Metal organic framework / zinc piperazine pyrophosphate flame retardant, flame-retardant master batch and application

By combining UIO-66 with piperazine pyrophosphate zinc and preparing flame retardant masterbatch, the agglomeration problem of piperazine pyrophosphate metal salt in polymer matrix is ​​solved, and its good dispersion and flame retardant properties in PA6 materials are achieved. Improvement.

CN119019853AActive Publication Date: 2024-11-26QINGYUAN CITY YICHENG FLAME RETARDANT MATERIALS

Patent Information

Application Number
CN202411120165.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-15
Publication Date
2024-11-26
Estimated Expiration
2044-08-15

AI Technical Summary

Technical Problem

Piperazine pyrophosphate metal salt is prone to agglomeration in polymer matrix, resulting in poor dispersion and affecting its application in polymers.

Method used

The combination of UIO-66 and piperazine pyrophosphate zinc is used to adjust its mass ratio in the base material, improve the dispersion performance of piperazine pyrophosphate zinc, and achieve better dispersion effect by preparing flame retardant masterbatches.

Benefits of technology

通过UIO-66与焦磷酸哌嗪锌的组合,显著降低了焦磷酸哌嗪锌的团聚性,提高了其在PA6材料中的分散性能,并提升了材料的阻燃性能和结构强度。

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119019853A_ABST
    Figure CN119019853A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of flame retardance, and discloses a metal organic framework / zinc piperazine pyrophosphate flame retardant which comprises UIO-66 and zinc piperazine pyrophosphate. The mass ratio of the UIO-66 to the zinc piperazine pyrophosphate is 5: (10-20). According to the flame retardant, UIO-66 and zinc piperazine pyrophosphate are adopted, and when UIO-66 and zinc piperazine pyrophosphate are added into a base material, the dispersing performance of zinc piperazine pyrophosphate can be improved, and the agglomeration performance can be reduced. Meanwhile, the invention also provides the flame-retardant master batch and application thereof.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of flame retardancy, and in particular relates to a metal organic framework / piperazine zinc pyrophosphate flame retardant, a flame retardant masterbatch and uses. Background Art

[0002] Piperazine pyrophosphate integrates flame retardant elements such as P, N, and C, and also functions as a carbon source, gas source, and acid source. It also has extremely high light stability and thermal stability, and a 5% decomposition temperature of over 300°C, which is suitable for the processing temperature of most resins. It can not only be used to flame retard PP, but also has good flame retardant effects on PE, ABS, EP, and PU, and is a halogen-free flame retardant with great market potential.

[0003] CN112778237A discloses a method for synthesizing piperazine pyrophosphate metal salt, which prepares piperazine pyrophosphate metal salt and is used to solve the problem that piperazine pyrophosphate is easy to absorb moisture and aggregate, and the problem that the dehydration is not complete and causes foaming during processing;

[0004] However, during the experiment, we found that piperazine pyrophosphate metal salts are also easy to agglomerate when dry. For example, "Research Progress on the Synthesis and Application of Piperazine Phosphate Flame Retardants" Engineering Plastics Applications, September 2020, written by Jin Feng et al., pointed out that there is a large polarity difference between piperazine phosphate and the polymer matrix, and there is a large charge interaction between piperazine phosphate powders, which are easy to agglomerate, resulting in poor dispersion of piperazine phosphate in polymers.

[0005] At the same time, we also found that piperazine pyrophosphate does not show obvious agglomeration when applied to a polymer matrix in a dry state.

[0006] That is to say, both piperazine pyrophosphate and piperazine pyrophosphate metal salt will agglomerate, but the former agglomerates under the condition of absorbing water, while the latter agglomerates in the polymer matrix.

[0007] The technical problem solved in this case is: how to reduce the agglomeration of metal piperazine pyrophosphate in a polymer matrix. Summary of the invention

[0008] In view of the shortcomings of the prior art, the purpose of the present invention is to provide a metal organic framework / piperazine zinc pyrophosphate flame retardant, which uses UIO-66 and piperazine zinc pyrophosphate. When the two are added to the base material, the dispersion performance of piperazine zinc pyrophosphate can be improved and the agglomeration performance can be reduced.

[0009] At the same time, the invention also provides flame retardant masterbatch and application.

[0010] To achieve the purpose of the invention, the present invention adopts the following technical scheme: a metal organic framework / piperazine zinc pyrophosphate flame retardant, including UIO-66 and piperazine zinc pyrophosphate; the mass ratio of UIO-66 to piperazine zinc pyrophosphate is 5:10-20.

[0011] In the above flame retardant, the mass ratio of UIO-66 to zinc piperazine pyrophosphate is 5:12-18.

[0012] Meanwhile, the invention also discloses a flame retardant masterbatch containing the flame retardant as described above.

[0013] In the above flame retardant masterbatch, the flame retardant masterbatch contains 30-50wt% of flame retardant.

[0014] The flame retardant masterbatch mentioned above also includes 0.1-0.5 wt% of a dispersant.

[0015] In the flame retardant masterbatch, the dispersant is sodium stearate, magnesium stearate or calcium stearate.

[0016] In the above-mentioned flame retardant masterbatch, the base material in the flame retardant masterbatch is PA6, PA66 or PA612.

[0017] In addition, the invention also discloses the use of UIO-66 to improve the dispersibility of zinc piperazine pyrophosphate in a base material.

[0018] Preferably, the base material is PA6, PA66 or PA612.

[0019] Compared with the prior art, the present invention has the following beneficial effects:

[0020] The present invention adopts UIO-66 and zinc piperazine pyrophosphate to be added to the base material, which can improve the dispersibility of zinc piperazine pyrophosphate and reduce the agglomeration performance;

[0021] After testing, it was found that by using about 5-7wt% of zinc pyrophosphate and matching UIO-66 in the PA6 substrate, the flame retardant performance of zinc pyrophosphate alone (the content in the substrate is 35wt%) can be achieved, and due to the reduction in the amount of zinc pyrophosphate, the structural strength of the PA6 material is also significantly improved. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 This is the XPS spectrum of UiO-66. DETAILED DESCRIPTION

[0023] The technical solution of the present invention is further described below by specific implementation methods. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention.

[0024] Part I

[0025] Synthesis of UiO-66

[0026] The synthesis process of UiO-66 is as follows: First, 1.98g ZrCl4 and 1.76g TPA are dissolved in 150mL anhydrous N, N-dimethylformamide (DMF), ultrasonicated for 20min, and then 4mL acetic acid is added for ultrasonication for 10min. The mixed solution is transferred to a blue bottle and placed in a 120℃ electric blast drying chamber. After removing the solvent for 36h, the powder is cooled to room temperature. Centrifuge at 6000r / min for 15min, filter the white precipitate, and wash it 3 times with DMF and ethanol. Finally, the white product is dried in a constant temperature vacuum drying tank at 85℃ for 36h to obtain UiO-66. The XPS spectrum of UiO-66 is shown below. Figure 1 As shown. Figure 1 In the figure, the meaning of each figure is: (a) overall spectrum; (b) C 1s; (c) O 1s; (d) Zr 3d.

[0027] Synthesis of Zinc Piperazine Pyrophosphate

[0028] It was prepared by the method of Example 3 of CN112778237A.

[0029] Part 2

[0030] Preparation of flame retardant masterbatch

[0031] Example 1

[0032] The flame retardant masterbatch is prepared by a twin-screw extrusion method. Specifically, the method is:

[0033] Step 1: drying zinc piperazine pyrophosphate, UiO-66, and PA6; the weight ratio of UiO-66, zinc piperazine pyrophosphate, PA6, and sodium stearate is 12.5:37:50:0.5;

[0034] Step 2: adding zinc piperazine pyrophosphate, UiO-66, PA6 and sodium stearate into a twin-screw extruder, setting the temperatures of each zone of the twin-screw extruder to 200°C, 230°C, 240°C, 250°C, 255°C, 255°C, 250°C, and 250°C, and setting the screw speed to 15-20r / min;

[0035] Step 3: Cut the extruded material into granules to obtain masterbatch.

[0036] Example 2

[0037] The method is substantially the same as Example 1, except that the weight ratio of UiO-66, zinc piperazine pyrophosphate, PA6, and sodium stearate is 10.5:40:50:0.5.

[0038] Example 3

[0039] The method is substantially the same as Example 1, except that the weight ratio of UiO-66, zinc piperazine pyrophosphate, PA6, and sodium stearate is 17:32.5:50:0.5.

[0040] Example 4

[0041] The method is substantially the same as Example 1, except that the weight ratio of UiO-66, zinc piperazine pyrophosphate, PA6, and sodium stearate is 10:30:59.5:0.5.

[0042] Example 5

[0043] The method is substantially the same as Example 1, except that the weight ratio of UiO-66, zinc piperazine pyrophosphate, PA6, and sodium stearate is 10:20:69.5:0.5.

[0044] Comparative Example 1

[0045] The method is substantially the same as Example 1, except that the raw materials are piperazine pyrophosphate, UiO-66, PA6, and sodium stearate;

[0046] The weight ratio of UiO-66, piperazine pyrophosphate, PA6, and sodium stearate is 12.5:37:50:0.5.

[0047] Part 3

[0048] Preparation of PA6 sheets

[0049] PA6 and the flame retardant masterbatch are heated and melted, and then injection molded to obtain a PA6 sheet having a specification of 12.7 cm*1.27 cm*0.32 cm; the formula is shown in Table 1 below;

[0050] Table 1 Recipe

[0051]

[0052]

[0053] In addition, the plates 7 and 8 are prepared by the following method:

[0054] Plate 7

[0055] PA6 and zinc piperazine pyrophosphate (after drying) are heated, melted and mixed, and then injection molded to obtain a PA6 sheet with a specification of 12.7 cm*1.27 cm*0.32 cm; the weight ratio of PA6 to zinc piperazine pyrophosphate is 65:35.

[0056] Plate 8

[0057] PA6 and piperazine pyrophosphate (after drying) are heated, melted and mixed, and then injection molded to obtain a PA6 sheet with a specification of 12.7 cm*1.27 cm*0.32 cm; the weight ratio of PA6 to piperazine pyrophosphate is 65:35.

[0058] Performance Testing

[0059] Test item 1: Physical properties of the board;

[0060] Test item 2: Flame retardant properties of the board, including vertical burning test and LOI test;

[0061] The test results are shown in Tables 1 and 2 below;

[0062] Table 1 Physical properties of sheet metal

[0063] sample Tensile strength(MPa) Elongation at break (%) Notched impact strength (kJ / m2) PA6 68.46 41.2 250.8 Plate 1 67.56 33.65 185.32 Plate 2 65.54 32.96 178.65 Plate 3 58.59 31.24 160.58 Plate 4 70.58 30.52 147.79 Plate 5 50.26 18.56 192.8 Plate 6 56.20 25.65 158.97 Plate 7 50.66 19.05 191.89 Plate 8 58.53 31.59 161.57

[0064] Table 2 Flame retardant properties of the board

[0065]

[0066]

[0067] Result analysis:

[0068] 1. From the perspective of the physical properties of the board, the structural strength of Boards 1 to 5 is weaker than that of PA6. This is expected because the addition of flame retardant materials will, in most cases, impair the strength of the board.

[0069] 2. Compared with Plate 1, Plate 6 has significantly lower elongation at break and notched impact strength. Compared with Plate 6, Plate 8 has slightly lower physical strength. The possible reasons are: referring to Plate 8 and Plate 1, piperazine pyrophosphate is used as the component of the masterbatch. Since it cannot be absolutely dry, it has slight agglomeration, which leads to its inability to achieve the optimal dispersion state in the matrix, and then leads to a certain degree of reduction in physical strength. By comparing Plate 6 and Plate 8, it can be inferred that UiO-66 does not improve the dispersibility of piperazine pyrophosphate in the system containing piperazine pyrophosphate, resulting in further reduction in physical strength. In Plate 1, the best dispersion is achieved by blending UiO-66 and zinc piperazine pyrophosphate. By pre-preparing it into a masterbatch, when the masterbatch is dispersed in the matrix, the zinc piperazine pyrophosphate can be better dispersed, so it is manifested as a relatively low weakening of structural strength.

[0070] 3. It can be seen from Plate 7 and Plate 8 that the agglomeration performance of zinc piperazine pyrophosphate in the PA6 substrate is more significant, and it can be seen from Plate 7 and Plate 1 that when a certain amount of UiO-66 is added, the physical properties of zinc piperazine pyrophosphate are significantly improved.

[0071] 4. From the perspective of flame retardant performance, there is no trend difference between sheets 1 and 8. There is one case worth noting, sheet 4 shows the best flame retardant performance. Whether from the perspective of the amount of zinc piperazine pyrophosphate or the amount of flame retardant masterbatch, it is not used the most or the least, and it shows excellent flame retardant performance. We speculate that it may be related to the ratio of materials in the masterbatch and the amount of masterbatch used in the sheet. Specifically: the amount of UiO-66 in the masterbatch should be between 10 and 12.5wt%, the amount of zinc piperazine pyrophosphate should be between 30 and 40wt%, and the amount of masterbatch in the sheet should not exceed 20wt%.

[0072] In practical applications, the comprehensive performance cannot be determined solely by flame retardancy. After comprehensive analysis, we believe that Plate 1 and Plate 2 represent the best material usage choices.

Claims

1. A metal organic framework / piperazine zinc pyrophosphate flame retardant, characterized in that: The invention comprises UIO-66 and zinc piperazine pyrophosphate; the mass ratio of the UIO-66 to the zinc piperazine pyrophosphate is 5:10-20.

2. The flame retardant according to claim 1, characterized in that The mass ratio of UIO-66 to zinc piperazine pyrophosphate is 5:12-18.

3. A flame retardant masterbatch, characterized in that: Contains the flame retardant as claimed in claim 1 or 2.

4. The flame retardant masterbatch according to claim 3, characterized in that: The flame retardant masterbatch contains 30-50wt% of flame retardant.

5. The flame retardant masterbatch according to claim 3, characterized in that: Also included is 0.1-0.5 wt% of a dispersant.

6. The flame retardant masterbatch according to claim 3, characterized in that: The dispersant is sodium stearate, magnesium stearate or calcium stearate.

7. The flame retardant masterbatch according to claim 3, characterized in that: The base material in the flame retardant masterbatch is PA6, PA66 or PA612.

8. Use of UIO-66 to improve the dispersibility of zinc piperazine pyrophosphate in base materials.

9. The use according to claim 8, characterized in that The base material is PA6, PA66 or PA612.

Citation Information

Patent Citations

  • Flame-retardant polyolefin resin containing piperazine-based metal salt blend

    CN103547625A

  • Synthesis method of pyrophosphate piperazine metal salt

    CN112778237A

  • Intumescent flame retardant containing piperazine pyrophosphate and polyaminocyclotriphosphazene as well as preparation method and application of intumescent flame retardant

    CN116589860A

  • Novel fireproof material as well as preparation method and application thereof

    CN116925497A

  • Flame-retardant polyolefin resin containing piperazine-based metal salt blend

    US20130296467A1

Cited By

  • Piperazine pyrophosphate / MOF composite material stable at high temperature and preparation method thereof

    CN120484521A