Hot-melt polyurethane sealant and preparation method thereof
By combining thermoplastic acrylic resin and high molecular weight liquid polyester polyol, hot melt polyurethane sealant is prepared, which solves the problem of traditional sealant lacking flexibility and requires UV light, and realizes stress relief of sealant after substrate deformation and High sealing effect.
Patent Information
- Application Number
- CN202411168678.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-23
- Publication Date
- 2024-11-26
AI Technical Summary
After curing, traditional polyurethane sealant is plastic, lacks flexibility, and is prone to stress concentration, cracking or leakage due to deformation of the substrate, and requires UV light to achieve a good initial bonding strength. It is suitable for light-transmitting materials. ideal.
Hot melt polyurethane sealant is used to combine thermoplastic acrylic resin and high molecular weight liquid polyester polyol to prepare the sealant to be rubber-like after curing, and has flexibility. The moisture curing characteristics are obtained through polyisocyanate reaction, and combined with latent curing. The agent and filler ensure that the sealant can flow at high temperatures and quickly form strength after cooling.
The sealant can deform accordingly when the substrate is deformed, reducing stress concentration, and can better cope with vibration, impact, cold and cold changes. The sealing effect is good and is not easy to crack and leak, and it can achieve high initial bonding strength without UV light.
Smart Images

Figure SMS_1 
Figure SMS_2 
Figure SMS_3
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of sealants, and in particular to a hot-melt polyurethane sealant and a preparation method thereof. Background Art
[0002] Traditional polyurethane sealants take several hours to form initial bonding strength, and the final bonding strength is low. This results in a long period of standing after application, and even requires auxiliary mechanical fixation. For this reason, new designs have been made for polyurethane sealants, such as the Chinese patent document: CN202311832489.4 discloses a UV moisture-curing polyurethane hot melt adhesive and a preparation method thereof. The UV moisture-curing polyurethane hot melt adhesive includes components in parts by weight: 30 to 80 parts of polyol polymer D, 10 to 40 parts of isocyanate compounds, 0.1 to 50 parts of modified acrylates, 0.1 to 10 parts of homemade cross-linking agents, 0.01 to 3 parts of catalysts, 0.1 to 5 parts of photoinitiators, 2 to 30 parts of thermoplastic resins, and 2 to 12 parts of tackifying resins. The UV moisture-curing polyurethane hot melt adhesive prepared by the invention has good initial bonding strength and can realize a pressure-free process. The glue that has not been exposed to light can still undergo a curing reaction to achieve good bonding strength. However, the hot melt adhesive prepared by the invention is plastic-like after curing, is relatively hard, and lacks flexibility. When the bonded substrate is deformed, stress concentration is easily formed, resulting in cracking, leakage, or excessive pulling of the substrate, affecting the sealing effect of use. At the same time, it requires UV light to be used in conjunction to achieve a good initial bonding strength, and the effect is not ideal when used on opaque materials. Summary of the invention
[0003] Therefore, in view of the above problems, the present invention provides a hot-melt polyurethane sealant and a preparation method thereof. The hot-melt polyurethane sealant prepared by the present invention is rubber-like after curing and is relatively soft. After bonding, it can deform along with the deformation of the substrate, thereby reducing stress concentration, being able to better cope with vibration, impact, cold and hot changes, etc., not easy to crack and leak, and having a good sealing effect.
[0004] To solve this technical problem, the present invention adopts the following scheme: a hot-melt polyurethane sealant, comprising the following components in parts by weight: 3-20 parts of a thermoplastic acrylic resin, 5-50 parts of a polyether polyol, 30-80 parts of a high molecular weight liquid polyester polyol, 10-20 parts of a polyisocyanate, 0-2 parts of a silane coupling agent, 0-1 parts of an antioxidant, 0-1 parts of a light stabilizer, 0-5 parts of a latent curing agent, and 0-20 parts of a filler. The high molecular weight liquid polyester polyol has a Tg of ≤-10°C and a molecular weight of ≥3500, the thermoplastic acrylic resin has a glass transition temperature of ≥40°C and a molecular weight of ≥30000, and the thermoplastic acrylic resin is any one of Mitsubishi BR-113 resin, Mitsubishi BR-116 resin, Lucite 2013 resin, Lucite 2016 resin, and Evonik DYNACOLL AC 2740 resin.
[0005] Furthermore, the latent curing agent is an amine latent curing agent, which is an oxazolidine type or imine type latent curing agent.
[0006] Furthermore, the filler is any one of carbon black, calcium carbonate, talcum powder, and white carbon black, or a mixture of two of them.
[0007] The preparation method of the hot melt polyurethane sealant comprises the following steps: Thermoplastic acrylic resin, polyether polyol, high molecular weight liquid polyester polyol and filler are weighed according to the mass parts, added into a mixer at a temperature environment of 100-180°C and stirred evenly, vacuumed to remove water for 0.5-2.5 hours, then polyisocyanate is added and reacted for 0.5-2.5 hours, then latent curing agent, silane coupling agent, antioxidant and light stabilizer are added, mixed evenly, discharged and sealed and packaged to prepare a hot-melt polyurethane sealant.
[0008] By adopting the above-mentioned technical scheme, the beneficial effects of the present invention are as follows: the sealant is endowed with the property of being flowable at high temperature and quickly forming strength after cooling by combining the thermoplastic acrylic resin and the polyester polyol, and having high strength after curing, and adopting a reasonable proportion of a high molecular weight liquid polyester polyol with a molecular weight ≥3500 and a Tg≤-10°C and a thermoplastic acrylic resin and other components, that is, the high molecular weight liquid polyester polyol is adopted to take into account the flexibility and strength of the product, and the moisture curing property is obtained by reacting the high molecular weight liquid polyester polyol with polyisocyanate to obtain an NCO-terminated prepolymer, and then combined with an appropriate amount of acrylic resin to improve the initial solidity and avoid the colloid from being too hard, so that the prepared hot-melt polyurethane sealant is rubber-like after curing, is relatively soft, can deform with the deformation of the substrate after bonding, thereby reducing stress concentration, can better cope with vibration, impact, cold and hot changes, etc., is not easy to crack and leak, and has a good sealing effect. DETAILED DESCRIPTION
[0009] The present invention will now be further described in conjunction with specific implementation methods.
[0010] Example 1
[0011] The preparation method of hot-melt polyurethane sealant comprises the following steps: Thermoplastic acrylic resin, polyether polyol (i.e., polypropylene glycol PPG-2000), high molecular weight liquid polyester polyol (i.e., high molecular weight liquid polyester polyol Dynacoll 7250) and filler (i.e., carbon black) are weighed according to the mass parts in the above table, added into a mixer at a temperature of 100-180°C, stirred evenly, vacuumed to remove water for 0.5-2.5 hours, then polyisocyanate (i.e., diphenylmethane-4,4'-diisocyanate) is added, reacted for 0.5-2.5 hours, then latent curing agent, silane coupling agent, antioxidant and light stabilizer are added, mixed evenly, discharged and sealed and packaged to obtain a hot-melt polyurethane sealant.
[0012] Example 2
[0013] The preparation method of hot-melt polyurethane sealant comprises the following steps: Thermoplastic acrylic resin (i.e., thermoplastic acrylic resin BR113 and thermoplastic acrylic resin DYNACOLL AC 2740), polyether polyol (i.e., polypropylene glycol PPG-2000), high molecular weight liquid polyester polyol (i.e., high molecular weight liquid polyester polyol Dynacoll 7250 and high molecular weight liquid polyester polyol Dynacoll 7255) and filler (i.e., carbon black) are weighed according to the mass parts in the above table, added into a mixer at a temperature of 100-180°C, stirred evenly, vacuumed to remove water for 0.5-2.5 hours, then polyisocyanate (i.e., diphenylmethane-4,4'-diisocyanate) is added, reacted for 0.5-2.5 hours, then a latent curing agent, a silane coupling agent, an antioxidant and a light stabilizer are added, mixed evenly, discharged and sealed and packaged, to obtain a hot-melt polyurethane sealant.
[0014] Comparative Example 1
[0015] The preparation method of the hot melt polyurethane sealant in the comparative example 1 is the same as that in the embodiment 1.
[0016] Example 1, Example 2 and Comparative Example 1 were tested (bonding a circular iron substrate with a diameter of 16 cm, and testing the tensile strength at room temperature for 10 minutes; bonding PC according to GB / T 7124, and testing the tensile shear strength after curing for 7 days at room temperature and 50% relative humidity). The test results are as follows:
[0017] It can be seen from the above tests that Examples 1 and 2 contain an appropriate amount of acrylic resin while Comparative Example 1 does not contain this ingredient, resulting in that the initial solidification strength of Examples 1 and 2 is higher than that of Comparative Example 1; Examples 1 and 2 contain high molecular weight liquid polyester polyol while Comparative Example 1 does not contain this ingredient, resulting in that the shear strength of Examples 1 and 2 after moisture curing is higher than that of Comparative Example 1.
[0018] The components of the hot-melt polyurethane sealant of the present invention are preferably in the following weight proportions: 3-20 parts of thermoplastic acrylic resin, 5-50 parts of polyether polyol, 30-80 parts of high molecular weight liquid polyester polyol, 10-20 parts of polyisocyanate, 0-2 parts of silane coupling agent, 0-1 parts of antioxidant, 0-1 parts of light stabilizer, 0-5 parts of latent curing agent, and 0-20 parts of filler.
[0019] The high molecular weight liquid polyester polyol preferably has a Tg of ≤-10°C and a molecular weight of ≥3500, the thermoplastic acrylic resin preferably has a glass transition temperature of ≥40°C and a molecular weight of ≥30000, the thermoplastic acrylic resin is polymerized from methyl methacrylate, methyl acrylate, butyl methacrylate, butyl acrylate, and isooctyl acrylate monomers, the thermoplastic acrylic resin is any one of Mitsubishi BR-113 resin, Mitsubishi BR-116 resin, Lucite 2013 resin, Lucite 2016 resin, and Evonik DYNACOLL AC2740 resin, the latent curing agent can also be an amine latent curing agent, an oxazolidine type or an imine type latent curing agent, and the filler can be any one of carbon black, calcium carbonate, talc, and white carbon black, or a mixture of two of them.
[0020] It should be noted that, in this article, words such as "include", "comprises" or any other variations thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device. In the absence of more restrictions. The phrase "including an element defined by ..." does not exclude the existence of other identical elements in the process, method, article or device including the element".
[0021] The above embodiments are only preferred embodiments of the present invention, and the present invention may also have other embodiments. For those of ordinary skill in the art, it will be appreciated that various changes, modifications, substitutions and variations may be made to these embodiments without departing from the principles and spirit of the present invention, and the scope of the present invention is limited by the appended claims and their equivalents.
Claims
1. A hot melt polyurethane sealant, characterized in that: The invention comprises the following components in parts by weight: 3-20 parts of thermoplastic acrylic resin, 5-50 parts of polyether polyol, 30-80 parts of high molecular weight liquid polyester polyol, 10-20 parts of polyisocyanate, 0-2 parts of silane coupling agent, 0-1 part of antioxidant, 0-1 part of light stabilizer, 0-5 parts of latent curing agent and 0-20 parts of filler. The high molecular weight liquid polyester polyol has a Tg of ≤-10°C and a molecular weight of ≥3500. The thermoplastic acrylic resin has a glass transition temperature of ≥40°C and a molecular weight of ≥30000. The thermoplastic acrylic resin is any one of Mitsubishi BR-113 resin, Mitsubishi BR-116 resin, Lucite 2013 resin, Lucite 2016 resin and Evonik DYNACOLL AC 2740 resin.
2. The hot melt polyurethane sealant according to claim 1, characterized in that: The latent curing agent is an amine latent curing agent, an oxazolidine type or an imine type latent curing agent.
3. The hot melt polyurethane sealant according to claim 1, characterized in that: The filler is any one of carbon black, calcium carbonate, talcum powder and white carbon black or a mixture of two of them.
4. A method for preparing the hot melt polyurethane sealant according to any one of claims 1 to 3, characterized in that: The following steps are involved: Thermoplastic acrylic resin, polyether polyol, high molecular weight liquid polyester polyol and filler are weighed according to the mass parts, added into a mixer at a temperature environment of 100-180°C and stirred evenly, vacuumed to remove water for 0.5-2.5 hours, then polyisocyanate is added and reacted for 0.5-2.5 hours, then latent curing agent, silane coupling agent, antioxidant and light stabilizer are added, mixed evenly, discharged and sealed and packaged to prepare a hot-melt polyurethane sealant.
Citation Information
Patent Citations
Reactive polyurethane hot melt adhesive with high initial adhesion and low wiredrawing performance and preparation method thereof
CN110484188A
Moisture-curable polyurethane hot melt adhesive for intelligent wearable product and preparation method of moisture-curable polyurethane hot melt adhesive
CN112646534A
Reactive polyurethane hot melt adhesive for sealing car lamp and preparation method thereof
CN115595109A
Polyurethane hot melt adhesive for thin base material and preparation method of polyurethane hot melt adhesive
CN115820193A
UV moisture dual-curing reactive polyurethane hot melt adhesive and preparation method thereof
CN115851208A