mol of intermediate 1 was added to the mixture. The mixture was reacted at 10° C. for 16 h. After the reaction was completed, the mixture was distilled under reduced pressure to obtain intermediate 2.
[0040] (3) Under nitrogen conditions, 0.35 mol of intermediate 2 was added to 200 mL of tetrahydrofuran solvent, stirred and dispersed, and then 0.15 mol of phenylphosphonic dichloride and 0.35 mol of triethylamine were added thereto. The temperature was raised to 60° C. and the reaction was carried out for 20 h. After the reaction was completed, the mixture was filtered, rotary evaporated, washed with deionized water, and dried to obtain intermediate 3.
[0041] (4) 40 mmol of the intermediate 3 was added to 100 mL of deionized water, stirred and dispersed, and then 100 mmol of sodium hypochlorite was added thereto. The pH was adjusted to 8 using 0.4 mol / L sulfuric acid. The mixture was stirred and reacted at 20° C. for 4 h. After the reaction was completed, the mixture was centrifuged, washed with deionized water, and dried to obtain a guanidine-containing halogenamine phenyl phosphate.
[0042] (5) 20 g of thermoplastic polyurethane elastomer, 5 g of montmorillonite, and 1 g of guanidine-containing halogenamine phenyl phosphate are added to a high-speed mixer and mixed evenly. The mixture is added to a twin-screw extruder and extruded into granules. The temperatures of the three zones of the twin-screw extruder are 170° C., 180° C., and 175° C. Finally, the mixture is placed in a flat vulcanizer at 180° C. and 10 MPa for pressing to obtain an antibacterial modified thermoplastic polyurethane elastomer.
[0043] Example 4
[0044] (1) 0.1 mol of 1-hydroxymethyl-5,5-dimethylhydantoin was added to 200 mL of isopropanol solvent, and the mixture was dispersed by stirring. Then, 0.12 mol of N-(2-hydroxyethyl)ethylenediamine was added thereto, and the mixture was reacted at 30° C. for 6 h. After the reaction was completed, the mixture was distilled under reduced pressure to obtain Intermediate 1.
[0045] (2) 0.3 mol of cyanamide was added to 200 mL of isopropanol solvent, and the mixture was stirred and dispersed. 2 mol / L hydrochloric acid was added to adjust the pH to 4, and then 0.2 mol of intermediate 1 was added to the mixture. The mixture was reacted at 25° C. for 12 h. After the reaction was completed, the mixture was distilled under reduced pressure to obtain intermediate 2.
[0046] (3) Under nitrogen conditions, 0.45 mol of intermediate 2 was added to 200 mL of tetrahydrofuran solvent, stirred and dispersed, and then 0.15 mol of phenylphosphonic dichloride and 0.33 mol of triethylamine were added thereto. The temperature was raised to 70° C. and the reaction was carried out for 36 hours. After the reaction was completed, the mixture was filtered, rotary evaporated, washed with deionized water, and dried to obtain intermediate 3.
[0047] (4) 40 mmol of the intermediate 3 was added to 100 mL of deionized water, stirred and dispersed, and then 140 mmol of sodium hypochlorite was added thereto. The pH was adjusted to 8 using 0.4 mol / L sulfuric acid. The mixture was stirred and reacted at 25° C. for 5 h. After the reaction was completed, the mixture was centrifuged, washed with deionized water, and dried to obtain a guanidine-containing halogenamine phenyl phosphate.
[0048] (5) 20 g of thermoplastic polyurethane elastomer, 3 g of montmorillonite, and 1.4 g of guanidine-containing halogenamine phenyl phosphate are added to a high-speed mixer and mixed evenly. The mixture is added to a twin-screw extruder and extruded into granules. The temperatures of the three zones of the twin-screw extruder are 170° C., 180° C., and 175° C. Finally, the mixture is placed in a flat vulcanizer at 180° C. and 10 MPa for pressing to obtain an antibacterial modified thermoplastic polyurethane elastomer.
[0049] Example 5
[0050] (1) 0.1 mol of 1-hydroxymethyl-5,5-dimethylhydantoin was added to 200 mL of isopropanol solvent, and the mixture was dispersed by stirring. Then, 0.1 mol of N-(2-hydroxyethyl)ethylenediamine was added thereto, and the mixture was reacted at 35° C. for 6 h. After the reaction was completed, the mixture was distilled under reduced pressure to obtain Intermediate 1.
[0051] (2) 0.25 mol of cyanamide was added to 200 mL of isopropanol solvent, and the mixture was stirred and dispersed. 5 mol / L hydrochloric acid was added to adjust the pH to 4, and then 0.2 mol of intermediate 1 was added to the mixture. The mixture was reacted at 15° C. for 8 h. After the reaction was completed, the mixture was distilled under reduced pressure to obtain intermediate 2.
[0052] (3) Under nitrogen conditions, 0.3 mol of intermediate 2 was added to 200 mL of tetrahydrofuran solvent, stirred and dispersed, and then 0.15 mol of phenylphosphonic dichloride and 0.39 mol of triethylamine were added thereto. The temperature was raised to 65° C. and the reaction was carried out for 24 h. After the reaction was completed, the mixture was filtered, rotary evaporated, washed with deionized water, and dried to obtain intermediate 3.
[0053] (4) 40 mmol of the intermediate 3 was added to 100 mL of deionized water, stirred and dispersed, and then 120 mmol of sodium hypochlorite was added thereto. The pH was adjusted to 7 with 0.4 mol / L sulfuric acid. The mixture was stirred and reacted at 25° C. for 2 h. After the reaction was completed, the mixture was centrifuged, washed with deionized water, and dried to obtain a guanidine-containing halogenamine phenyl phosphate.
[0054] (5) 20 g of thermoplastic polyurethane elastomer, 6 g of montmorillonite, and 1.6 g of guanidine-containing halogenamine phenyl phosphate are added to a high-speed mixer and mixed evenly. The mixture is added to a twin-screw extruder and extruded into granules. The temperatures of the three zones of the twin-screw extruder are 170° C., 180° C., and 175° C. Finally, the mixture is placed in a flat vulcanizer at 180° C. and 10 MPa for pressing to obtain an antibacterial modified thermoplastic polyurethane elastomer.
[0055] Comparative Example 1
[0056] The difference between this comparative example and Example 1 is that in step (5), intermediate 2 is used instead of guanidine-containing halogenamine phenyl phosphate.
[0057] Referring to GB / T2406, the LOI of the material was tested using a limiting oxygen index tester with a sample size of 75mm×6.5mm×3mm.
[0058] Refer to GB / T2408 and use a vertical combustion tester to test the vertical combustion grade of the material. The sample size is 125mm×13mm×3mm.
[0059] Table 1: Flame retardant performance test results of various embodiments and comparative examples
[0060]
[0061]
[0062] It can be seen from the table that the flame retardant effect of Examples 1-5 is better than that of Comparative Example 1. This is because Examples 1-5 contain guanidine-containing halogenamine phenyl phosphate, and the phosphorus element contained in the guanidine-containing halogenamine phenyl phosphate has a good flame retardant effect. Adding it to the thermoplastic elastomer can increase the flame retardant effect of the elastomer, while Comparative Example 1 does not contain such a substance, so its flame retardant effect is not as good as that of Examples 1-5.
[0063] Antibacterial test: Use a sterile cotton swab to scrape Staphylococcus aureus and Escherichia coli, place them in pH = 7.0 sodium chloride-peptone buffer, and use a sterile cotton swab to dip into 6×10 6 cfu / mL of bacterial suspension was evenly spread on the surface of tryptic soy agar medium plate, and a sample with a diameter of 5 mm was placed on the stained plate in the center of the plate. The plate was covered and cultured in an incubator at 32°C for 24 hours. After the culture was completed, the diameter of the inhibition ring was measured with a vernier caliper.
[0064] Table 2: Antibacterial performance test results of various embodiments and comparative examples
[0065]
[0066]
[0067] Comparative Example 2 is pure thermoplastic polyurethane elastomer.
[0068] As can be seen from the table, the antibacterial performance test results of Examples 1-5 and Comparative Example 1 are better than those of Comparative Example 2. This is because Examples 1-5 and Comparative Example 1 contain guanidine structures and halamine structures, which are antibacterial structures. Therefore, adding them to thermoplastic polyurethane can increase the antibacterial performance of the thermoplastic polyurethane elastomer. Therefore, the thermoplastic polyurethane elastomer prepared by the present invention has excellent antibacterial effect.
[0069] The above-mentioned embodiments only express several implementation methods of the present invention, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the invention patent. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, and these all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.
Claims
1. A method for preparing an antibacterial modified thermoplastic polyurethane elastomer, characterized in that: The preparation method is as follows: Thermoplastic polyurethane elastomer, montmorillonite, and guanidine-containing halogenamine phenyl phosphate are added to a high-speed mixer and mixed evenly. The mixture is added to a twin-screw extruder, extruded into granules, and finally placed in a flat vulcanizer at 180° C. and 10 MPa for pressing to obtain an antibacterial modified thermoplastic polyurethane elastomer.
2. The method for preparing the antibacterial modified thermoplastic polyurethane elastomer according to claim 1, characterized in that: The temperatures of the three zones of the twin-screw extruder are 170°C, 180°C and 175°C.
3. The method for preparing the antibacterial modified thermoplastic polyurethane elastomer according to claim 1, characterized in that: The mass ratio of the thermoplastic polyurethane elastomer, montmorillonite and guanidine-containing halogenamine phenyl phosphate is 100:(15-30):(1-8).
4. The method for preparing the antibacterial modified thermoplastic polyurethane elastomer according to claim 1, characterized in that: The preparation method of the guanidine-containing halogenamine phenyl phosphate is as follows: (1) adding 1-hydroxymethyl-5,5-dimethylhydantoin to isopropanol solvent, stirring and dispersing, and then adding N-(2-hydroxyethyl)ethylenediamine thereto, reacting at 20-35° C. for 3-6 hours. After the reaction is completed, distilling under reduced pressure to obtain intermediate 1; (2) adding cyanamide to isopropanol solvent, stirring and dispersing, adding 2-5 mol / L hydrochloric acid to adjust the pH to 4-5, then adding intermediate 1 to the solvent, reacting at 10-25° C. for 8-16 hours, and after the reaction is completed, distilling under reduced pressure to obtain intermediate 2; (3) Under nitrogen conditions, the intermediate 2 is added to tetrahydrofuran solvent, stirred and dispersed, and then phenylphosphonic acid dichloride and triethylamine are added thereto, the temperature is raised to 60-70° C., and the reaction is carried out for 20-36 hours. After the reaction is completed, the intermediate 3 is filtered, rotary evaporated, washed with deionized water, and dried to obtain the intermediate 3; (4) Add the intermediate 3 to deionized water, stir and disperse, then add sodium hypochlorite, adjust the pH to 7-8 with 0.4 mol / L sulfuric acid, stir and react at 20-35° C. for 3-6 h. After the reaction is completed, centrifuge, wash with deionized water, and dry to obtain guanidine-containing halogenamine phenyl phosphate.
5. The method for preparing the antibacterial modified thermoplastic polyurethane elastomer according to claim 4, characterized in that: In the step (1), the molar ratio of 1-hydroxymethyl-5,5-dimethylhydantoin to N-(2-hydroxyethyl)ethylenediamine is 1:(1-1.2).
6. The method for preparing the antibacterial modified thermoplastic polyurethane elastomer according to claim 4, characterized in that: In the step (2), the molar ratio of cyanamide to intermediate 1 is (1-1.5):
1.
7. The method for preparing the antibacterial modified thermoplastic polyurethane elastomer according to claim 4, characterized in that: In the step (3), the molar ratio of intermediate 2, phenylphosphonic dichloride and triethylamine is (2-3):1:(2.2-2.6).
8. The method for preparing the antibacterial modified thermoplastic polyurethane elastomer according to claim 4, characterized in that: In the step (4), the molar ratio of the intermediate 3 to sodium hypochlorite is 1:(2.5-4).
Citation Information
Patent Citations
Hydroxy halogen amine compound containing quaternary ammonium salt functional group and preparation method and application thereof
CN102786477A
Antibacterial halamine derivative modified acrylic fiber and preparation method thereof
CN114214749A
Bentonite-loaded antibacterial agent and application thereof in antibacterial fibers
CN117265683A
Preparation method of flame-retardant bio-based thermoplastic polyurethane elastomer
CN118047926A
Thermoplastic polyurethane antibacterial mildew-proof master batch as well as preparation method and preparation device thereof
CN118146627A
Cited By
Polyurethane hot melt adhesive powder as well as preparation method and application thereof
CN119823698A
Polyurethane hot melt adhesive powder and preparation method and application thereof
CN119823698B