Electrolyzed water diaphragm additive, electrolyzed water diaphragm and application of electrolyzed water diaphragm additive
By using hydrophobic high-stereostatic organic small molecule additives in alkaline electrolytic separators, the stability and uniformity of the separator under extreme alkaline liquid conditions are solved, and the alkali resistance and film formation are improved, and the use is extended. Lifespan and increased flux.
Patent Information
- Application Number
- CN202411138673.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-19
- Publication Date
- 2024-11-26
AI Technical Summary
The existing alkaline electrolytic separators have poor stability under extreme alkaline liquid conditions and insufficient dispersion and uniformity of the coating slurry, resulting in a degradation of membrane performance and short service life.
Using hydrophobic high-stereostatic organic small molecule electrolytic separator additives, such as tetraphenylhexafluorobisphenol A, promotes the dispersion and micro-phase separation of the coating slurry, forms a bicontinuous macropore structure, and improves the membrane in alkaline extreme conditions. stability under .
It significantly improves the alkali resistance and film formation of the electrolytic water separator, extends the service life, and improves the flux and stability of the film.
Smart Images

Figure CN119019883A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of water electrolysis, and in particular to a water electrolysis membrane additive, a water electrolysis membrane and applications thereof. Background Art
[0002] The demand for clean and renewable energy is increasing, and hydrogen energy, as a clean and efficient energy carrier, has received widespread attention. However, high-purity hydrogen is difficult to obtain directly from nature and needs to be prepared through different technical paths and production processes. Hydrogen production technology is the key to the development of hydrogen energy.
[0003] There are three main ways to produce hydrogen: hydrogen from fossil energy reforming, hydrogen from industrial byproduct gas, and hydrogen from water electrolysis. So far, hydrogen, as a raw material and intermediate product for chemical production, is mainly obtained through hydrogen production from fossil energy and industrial byproduct. Although the cost of hydrogen production from fossil energy and industrial byproduct is low, there is environmental pollution in the process of hydrogen production. Hydrogen production from water electrolysis can be powered by renewable electricity such as photovoltaic power generation, wind power, and hydropower, and can achieve zero carbon emissions during use, so it is called green hydrogen.
[0004] At present, the technologies for producing hydrogen by water electrolysis include alkaline water electrolysis, PEM (proton exchange membrane) water electrolysis, solid oxide water electrolysis and anion exchange membrane water electrolysis. Among them, alkaline water electrolysis is the most mature and earliest industrialized water electrolysis hydrogen production technology, which is characterized by low investment cost of electrolyzer, long service life and large-scale production capacity. Alkaline water electrolyzer is the main equipment of water electrolysis hydrogen production device, which consists of multiple electrolytic cells. Each electrolytic cell includes an anode, a cathode, a diaphragm and an electrolyte. In order to ensure the purity of the gas produced by electrolysis and the safety of the electrolytic cell, the diaphragm is required to have good stability under extreme alkaline conditions, and its existence must allow the ions in the solution to migrate freely between the cathode and the anode. The quality of the diaphragm is directly related to the service life of the electrolyzer, the purity of hydrogen, the energy consumption of electrolysis and the safety.
[0005] At present, the technical means for producing alkaline water electrolysis membranes is usually to prepare composite membranes by coating slurry on both sides of the membrane. However, the main disadvantages of this method are: (1) the coating slurry without additives cannot be fully dispersed, and thus the uniformity of the membrane cannot be guaranteed; (2) during the subsequent stability test, the coating slurry will fall off significantly on the surface of the membrane. Summary of the invention
[0006] The present invention is based on the inventors' discovery and understanding of the following facts and problems: At present, the defects of additives contained in coating slurries include: (1) the additives themselves are mostly inorganic substances and are almost insoluble in polar solvents. They cannot promote dispersion during the preparation of the slurry, and thus cannot ensure membrane uniformity; (2) during the phase separation process of the steam-induced phase separation (VIPS) method, high-temperature and high-humidity steam is used, mainly non-solvents, to induce phase separation. Some low-steric hindrance additives are easily oxidized and denatured during this period of time, which leads to a decrease in membrane performance.
[0007] The present invention aims to solve one of the technical problems in the related art at least to a certain extent. To this end, the embodiments of the present invention provide an electrolytic water diaphragm additive, an electrolytic water diaphragm and its application, which can improve the stability of the membrane under alkaline extreme conditions, effectively promote the dispersion of the coating slurry, promote the microphase separation of the coating slurry, and then form a bicontinuous macroporous structure, so as to prepare an alkaline electrolytic water diaphragm with excellent alkali resistance and film-forming properties.
[0008] An embodiment of the present invention provides an electrolytic water diaphragm additive, including at least one of tetraphenyl hexafluorobisphenol A, tetrakis(3',5'-bistrifluoromethyl)phenyl hexafluorobisphenol A, tetrakis(3'-trifluoromethyl)phenyl hexafluorobisphenol A, tetrakis(4'-trifluoromethyl)phenyl hexafluorobisphenol A, tetrakis(4'-tert-butyl)phenyl hexafluorobisphenol A or tetrakis(3',5'-di-tert-butyl)phenyl hexafluorobisphenol A.
[0009] Advantages and technical effects brought by the electrolytic water diaphragm additive of the embodiment of the present invention: the electrolytic water diaphragm additive is a hydrophobic high steric hindrance organic small molecule, which is compatible with polar organic solvents, can effectively promote the dispersion of the coating slurry, and ensure the uniformity of the coating. By virtue of the special chemical structure of the high steric hindrance additive and its own excellent chemical stability, it can reduce the performance loss of the membrane under alkaline extreme conditions, and the stability of the electrolytic water diaphragm in alkaline solution is greatly improved, and it can be used for alkaline electrolysis of water. Organic high steric hindrance small molecules are selected as additives to ensure their compatibility with polar organic solvents. At the same time, due to their hydrophobicity, capillary penetration can be formed between the coating slurry and the separator, slowly promoting the microphase separation of the coating slurry, and then forming a bicontinuous macroporous structure, which is beneficial to improve the flux of the electrolytic water diaphragm. The electrolytic water diaphragm additive of the present invention can be used to prepare an alkaline electrolytic water diaphragm with excellent alkali resistance and film-forming properties.
[0010] The embodiment of the present invention provides a method for preparing an electrolytic water diaphragm additive, wherein tetrabromohexafluorobisphenol A and a phenylboric acid compound are reacted under the catalysis of a catalyst to obtain the electrolytic water diaphragm additive;
[0011] The phenylboronic acid compound includes at least one of phenylboric acid, 4-tert-butylphenylboric acid, 3,5-di-tert-butylphenylboric acid, 3,5-bis(trifluoromethyl)phenylboric acid, 3-(trifluoromethyl)phenylboric acid and 4-(trifluoromethyl)phenylboric acid.
[0012] In some embodiments, the molar ratio of tetrabromohexafluorobisphenol A to phenylboronic acid compound is 1:4.1-4.5;
[0013] And / or, the reaction temperature is 90-140°C;
[0014] And / or, the reaction time is 6-24h.
[0015] In some embodiments, the catalyst comprises a base and a palladium catalyst; preferably, the base comprises at least one of potassium carbonate, sodium carbonate, potassium hydroxide, sodium hydroxide, cesium carbonate or sodium bicarbonate; the palladium catalyst comprises at least one of tetrakis(triphenylphosphine)palladium, (2-dicyclohexylphosphine-2′,6′-diisopropyl-1,1′-biphenyl)[2-(2-aminoethyl)phenyl)]palladium(II), chloro[(di-tert-butylneopentylphosphine)-2-(2-aminobiphenyl)]palladium(II), methanesulfonate-2-dicyclohexylphosphine-2′-methylbiphenyl(2-amino-1,1′-biphenyl-2-yl)palladium(II), [N-[2-(di-1-adamantane)phosphinophenyl]morpholine](4-trifluoromethylphenyl)trifluoromethanesulfonate palladium or [n-butyldi(1-adamantyl)phosphine](4-trifluoromethylphenyl)palladium bromide dimer.
[0016] In some embodiments, the molar ratio of tetrabromohexafluorobisphenol A, base and palladium catalyst is 1:4.1-4.5:0.02-0.08.
[0017] The embodiment of the present invention provides an electrolytic water diaphragm coating slurry, including the electrolytic water diaphragm additive described in the embodiment of the present invention or the electrolytic water diaphragm additive prepared by the preparation method described in the embodiment of the present invention. In the embodiment of the present invention, the electrolytic water diaphragm coating slurry has all the advantages of the electrolytic water diaphragm additive, which will not be repeated here.
[0018] In some embodiments, it also includes high molecular organic matter, inorganic nanomaterials and solvents;
[0019] And / or, the mass percentage of the electrolytic water membrane additive in the electrolytic water membrane coating slurry is 0.1-1%.
[0020] In some embodiments, the high molecular organic material includes at least one of polysulfone, polyethersulfone or polyphenylsulfone;
[0021] And / or, the inorganic nanomaterial includes at least one of zirconium oxide, titanium dioxide, barium sulfate and barium titanate;
[0022] And / or, the solvent comprises at least one of DMF, DMAC, NMP, and DMSO;
[0023] And / or, further comprising a porogen; the porogen comprises at least one of polyvinyl pyrrolidone, polyethylene glycol, glycerol, acetone, ethanol, and ethylene glycol monomethyl ether.
[0024] An embodiment of the present invention provides an electrolytic water membrane, comprising the electrolytic water membrane additive described in the embodiment of the present invention, or comprising a separator and a coating layer, wherein the coating layer is obtained by coating the electrolytic water membrane coating slurry described in the embodiment of the present invention on the surface of the separator.
[0025] In the embodiment of the present invention, the electrolytic water membrane has excellent alkali resistance and film-forming properties. Relying on the special chemical structure of the high steric hindrance electrolytic water membrane additive and its own excellent chemical stability, the performance loss of the membrane under extreme alkaline conditions can be reduced, and the stability of the electrolytic water membrane in alkaline solution is greatly improved. The electrolytic water membrane additive is a hydrophobic high steric hindrance organic small molecule, which is compatible with polar organic solvents, can effectively promote the dispersion of the coating slurry and improve the uniformity of the membrane. The electrolytic water membrane additive allows capillary penetration to be formed between the coating slurry and the separator, slowly promotes the microphase separation of the coating slurry, and then forms a bicontinuous macroporous structure, which is beneficial to improve the flux of the electrolytic water membrane.
[0026] In some embodiments, the coating layer has a thickness of 200-600 μm.
[0027] The embodiment of the present invention provides a method for preparing an electrolytic water membrane, comprising: coating the electrolytic water membrane coating slurry on both sides of the separator, performing phase separation by steam induced phase separation after coating, and then entering into a gel bath for coagulation and fixing to obtain the electrolytic water membrane.
[0028] In the embodiment of the present invention, an electrolytic water membrane additive is added to obtain an electrolytic water membrane through steam-induced phase separation and coagulation fixation. The electrolytic water membrane additive enables capillary penetration to be formed between the coating slurry and the separator, slowly promotes microphase separation of the coating slurry, and then forms a bicontinuous macroporous structure, which is beneficial to improve the flux of the electrolytic water membrane.
[0029] In some embodiments, the phase separation temperature is 25-80°C;
[0030] and / or, the relative humidity of the phase separation is 10-90%;
[0031] And / or, the phase separation time is 5s-1min;
[0032] And / or, the temperature of the solidification is 15-80°C;
[0033] And / or, the solidification time is 5-45 minutes.
[0034] The embodiment of the present invention provides an application of an electrolytic water membrane additive or an electrolytic water membrane coating slurry or an electrolytic water membrane for alkaline electrolysis of water. In the embodiment of the present invention, the electrolytic water membrane additive improves the stability of the membrane in alkaline solution.
[0035] The embodiment of the present invention provides an alkaline water electrolysis device, including a water electrolysis membrane additive or a water electrolysis membrane. In the embodiment of the present invention, the water electrolysis membrane additive improves the stability and service life of the alkaline water electrolysis device. BRIEF DESCRIPTION OF THE DRAWINGS
[0036] Figure 1 It is a synthesis route of the electrolytic water diaphragm additive of the present invention.
[0037] Figure 2 It is the structure and name of the electrolytic water diaphragm additive of the present invention.
[0038] Figure 3 This is the two-side pore structure of the alkaline water electrolysis membrane in Example 1.
[0039] Figure 4 This is the NMR spectrum of tetrakis(3',5'-di-tert-butyl)phenylhexafluorobisphenol A in deuterated chloroform in Example 1.
[0040] Figure 5 This is the NMR spectrum of tetrakis(4'-trifluoromethyl)phenylhexafluorobisphenol A in deuterated dimethyl sulfoxide in Example 2.
[0041] Figure 6 This is the NMR spectrum of tetraphenylhexafluorobisphenol A in Example 3.
[0042] Figure 7 This is the NMR spectrum of tetrakis(3',5'-bistrifluoromethyl)phenylhexafluorobisphenol A in Example 4. DETAILED DESCRIPTION
[0043] Embodiments of the present invention are described in detail below, and examples of the embodiments are shown in the accompanying drawings. The embodiments described below with reference to the accompanying drawings are exemplary and intended to be used to explain the present invention, but should not be understood as limiting the present invention.
[0044] An electrolytic water diaphragm additive according to an embodiment of the present invention includes at least one of tetraphenyl hexafluorobisphenol A, tetrakis(3',5'-bistrifluoromethyl)phenyl hexafluorobisphenol A, tetrakis(3'-trifluoromethyl)phenyl hexafluorobisphenol A, tetrakis(4'-trifluoromethyl)phenyl hexafluorobisphenol A, tetrakis(4'-tert-butyl)phenyl hexafluorobisphenol A or tetrakis(3',5'-di-tert-butyl)phenyl hexafluorobisphenol A.
[0045] The electrolytic water diaphragm additive of the embodiment of the present invention is a hydrophobic high steric hindrance organic small molecule, which is compatible with polar organic solvents, can effectively promote the dispersion of the coating slurry, and ensure the uniformity of the coating. By virtue of the special chemical structure of the high steric hindrance additive and its own excellent chemical stability, the performance loss of the membrane under alkaline extreme conditions can be reduced, and the stability of the electrolytic water diaphragm in alkaline solution is greatly improved, and it can be used for alkaline electrolysis of water. Organic high steric hindrance small molecules are selected as additives to ensure their compatibility with polar organic solvents. At the same time, due to their hydrophobicity, capillary penetration can be formed between the coating slurry and the separator, slowly promoting the microphase separation of the coating slurry, and then forming a bicontinuous macroporous structure, which is beneficial to improve the flux of the electrolytic water diaphragm. The electrolytic water diaphragm additive of the present invention can be used to prepare an alkaline electrolytic water diaphragm with excellent alkali resistance and film-forming properties.
[0046] like Figure 1 As shown, the preparation method of the electrolytic water diaphragm additive of the embodiment of the present invention is to react tetrabromohexafluorobisphenol A with a phenylboric acid compound (Ar1) under the catalysis of a catalyst to obtain the electrolytic water diaphragm additive;
[0047] The phenylboronic acid compound includes at least one of phenylboric acid, 4-tert-butylphenylboric acid, 3,5-di-tert-butylphenylboric acid, 3,5-bis(trifluoromethyl)phenylboric acid, 3-(trifluoromethyl)phenylboric acid and 4-(trifluoromethyl)phenylboric acid.
[0048] In some embodiments, Figure 1 As shown, the electrolytic water membrane additive has an Ar4 group, and the Ar4 includes at least one of phenyl, (3',5'-bistrifluoromethyl)phenyl, (3'-trifluoromethyl)phenyl, (4'-trifluoromethyl)phenyl, (4'-tert-butyl)phenyl or (3',5'-bis-tert-butyl)phenyl.
[0049] In some embodiments, the molar ratio of tetrabromohexafluorobisphenol A to phenylboronic acid compounds is 1:4.1-4.5, specifically, for example, 1:4.1, 1:4.2, 1:4.3, 1:4.4, 1:4.5.
[0050] In some embodiments, the reaction temperature is 90-140°C, specifically, for example, 90°C, 100°C, 110°C, 120°C, 130°C, 140°C; and / or the reaction time is 6-24h, specifically, for example, 6h, 9h, 12h, 15h, 18h, 21h, 24h.
[0051] In some embodiments, the catalyst includes a base (Ar3) and a palladium catalyst (Ar2); preferably, the base includes at least one of potassium carbonate, sodium carbonate, potassium hydroxide, sodium hydroxide, cesium carbonate or sodium bicarbonate; the palladium catalyst includes at least one of tetrakis(triphenylphosphine)palladium, (2-dicyclohexylphosphine-2′,6′-diisopropyl-1,1′-biphenyl)[2-(2-aminoethyl)phenyl)]palladium(II), chloro[(di-tert-butylneopentylphosphine)-2-(2-aminobiphenyl)]palladium(II), methanesulfonate-2-dicyclohexylphosphine-2′-methylbiphenyl(2-amino-1,1′-biphenyl-2-yl)palladium(II), [N-[2-(di-1-adamantane)phosphinophenyl]morpholine](4-trifluoromethylphenyl)trifluoromethanesulfonate palladium or [n-butyldi(1-adamantyl)phosphine](4-trifluoromethylphenyl)palladium bromide dimer. In the embodiments of the present invention, the base and the palladium catalyst can accelerate the reaction rate, which is beneficial to improving the yield of the final product.
[0052] In some embodiments, the molar ratio of tetrabromohexafluorobisphenol A, alkali and palladium catalyst is 1:4.1-4.5:0.02-0.08, specifically, 1:4.1-4.5 (e.g., 4.1, 4.2, 4.3, 4.4, 4.5):0.02-0.08 (e.g., 0.02, 0.03, 0.04, 0.05, 0.06, 0.07, 0.08). In the embodiments of the present invention, by adjusting the amount of alkali and palladium catalyst, the yield of the final product can be improved.
[0053] In some embodiments, the molar ratio of tetrabromohexafluorobisphenol A, phenylboric acid compound (Ar1), palladium catalyst (Ar2) and base (Ar3) is 1:4.1-4.5:0.02-0.08:4.1-4.5, specifically, 1:4.1-4.5 (e.g., 4.1, 4.2, 4.3, 4.4, 4.5):0.02-0.08 (e.g., 0.02, 0.03, 0.04, 0.05, 0.06, 0.07, 0.08):4.1-4.5 (e.g., 4.1, 4.2, 4.3, 4.4, 4.5).
[0054] In some embodiments, tetrabromohexafluorobisphenol A, phenylboric acid compounds, palladium catalysts and bases are dispersed in a solvent for reaction; optionally, the solvent includes dimethylformamide; optionally, the mass fraction of the organic raw material relative to the solvent is 5%-25%, specifically, for example, 5%, 10%, 15%, 20%, 25%; optionally, tetrabromohexafluorobisphenol A, phenylboric acid compounds and palladium catalysts are first dispersed in a solvent for dissolution, and then a base is added for reaction; optionally, the dissolution is carried out under a nitrogen atmosphere; and the dissolution is promoted by heating.
[0055] In some embodiments, the reaction is carried out under the protection of an inert gas. Optionally, the inert gas includes at least one of nitrogen or argon.
[0056] In some embodiments, after the reaction is completed, the temperature is lowered to room temperature, and the electrolytic water diaphragm additive is obtained by filtration, column chromatography and drying; optionally, drying is performed by oven drying.
[0057] An electrolytic water diaphragm coating slurry according to an embodiment of the present invention comprises the electrolytic water diaphragm additive according to an embodiment of the present invention or the electrolytic water diaphragm additive prepared by the preparation method according to an embodiment of the present invention. In the embodiment of the present invention, the electrolytic water diaphragm coating slurry has all the advantages of the electrolytic water diaphragm additive, which will not be described in detail here.
[0058] In some embodiments, the electrolyzed water membrane additive includes at least one of tetraphenyl hexafluorobisphenol A, tetrakis (3', 5'-bis trifluoromethyl) phenyl hexafluorobisphenol A, tetrakis (3'-trifluoromethyl) phenyl hexafluorobisphenol A, tetrakis (4'-trifluoromethyl) phenyl hexafluorobisphenol A, tetrakis (4'-tert-butyl) phenyl hexafluorobisphenol A or tetrakis (3', 5'-di-tert-butyl) phenyl hexafluorobisphenol A, such as Figure 2 As shown; the mass percentage of the electrolytic water diaphragm additive in the electrolytic water diaphragm coating slurry is 0.1-1%, specifically, for example, 0.1%, 0.2%, 0.3%, 0.4%, 0.5%, 0.6%, 0.7%, 0.8%, 0.9%, 1%. In the embodiment of the present invention, the content of the additive in the coating slurry is 0.1-1%, which can effectively balance the stability of the membrane and the performance of the electrolytic cell. When the content of the additive is too low, the additive does not significantly improve the stability of the membrane; when the content of the additive is too high, the performance of the electrolytic cell will decrease due to excessive hydrophobicity.
[0059] In some embodiments, it also includes high molecular organic matter, inorganic nanomaterials and solvents;
[0060] Optionally, the high molecular organic matter is an organic heat-resistant and alkali-resistant high molecular substance, and optionally, the high molecular organic matter includes at least one of polysulfone, polyethersulfone or polyphenylsulfone; optionally, the mass percentage of the high molecular organic matter in the electrolytic water diaphragm coating slurry is 10-30wt%, specifically, for example, 10wt%, 15wt%, 20wt%, 25wt%, 30wt%;
[0061] Optionally, the inorganic nanomaterial comprises at least one of zirconium oxide, titanium dioxide, barium sulfate, and barium titanate, preferably zirconium oxide; Optionally, the particle size of the inorganic nanomaterial is 30-50 nm, specifically, for example, 30 nm, 40 nm, 50 nm; the packing density of the inorganic nanomaterial is 0.3-0.7 g / ml; the mass percentage of the inorganic nanomaterial in the electrolytic water diaphragm coating slurry is 35-70 wt%, specifically, for example, 35 wt%, 40 wt%, 50 wt%, 60 wt%, 70 wt%;
[0062] Optionally, the solvent includes at least one of DMF, DMAC, NMP, and DMSO; optionally, the mass percentage of the solvent in the electrolytic water diaphragm coating slurry is 25%-50%, specifically, for example, 25wt%, 30wt%, 35wt%, 40wt%, 50wt%.
[0063] In the embodiment of the present invention, the slurry includes high molecular organic matter, inorganic nanomaterials and solvents. By adjusting the content of each component, it is advantageous to obtain a slurry with a viscosity suitable for coating. Adding an electrolyzed water diaphragm additive to prepare the coating slurry can ensure that the high molecular organic matter and the inorganic nanomaterials in the coating slurry are fully mixed, while ensuring that the membrane has a high stability in the alkaline solution.
[0064] In some embodiments, a porogen is further included; the porogen includes at least one of polyvinyl pyrrolidone, polyethylene glycol, glycerol, acetone, ethanol, and ethylene glycol monomethyl ether; optionally, the mass percentage of the porogen in the electrolytic water diaphragm coating slurry is 0-15%, specifically, for example, 0%, 0.1%, 1%, 3%, 5%, 7%, 10%, 12%, 15%. In the embodiment of the present invention, the porogen can form pores of different shapes, and by adjusting the content of the porogen, it is beneficial to control the pore size and distribution of the electrolytic water diaphragm.
[0065] A method for preparing a water electrolysis membrane coating slurry according to an embodiment of the present invention comprises: mixing various components to obtain the water electrolysis membrane coating slurry.
[0066] In some embodiments, the mixing is performed using planetary stirring.
[0067] In some embodiments, dissolution and degassing are performed after mixing. Optionally, the dissolution and degassing temperature is 80-120°C, optionally, 100°C.
[0068] A water electrolysis membrane according to an embodiment of the present invention comprises the water electrolysis membrane additive according to the embodiment of the present invention, or comprises a separator and a coating layer, wherein the coating layer is obtained by coating the water electrolysis membrane coating slurry according to the embodiment of the present invention on the surface of the separator, and optionally, coated on both sides of the separator.
[0069] In the embodiment of the present invention, the electrolytic water membrane has excellent alkali resistance and film-forming properties. Relying on the special chemical structure of the high steric hindrance electrolytic water membrane additive and its own excellent chemical stability, the performance loss of the membrane under extreme alkaline conditions can be reduced, and the stability of the electrolytic water membrane in alkaline solution is greatly improved. The electrolytic water membrane additive is a hydrophobic high steric hindrance organic small molecule, which is compatible with polar organic solvents, can effectively promote the dispersion of the coating slurry and improve the uniformity of the membrane. The electrolytic water membrane additive allows capillary penetration to be formed between the coating slurry and the separator, slowly promotes the microphase separation of the coating slurry, and then forms a bicontinuous macroporous structure, which is beneficial to improve the flux of the electrolytic water membrane.
[0070] In some embodiments, the thickness of the coating layer is 200-600 μm, specifically, for example, 200 μm, 250 μm, 300 μm, 400 μm, 500 μm, 600 μm, optionally, the thickness of the coating layer is the thickness of the coating layer on one side of the separator or the thickness of the coating layer on both sides; and / or, the mass percentage of the coating layer in the water electrolysis membrane is 40%-70%, specifically, for example, 40%, 50%, 60%, 70%.
[0071] In some embodiments, the separator includes at least one of polyphenylene sulfide or nylon, specifically, for example, a polyphenylene sulfide separator; optionally, the separator has a thickness of 250-300 μm.
[0072] In some embodiments, the electrolytic water membrane is a double-sided asymmetric structure; and / or, the electrolytic water membrane has a bicontinuous pore structure. In the embodiments of the present invention, the addition of the electrolytic water membrane additive allows capillary penetration to be formed between the coating slurry and the separator, slowly promoting the microphase separation of the coating slurry, and then forming a bicontinuous macroporous structure, which is beneficial to improving the flux of the electrolytic water membrane, rather than forming a discontinuous pore structure or a small pore structure.
[0073] A method for preparing a water electrolysis membrane according to an embodiment of the present invention comprises: coating the water electrolysis membrane coating slurry on both sides of the separator, performing phase separation by steam induced phase separation after coating, and then entering into a gel bath for coagulation and fixing to obtain the water electrolysis membrane.
[0074] In the embodiment of the present invention, an electrolytic water membrane additive is added to obtain an electrolytic water membrane through steam-induced phase separation and coagulation fixation. The electrolytic water membrane additive enables capillary penetration to be formed between the coating slurry and the separator, slowly promotes microphase separation of the coating slurry, and then forms a bicontinuous macroporous structure, which is beneficial to improve the flux of the electrolytic water membrane.
[0075] In some embodiments, the temperature of the phase separation is 25-80°C, specifically, for example, 25°C, 30°C, 40°C, 50°C, 60°C, 70°C, 80°C; and / or the relative humidity of the phase separation is 10-90%, specifically, for example, 10%, 20%, 30%, 40%, 50%, 60%, 70%, 80%, 85%, 90%; optionally, the relative humidity on one side is 10-90%, and the relative humidity on the other side is 10-90%, specifically, for example, 10%, 20%, 30%, 40%, 50%, 60%, 70%, 80%, 85%, 90%; and / or the time of the phase separation is 5s-1min, specifically, for example, 5s, 10s, 20s, 30s, 40s, 50s, 60s;
[0076] and / or, the setting temperature is 15-80°C, specifically, for example, 15°C, 30°C, 40°C, 50°C, 60°C, 70°C, 80°C; and / or, the setting time is 5-45min, specifically, for example, 5min, 10min, 15min, 20min, 30min, 40min, 45min; and / or, the coagulation bath used includes water, optionally, the gel bath uses water or a mixture of water and other solvents, optionally, the other solvents include at least one of methanol, ethanol or isopropanol; the volume concentration of the organic solvent in the mixture is 0%-40%, optionally, 30%;
[0077] Optionally, the film is rolled up after solidification and fixed, and cleaned offline; optionally, it is cleaned with hot water after solidification.
[0078] In the embodiment of the present invention, after coating is completed, the membrane enters the VIPS area, and the VIPS step is adjusted according to the surface pore size requirements, and then enters the gel bath for coagulation and shaping, and finally is rolled up and cleaned offline, which is conducive to the preparation of an alkaline electrolyzed water composite membrane with suitable thickness and pore size.
[0079] The application of an electrolytic water membrane additive or electrolytic water membrane coating slurry or electrolytic water membrane in the embodiment of the present invention is used for alkaline electrolysis of water. In the embodiment of the present invention, the electrolytic water membrane additive improves the stability of the membrane in alkaline solution. The electrolytic water membrane used for alkaline electrolysis of water is an alkaline electrolytic water membrane.
[0080] An alkaline water electrolysis device according to an embodiment of the present invention comprises a water electrolysis membrane additive or a water electrolysis membrane. In the embodiment of the present invention, the water electrolysis membrane additive improves the stability and service life of the alkaline water electrolysis device.
[0081] The present invention is described below with reference to specific embodiments. It should be noted that these embodiments are merely illustrative and do not limit the present invention in any way.
[0082] Example 1
[0083] Dissolve tetrabromohexafluorobisphenol A (1 eq), tetrakis(triphenylphosphine)palladium (0.04 eq) and 3,5-di-tert-butylphenylboronic acid (4.3 eq) in dimethylformamide (the mass fraction of organic raw materials relative to the solvent is 20%) in a nitrogen atmosphere, slightly heat until the substrate is completely dissolved, add potassium carbonate (4.5 eq), heat to 90°C, and continue the reaction for 16 hours. After the reaction is completed, cool to room temperature, filter, column chromatography, and dry to obtain tetrakis(3',5'-di-tert-butyl)phenylhexafluorobisphenol A, an electrolytic water diaphragm additive, whose NMR spectrum is as follows: Figure 4 shown.
[0084] The electrolytic water diaphragm coating slurry was prepared as follows: by mass: 13% polysulfone, 50% nano zirconium oxide (particle size 30nm), 1.5% glycerol, 0.5% tetrakis (3', 5'-di-tert-butyl) phenyl hexafluorobisphenol A and 35% NMP. Planetary stirring was used and the electrolytic water diaphragm coating slurry was dissolved and degassed at 100°C to obtain the electrolytic water diaphragm coating slurry that met the requirements.
[0085] The alkaline water electrolysis membrane was prepared according to the double slot-die method. The water electrolysis membrane coating slurry was applied to both sides of the PPS separator at the same time, with the coating film thickness of 250μm on one side and 250μm on the other side. After coating, it was placed in a closed area at 25℃, 85% and 25℃, 10% relative humidity, and phase separation was induced on both sides for 30s, then placed in a 60℃ water bath for gelation for 5min, and then washed with 80℃ hot water for 30min to obtain an alkaline water electrolysis membrane.
[0086] Comparative Example 1
[0087] The electrolytic water diaphragm coating slurry was prepared as follows: by mass: 10% polysulfone, 44% nano zirconium oxide (particle size 30nm), 1.5% glycerol, 0.5% inorganic additive calcium carbonate and 44% NMP. Planetary stirring was used and the electrolytic water diaphragm coating slurry was dissolved and degassed at 100°C to obtain the electrolytic water diaphragm coating slurry.
[0088] The alkaline water electrolysis membrane was prepared according to the double slot-die method. The water electrolysis membrane coating slurry was applied to both sides of the PPS separator at the same time, with the coating film thickness of 250μm on one side and 250μm on the other side. After coating, it was placed in a closed area at 25℃, 85% and 25℃, 10% relative humidity, and phase separation was induced on both sides for 30s, then placed in a 60℃ water bath for gelation for 5min, and then washed with 80℃ hot water for 30min to obtain an alkaline water electrolysis membrane.
[0089] Example 2
[0090] Tetrabromohexafluorobisphenol A (1 eq), methanesulfonic acid-2-dicyclohexylphosphino-2'-methylbiphenyl (2-amino-1,1'-biphenyl-2-yl) palladium (II) (0.02 eq) and 4-(trifluoromethyl)phenylboronic acid (4.15 eq) were dissolved in an organic solvent dimethylformamide (the mass fraction of the organic raw material relative to the solvent was 10%) in a nitrogen atmosphere, and the temperature was slightly raised until the substrate was completely dissolved, potassium carbonate (4.1 eq) was added, and the mixture was heated to 90°C and the reaction was continued for 16 hours. After the reaction was completed, the mixture was cooled to room temperature, filtered, column chromatographed, and dried to obtain tetrakis(4'-trifluoromethyl)phenylhexafluorobisphenol A, an electrolytic water diaphragm additive, whose NMR spectrum is shown in the following figure. Figure 5 shown.
[0091] The electrolytic water diaphragm coating slurry was prepared as follows: by mass: 17% polysulfone, 44% nano zirconium oxide (particle size 30nm), 2.5% glycerol, 0.5% tetrakis (4'-trifluoromethyl) phenyl hexafluorobisphenol A and 36% NMP. Planetary stirring was used and the electrolytic water diaphragm coating slurry was dissolved and degassed at 100°C to obtain the electrolytic water diaphragm coating slurry that met the requirements.
[0092] The alkaline water electrolysis membrane was prepared according to the double slot-die method. The water electrolysis membrane coating slurry was applied to both sides of the PPS separator at the same time, with the coating film thickness of 250μm on one side and 250μm on the other side. After coating, it was placed in a closed area at 25℃, 45% and 25℃, 10% relative humidity, and phase separation was induced on both sides for 30s, then placed in a 60℃ water bath for gelation for 5min, and then washed with 80℃ hot water for 30min to obtain an alkaline water electrolysis membrane.
[0093] Comparative Example 2
[0094] The electrolytic water diaphragm coating slurry was prepared according to the following concentrations, by mass: 17% polysulfone, 44% zirconium oxide (particle size 30nm), 2.5% glycerol, 0.5% low steric additive tetrabutyl titanate, 36% NMP, and planetary stirring was used to dissolve and degas at 100°C to obtain the electrolytic water diaphragm coating slurry.
[0095] The alkaline water electrolysis membrane was prepared by the double slot-die method. The water electrolysis membrane coating slurry was applied to both sides of the PPS separator at the same time, with the coating film thickness of 250μm on one side and 250μm on the other side. After coating, it was placed in a closed area at 25℃, 45% and 25℃, 10% relative humidity, and phase separation was induced on both sides for 30s, then placed in a 60℃ water bath for gelation for 5min, and then washed with 80℃ hot water for 30min to obtain an alkaline water electrolysis membrane.
[0096] Example 3
[0097] The preparation method of the alkaline water electrolysis membrane is the same as that of Example 1, except that the additive tetrakis (3', 5'-di-tert-butyl) phenyl hexafluorobisphenol A is replaced by tetraphenyl hexafluorobisphenol A. The NMR spectrum of tetraphenyl hexafluorobisphenol A is as follows: Figure 6 shown.
[0098] Example 4
[0099] The preparation method of the alkaline electrolyzed water membrane is the same as that of Example 1, except that the additive tetrakis(3',5'-di-tert-butyl)phenylhexafluorobisphenol A is replaced by tetrakis(3',5'-bistrifluoromethyl)phenylhexafluorobisphenol A. The nuclear magnetic spectrum of tetrakis(3',5'-bistrifluoromethyl)phenylhexafluorobisphenol A is as follows: Figure 7 shown.
[0100] Example 5
[0101] The preparation method of the alkaline water electrolysis membrane is the same as that of Example 1, except that the additive tetrakis(3',5'-di-tert-butyl)phenylhexafluorobisphenol A is replaced by tetrakis(3'-trifluoromethyl)phenylhexafluorobisphenol A.
[0102] Example 6
[0103] The preparation method of the alkaline water electrolysis membrane is the same as that of Example 1, except that the additive tetrakis(3',5'-di-tert-butyl)phenylhexafluorobisphenol A is replaced by tetrakis(4'-tert-butyl)phenylhexafluorobisphenol A.
[0104] The viscosity of the coating slurry and the mass loss of the alkaline electrolytic water membrane in the alkaline solution of all the embodiments and comparative examples are shown in Table 1. The viscosity of the coating slurry at a rotation speed of 1 rpm was tested using a lamina viscometer. The mass loss of the alkaline electrolytic water membrane was tested after being immersed in a KOH solution at 120°C and 1.5 MPa for 15 days.
[0105] Table 1
[0106]
[0107] It can be seen from Table 1 that the viscosity of the coating slurry of Examples 1-6 is in the range of 700000-800000 mPa·s, and the viscosity of the coating slurry of Examples 1-6 is much higher than that of the coating slurry of Comparative Examples 1 and 2. This is because the high steric hindrance additive of the present invention has low solubility itself and has a certain bonding effect, thereby changing the fluidity of the entire slurry. The viscosity is controlled at 700000-800000 mPa·s, which is conducive to coating a water electrolysis diaphragm with a suitable pore size on the production line.
[0108] The alkaline water electrolysis membranes of Examples 1-6 use the high steric hindrance additive of the present invention, and the mass loss in the alkali solution is less than 0.6%, which is much lower than the mass loss of the membrane using the inorganic additive calcium carbonate in Comparative Example 1 and the membrane using the low steric hindrance additive tetrabutyl titanate in Comparative Example 2. This is because after adding the electrolytic water membrane additive of the present invention, the inorganic nanomaterial zirconium oxide has good dispersibility in the slurry, avoiding the unevenness of the film and the shedding of zirconium oxide during the test, and preparing an alkaline water electrolysis membrane with excellent alkali resistance, stability and film-forming properties. In Comparative Example 1, the inorganic additive calcium carbonate is used. Calcium carbonate is insoluble in the solvent and cannot play a role in promoting dispersion in the process of configuring the slurry, and the uniformity of the membrane cannot be guaranteed. The mass loss in the alkali solution is as high as 4.63%. In Comparative Document 2, the low steric hindrance additive tetrabutyl titanate is used, and the mass loss in the alkali solution is as high as 3.77%.
[0109] Figure 3 This is an electron microscope image of the alkaline water electrolysis membrane prepared in Example 1, with the dense surface on the left and the macroporous surface on the right. It can be seen that the alkaline water electrolysis membrane containing the water electrolysis membrane additive of the present invention has a sponge-like pore structure and presents a bicontinuous phase morphology, which is beneficial to improving the flux of the water electrolysis membrane.
[0110] In the present invention, the terms "one embodiment", "some embodiments", "examples", "specific examples", or "some examples" etc. mean that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representations of the above terms do not necessarily refer to the same embodiment or example. Moreover, the described specific features, structures, materials or characteristics may be combined in any one or more embodiments or examples in a suitable manner. In addition, those skilled in the art may combine and combine the different embodiments or examples described in this specification and the features of the different embodiments or examples, without contradiction.
[0111] Although the above embodiments have been shown and described, it is to be understood that the above embodiments are exemplary and are not to be construed as limitations on the present invention. Changes, modifications, substitutions and variations of the above embodiments by those of ordinary skill in the art are all within the scope of protection of the present invention.
Claims
1. An electrolytic water membrane additive, characterized in that: The invention comprises at least one of tetraphenyl hexafluorobisphenol A, tetrakis(3',5'-bistrifluoromethyl)phenyl hexafluorobisphenol A, tetrakis(3'-trifluoromethyl)phenyl hexafluorobisphenol A, tetrakis(4'-trifluoromethyl)phenyl hexafluorobisphenol A, tetrakis(4'-tert-butyl)phenyl hexafluorobisphenol A or tetrakis(3',5'-di-tert-butyl)phenyl hexafluorobisphenol A.
2. A method for preparing the electrolytic water diaphragm additive according to claim 1, characterized in that: Tetrabromohexafluorobisphenol A and phenylboric acid compounds are reacted under the catalysis of a catalyst to obtain an electrolytic water diaphragm additive; The phenylboronic acid compound includes at least one of phenylboric acid, 4-tert-butylphenylboric acid, 3,5-di-tert-butylphenylboric acid, 3,5-bis(trifluoromethyl)phenylboric acid, 3-(trifluoromethyl)phenylboric acid and 4-(trifluoromethyl)phenylboric acid.
3. The preparation method of the electrolytic water diaphragm additive according to claim 2, characterized in that: The molar ratio of tetrabromohexafluorobisphenol A to phenylboronic acid compound is 1:4.1-4.5; And / or, the reaction temperature is 90-140°C; And / or, the reaction time is 6-24h.
4. The method for preparing the electrolytic water membrane additive according to claim 2, characterized in that: The catalyst includes a base and a palladium catalyst; The base includes at least one of potassium carbonate, sodium carbonate, potassium hydroxide, sodium hydroxide, cesium carbonate or sodium bicarbonate; The palladium catalyst includes at least one of tetrakis(triphenylphosphine)palladium, (2-dicyclohexylphosphine-2′,6′-diisopropyl-1,1′-biphenyl)[2-(2-aminoethyl)phenyl)]palladium(II), chloro[(di-tert-butylneopentylphosphine)-2-(2-aminobiphenyl)]palladium(II), methanesulfonate-2-dicyclohexylphosphine-2′-methylbiphenyl(2-amino-1,1′-biphenyl-2-yl)palladium(II), [N-[2-(di-1-adamantane)phosphinophenyl]morpholine](4-trifluoromethylphenyl)trifluoromethanesulfonate palladium or [n-butyldi(1-adamantyl)phosphine](4-trifluoromethylphenyl)palladium bromide dimer.
5. The method for preparing the electrolytic water diaphragm additive according to claim 4, characterized in that: The molar ratio of tetrabromohexafluorobisphenol A, alkali and palladium catalyst is 1:4.1-4.5:0.02-0.
08.
6. A slurry for coating an electrolytic water diaphragm, characterized in that: The invention comprises the electrolytic water diaphragm additive according to claim 1 or the electrolytic water diaphragm additive prepared by the preparation method according to any one of claims 2 to 5.
7. The electrolytic water diaphragm coating slurry according to claim 6, characterized in that: It also includes high molecular organic matter, inorganic nanomaterials and solvents; And / or, the mass percentage of the electrolytic water membrane additive in the electrolytic water membrane coating slurry is 0.1-1%.
8. The electrolytic water diaphragm coating slurry according to claim 7, characterized in that: The macromolecular organic matter comprises at least one of polysulfone, polyethersulfone or polyphenylsulfone; And / or, the inorganic nanomaterial includes at least one of zirconium oxide, titanium dioxide, barium sulfate and barium titanate; And / or, the solvent comprises at least one of DMF, DMAC, NMP, and DMSO; And / or, further comprising a porogen; the porogen comprises at least one of polyvinyl pyrrolidone, polyethylene glycol, glycerol, acetone, ethanol, and ethylene glycol monomethyl ether.
9. A water electrolysis membrane, characterized in that: It comprises the electrolytic water diaphragm additive according to claim 1, or comprises a separator and a coating layer, wherein the coating layer is obtained by coating the electrolytic water diaphragm coating slurry according to any one of claims 6 to 8 on the surface of the separator.
10. The water electrolysis membrane according to claim 9, characterized in that: The coating layer has a thickness of 200-600 μm.
11. A method for preparing a water electrolysis membrane according to claim 9 or 10, characterized in that: include: The electrolytic water diaphragm coating slurry is coated on both sides of the separator, and after coating, the phases are separated by a steam-induced phase separation method, and then the slurry enters a gel bath for coagulation and fixation to obtain the electrolytic water diaphragm.
12. The method for preparing a water electrolysis membrane according to claim 11, characterized in that: The phase separation temperature is 25-80°C; and / or, the relative humidity of the phase separation is 10-90%; And / or, the phase separation time is 5s-1min; And / or, the temperature of the solidification is 15-80°C; And / or, the solidification time is 5-45 minutes.
13. Use of the electrolytic water diaphragm additive according to claim 1, the electrolytic water diaphragm coating slurry according to any one of claims 6 to 8, or the electrolytic water diaphragm according to claim 9 or 10, characterized in that: For alkaline electrolysis of water.
14. An alkaline water electrolysis device, characterized in that it comprises the water electrolysis membrane additive according to claim 1 or the water electrolysis membrane according to claim 9 or 10.