High-performance silicon-carbon-based negative electrode adhesive for new energy battery and preparation method of high-performance silicon-carbon-based negative electrode adhesive

By preparing high-performance silicon-carbon-based negative electrode adhesives, using polymer cross-linking and nanofillers, the stress problems caused by volume expansion of silicon-based negative electrode materials are solved, the stability and energy density of the battery are improved, the cycle life is extended and the cycle life is simplified. Production process.

CN119019975APending Publication Date: 2024-11-26SUZHOU RUITENGNING ENERGY TECHNOLOGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411361071.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-27
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

The huge volume changes in the silicon-based negative electrode material during charging and discharging lead to internal stress, prone to cracks and powdering, resulting in reduced battery capacity and safety problems. Traditional carbon-based adhesives cannot effectively deal with the expansion of silicon-carbon negative electrode material.

Method used

Prepare high-quality raw materials such as polyacrylonitrile, polyvinylidene fluoride, polyimide, polypyrrole, polyaniline, polyvinyl alcohol, nanosilicon dioxide, nanocarbon tubes, aziridine crosslinking agent and sodium stearate. Properties of silicon-carbon-based negative electrode adhesives form high mechanical strength, conductive and stable adhesives through cross-linking reaction and defoaming treatment.

Benefits of technology

Effectively alleviate the volume expansion of silicon material, improve the stability and mechanical strength of electrode materials, optimize electrochemical performance, extend battery cycle life, and improve energy density and production efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The invention discloses a high-performance silicon-carbon-based negative electrode adhesive for a new energy battery and a preparation method of the high-performance silicon-carbon-based negative electrode adhesive. The preparation method comprises the following steps: S1, sequentially weighing the following raw materials in parts by weight: 10-15 parts of polyacrylonitrile, 8-12 parts of polyvinylidene fluoride, 14-18 parts of polyimide, 20-22 parts of polypyrrole, 7-9 parts of polyaniline, 4-6 parts of polyvinyl alcohol, 18-22 parts of nano silicon dioxide, 15-20 parts of carbon nanotubes, 15-20 parts of an aziridine cross-linking agent, 8-12 parts of sodium stearate and 2-6 parts of polydimethylsiloxane for later use; s2, adding the weighed polyacrylonitrile, polyvinylidene fluoride, polyimide, polypyrrole, polyaniline and polyvinyl alcohol into a reaction container. The volume expansion of the silicon material can be effectively relieved, the electrochemical performance is optimized, the heat resistance and chemical resistance of the adhesive are remarkably improved, and the mechanical strength and conductivity of the adhesive are improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of new energy battery materials, and in particular to a high-performance silicon-carbon-based negative electrode adhesive for new energy batteries and a preparation method thereof. Background Art

[0002] Silicon-carbon-based negative electrode material is an interfacial binder for lithium-ion batteries. With the popularity of wearable devices and electric vehicles, the demand for high-performance lithium-ion batteries is increasing. At present, graphite is the mainstream negative electrode material, and commercial graphite negative electrode is close to the theoretical specific capacity upper limit of 372mAh / g, which limits its further application. Among the known negative electrode materials, silicon has a theoretical specific capacity of up to 4200mAh / g, which is more than 10 times that of graphite materials, and can provide channels for lithium ion embedding and extraction from all directions. It has excellent fast charging performance and better safety than graphite negative electrode materials. It is also rich in reserves and low in cost. It is the most promising new generation of lithium battery negative electrode material.

[0003] Although silicon-based negative electrode materials are expected to become the next generation of negative electrode materials, they will undergo huge volume changes during the charging and discharging process, which has become a major problem for their industrial application. When silicon is fully lithiated, its volume expands by more than 300%, which will lead to many problems, such as: the volume expansion produces huge internal stress, which can easily cause cracks or even powderization of silicon negative electrode materials; this effect makes it easy for electrode materials to lose contact with the current collector, causing the active material to fall off and the battery capacity to drop rapidly; the volume expansion can easily form an unstable SEI film, which breaks and continuously consumes lithium ions in the electrolyte as the silicon volume changes, causing irreversible capacity loss and reduced initial charging efficiency.

[0004] Since silicon and carbon materials are two completely different materials, traditional carbon-based negative electrode adhesives cannot be used well on silicon-based negative electrodes. A suitable silicon-carbon negative electrode material should have high tensile strength and elastic modulus, be able to withstand the stress caused by large volume expansion, and have self-healing ability. Adhesive is one of the important components of lithium-ion batteries. It is a polymer compound that adheres the active material and conductive agent in the electrode sheet to the electrode current collector. The performance of the adhesive directly affects the capacity, life and safety of the battery. As an auxiliary material, the gross profit margin of the adhesive is 70%, which is higher than the four main materials of lithium batteries. Compared with the existing positive and negative electrode adhesives, it has significant advantages in cost, environmental protection and performance. Adhesives are a "small and beautiful" subdivision of the battery industry, with a high gross profit margin, higher than other main materials. Water-based adhesive materials are the main development trend of lithium battery adhesives. However, previous reports on silicon-based negative electrode adhesives have paid less attention to and research on silicon-carbon negative electrode adhesives, and due to the coexistence of multiple interfaces in the interface of silicon-carbon particles, most silicon negative electrode adhesives are not suitable for silicon-carbon negative electrodes. Therefore, a high-performance silicon-carbon-based negative electrode adhesive for new energy batteries and its preparation method are proposed to solve the above problems. Summary of the invention

[0005] Based on the technical problems existing in the background technology, the present invention proposes a high-performance silicon-carbon-based negative electrode adhesive for new energy batteries and a preparation method thereof to solve the above problems.

[0006] The invention provides a high-performance silicon-carbon-based negative electrode adhesive for a new energy battery, comprising the following raw materials in parts by weight: 10 to 15 parts of polyacrylonitrile, 8 to 12 parts of polyvinylidene fluoride, 14 to 18 parts of polyimide, 20 to 22 parts of polypyrrole, 7 to 9 parts of polyaniline, 4 to 6 parts of polyvinyl alcohol, 18 to 22 parts of nano-silicon dioxide, 15 to 20 parts of nano-carbon tubes, 15 to 20 parts of aziridine cross-linking agent, 8 to 12 parts of sodium stearate and 2 to 6 parts of polydimethylsiloxane.

[0007] In a preferred embodiment, the raw materials include the following parts by weight: 10 parts of polyacrylonitrile, 8 parts of polyvinylidene fluoride, 14 parts of polyimide, 20 parts of polypyrrole, 7 parts of polyaniline, 4 parts of polyvinyl alcohol, 18 parts of nano-silicon dioxide, 15 parts of carbon nanotubes, 15 parts of aziridine crosslinking agent, 8 parts of sodium stearate and 2 parts of polydimethylsiloxane.

[0008] In a preferred embodiment, the raw materials include the following parts by weight: 15 parts of polyacrylonitrile, 12 parts of polyvinylidene fluoride, 18 parts of polyimide, 22 parts of polypyrrole, 9 parts of polyaniline, 6 parts of polyvinyl alcohol, 22 parts of nano-silicon dioxide, 20 parts of carbon nanotubes, 20 parts of aziridine crosslinking agent, 12 parts of sodium stearate and 6 parts of polydimethylsiloxane.

[0009] In a preferred embodiment, the method for preparing a high-performance silicon-carbon-based negative electrode adhesive for new energy batteries comprises the following steps: Step S1: weigh the following raw materials in parts by weight: 10-15 parts of polyacrylonitrile, 8-12 parts of polyvinylidene fluoride, 14-18 parts of polyimide, 20-22 parts of polypyrrole, 7-9 parts of polyaniline, 4-6 parts of polyvinyl alcohol, 18-22 parts of nano-silicon dioxide, 15-20 parts of carbon nanotubes, 15-20 parts of aziridine crosslinking agent, 8-12 parts of sodium stearate and 2-6 parts of polydimethylsiloxane, and set aside; Step S2: adding weighed polyacrylonitrile, polyvinylidene fluoride, polyimide, polypyrrole, polyaniline and polyvinyl alcohol into a reaction container, stirring and dissolving at a certain temperature to form a uniform polymer solution; Step S3: Slowly adding nano-silicon dioxide and nano-carbon tubes to the polymer solution under stirring, and continuing stirring for a period of time to ensure that the nano-filler is fully dispersed in the polymer solution; Step S4: adding aziridine crosslinking agent to the mixed solution, raising the temperature to an appropriate temperature, stirring and reacting for a certain period of time to allow the polymer to undergo a crosslinking reaction; Step S5: adding sodium stearate and continuing stirring at the same temperature for a period of time to improve the dispersion uniformity of the nanofiller in the system; Step S6: adding polydimethylsiloxane, stirring evenly, and then degassing the mixed solution; Step S7: coating the prepared adhesive solution on the silicon-carbon-based negative electrode material of the new energy battery, drying it at an appropriate temperature for a certain period of time to solidify the adhesive, thereby obtaining a high-performance silicon-carbon-based negative electrode adhesive.

[0010] In a preferred embodiment, in step S2, the temperature is set to 50-70° C., and the stirring time is set to 20-30 min.

[0011] In a preferred embodiment, in step S3, stirring is performed at room temperature for 2 to 3 hours and then heating and stirring in a water bath. The speed of the stirrer is set to 200 to 300 r / min during stirring at room temperature and to 400 to 600 r / min during heating and stirring in a water bath.

[0012] In a preferred embodiment, in step S4, the temperature is raised to 80-100° C., and the stirring time is set to 3-5 h.

[0013] In a preferred embodiment, in step S5, the stirring speed is set to 100-150 r / min, and the stirring time is set to 60-80 min.

[0014] In a preferred embodiment, in step S7, the temperature is set to 60-80° C., and the drying time is set to 2-4 hours.

[0015] Beneficial effects of the present invention: The present invention proposes a high-performance silicon-carbon-based negative electrode adhesive for new energy batteries and a preparation method thereof. By adding polyacrylonitrile, polyvinylidene fluoride and polyimide, the adhesive has good elasticity and mechanical strength and can effectively alleviate the volume expansion of silicon materials. The present invention proposes a high-performance silicon-carbon-based negative electrode adhesive for new energy batteries and a preparation method thereof. By adding polypyrrole and polyaniline, an electron conduction path is provided and the stability of the electrode material can be improved. By adding polyvinyl alcohol, the interface compatibility between the electrolyte and the electrode material is improved and the electrochemical performance is optimized. The present invention provides a high-performance silicon-carbon-based negative electrode adhesive for new energy batteries and a preparation method thereof. Nano-silicon dioxide and nano-carbon tubes are added to improve the mechanical strength and conductivity of the adhesive. An aziridine cross-linking agent is added, and the aziridine cross-linking agent can react with carboxyl, hydroxyl, amine and other groups at room temperature to form a three-dimensional network structure, thereby significantly improving the heat resistance and chemical resistance of the adhesive. The present invention proposes a high-performance silicon-carbon-based negative electrode adhesive for new energy batteries and a preparation method thereof. By adding sodium stearate, negatively charged micelles can be formed in water, and the particles are dispersed by electrostatic repulsion; by adding polydimethylsiloxane, a good defoaming effect can be achieved. DETAILED DESCRIPTION

[0016] The present invention will be further explained below in conjunction with specific embodiments. Example

[0017] In this embodiment, a high-performance silicon-carbon-based negative electrode adhesive for new energy batteries is proposed, which includes the following raw materials in parts by weight: 10 parts of polyacrylonitrile, 8 parts of polyvinylidene fluoride, 14 parts of polyimide, 20 parts of polypyrrole, 7 parts of polyaniline, 4 parts of polyvinyl alcohol, 18 parts of nano-silicon dioxide, 15 parts of nano-carbon tubes, 15 parts of aziridine crosslinking agent, 8 parts of sodium stearate and 2 parts of polydimethylsiloxane.

[0018] Furthermore, the preparation method of the high-performance silicon-carbon-based negative electrode adhesive for new energy batteries comprises the following steps: Step S1: weigh the following raw materials in order by weight: 10 parts of polyacrylonitrile, 8 parts of polyvinylidene fluoride, 14 parts of polyimide, 20 parts of polypyrrole, 7 parts of polyaniline, 4 parts of polyvinyl alcohol, 18 parts of nano-silicon dioxide, 15 parts of carbon nanotubes, 15 parts of aziridine crosslinking agent, 8 parts of sodium stearate and 2 parts of polydimethylsiloxane, and set aside; Step S2: adding weighed polyacrylonitrile, polyvinylidene fluoride, polyimide, polypyrrole, polyaniline and polyvinyl alcohol into a reaction container, stirring and dissolving at a certain temperature to form a uniform polymer solution; Step S3: Slowly adding nano-silicon dioxide and nano-carbon tubes to the polymer solution under stirring, and continuing stirring for a period of time to ensure that the nano-filler is fully dispersed in the polymer solution; Step S4: adding aziridine crosslinking agent to the mixed solution, raising the temperature to an appropriate temperature, stirring and reacting for a certain period of time to allow the polymer to undergo a crosslinking reaction; Step S5: adding sodium stearate and continuing stirring at the same temperature for a period of time to improve the dispersion uniformity of the nanofiller in the system; Step S6: adding polydimethylsiloxane, stirring evenly, and then degassing the mixed solution; Step S7: coating the prepared adhesive solution on the silicon-carbon-based negative electrode material of the new energy battery, drying it at an appropriate temperature for a certain period of time to solidify the adhesive, thereby obtaining a high-performance silicon-carbon-based negative electrode adhesive.

[0019] Furthermore, in step S2, the temperature is set to 50°C and the stirring time is set to 20 min. In step S3, the mixture is first stirred at room temperature for 2 h and then heated and stirred in a water bath. The speed of the stirrer is set to 200 r / min during stirring at room temperature and to 400 r / min during heating and stirring in a water bath. In step S4, the temperature is increased to 80°C and the stirring time is set to 3 h. In step S5, the stirring speed is set to 100 r / min and the stirring time is set to 60 min. In step S7, the temperature is set to 60°C and the drying time is set to 2 h. Example

[0020] In this embodiment, a high-performance silicon-carbon-based negative electrode adhesive for new energy batteries is proposed, which includes the following raw materials in parts by weight: 11 parts of polyacrylonitrile, 9 parts of polyvinylidene fluoride, 15 parts of polyimide, 20 parts of polypyrrole, 7 parts of polyaniline, 4 parts of polyvinyl alcohol, 19 parts of nano-silicon dioxide, 16 parts of nano-carbon tubes, 16 parts of aziridine crosslinking agent, 8 parts of sodium stearate and 3 parts of polydimethylsiloxane.

[0021] Furthermore, the preparation method of the high-performance silicon-carbon-based negative electrode adhesive for new energy batteries comprises the following steps: Step S1: weigh the following raw materials in parts by weight: 11 parts of polyacrylonitrile, 9 parts of polyvinylidene fluoride, 15 parts of polyimide, 20 parts of polypyrrole, 7 parts of polyaniline, 4 parts of polyvinyl alcohol, 19 parts of nano-silicon dioxide, 16 parts of carbon nanotubes, 16 parts of aziridine crosslinking agent, 8 parts of sodium stearate and 3 parts of polydimethylsiloxane, and set aside; Step S2: adding weighed polyacrylonitrile, polyvinylidene fluoride, polyimide, polypyrrole, polyaniline and polyvinyl alcohol into a reaction container, stirring and dissolving at a certain temperature to form a uniform polymer solution; Step S3: Slowly adding nano-silicon dioxide and nano-carbon tubes to the polymer solution under stirring, and continuing stirring for a period of time to ensure that the nano-filler is fully dispersed in the polymer solution; Step S4: adding aziridine crosslinking agent to the mixed solution, raising the temperature to an appropriate temperature, stirring and reacting for a certain period of time to allow the polymer to undergo a crosslinking reaction; Step S5: adding sodium stearate and continuing stirring at the same temperature for a period of time to improve the dispersion uniformity of the nanofiller in the system; Step S6: adding polydimethylsiloxane, stirring evenly, and then degassing the mixed solution; Step S7: coating the prepared adhesive solution on the silicon-carbon-based negative electrode material of the new energy battery, drying it at an appropriate temperature for a certain period of time to solidify the adhesive, thereby obtaining a high-performance silicon-carbon-based negative electrode adhesive.

[0022] Furthermore, in step S2, the temperature is set to 55°C, and the stirring time is set to 22 min. In step S3, the mixture is first stirred at room temperature for 2 h and then heated and stirred in a water bath. The speed of the stirrer is set to 220 r / min during stirring at room temperature, and the speed of the stirrer is set to 450 r / min during heating and stirring in a water bath. In step S4, the temperature is increased to 85°C, and the stirring time is set to 3 h. In step S5, the stirring speed is set to 110 r / min, and the stirring time is set to 65 min. In step S7, the temperature is set to 65°C, and the drying time is set to 2 h. Example

[0023] In this embodiment, a high-performance silicon-carbon-based negative electrode adhesive for new energy batteries is proposed, which includes the following raw materials in parts by weight: 12 parts of polyacrylonitrile, 10 parts of polyvinylidene fluoride, 16 parts of polyimide, 21 parts of polypyrrole, 8 parts of polyaniline, 5 parts of polyvinyl alcohol, 20 parts of nano-silicon dioxide, 17 parts of nano-carbon tubes, 17 parts of aziridine crosslinking agent, 10 parts of sodium stearate and 4 parts of polydimethylsiloxane.

[0024] Furthermore, the preparation method of the high-performance silicon-carbon-based negative electrode adhesive for new energy batteries comprises the following steps: Step S1: weigh the following raw materials in order by weight: 12 parts of polyacrylonitrile, 10 parts of polyvinylidene fluoride, 16 parts of polyimide, 21 parts of polypyrrole, 8 parts of polyaniline, 5 parts of polyvinyl alcohol, 20 parts of nano-silicon dioxide, 17 parts of carbon nanotubes, 17 parts of aziridine crosslinking agent, 10 parts of sodium stearate and 4 parts of polydimethylsiloxane, and set aside; Step S2: adding weighed polyacrylonitrile, polyvinylidene fluoride, polyimide, polypyrrole, polyaniline and polyvinyl alcohol into a reaction container, stirring and dissolving at a certain temperature to form a uniform polymer solution; Step S3: Slowly adding nano-silicon dioxide and nano-carbon tubes to the polymer solution under stirring, and continuing stirring for a period of time to ensure that the nano-filler is fully dispersed in the polymer solution; Step S4: adding aziridine crosslinking agent to the mixed solution, raising the temperature to an appropriate temperature, stirring and reacting for a certain period of time to allow the polymer to undergo a crosslinking reaction; Step S5: adding sodium stearate and continuing stirring at the same temperature for a period of time to improve the dispersion uniformity of the nanofiller in the system; Step S6: adding polydimethylsiloxane, stirring evenly, and then degassing the mixed solution; Step S7: coating the prepared adhesive solution on the silicon-carbon-based negative electrode material of the new energy battery, drying it at an appropriate temperature for a certain period of time to solidify the adhesive, thereby obtaining a high-performance silicon-carbon-based negative electrode adhesive.

[0025] Furthermore, in step S2, the temperature is set to 60°C and the stirring time is set to 26 min. In step S3, the mixture is first stirred at room temperature for 2 h and then heated and stirred in a water bath. The speed of the stirrer is set to 250 r / min during stirring at room temperature and to 500 r / min during heating and stirring in a water bath. In step S4, the temperature is increased to 90°C and the stirring time is set to 4 h. In step S5, the stirring speed is set to 125 r / min and the stirring time is set to 70 min. In step S7, the temperature is set to 70°C and the drying time is set to 3 h. Example

[0026] In this embodiment, a high-performance silicon-carbon-based negative electrode adhesive for new energy batteries is proposed, which includes the following raw materials in parts by weight: 14 parts of polyacrylonitrile, 11 parts of polyvinylidene fluoride, 17 parts of polyimide, 21 parts of polypyrrole, 8 parts of polyaniline, 6 parts of polyvinyl alcohol, 21 parts of nano-silicon dioxide, 19 parts of nano-carbon tubes, 18 parts of aziridine crosslinking agent, 11 parts of sodium stearate and 5 parts of polydimethylsiloxane.

[0027] Furthermore, the preparation method of the high-performance silicon-carbon-based negative electrode adhesive for new energy batteries comprises the following steps: Step S1: weigh the following raw materials in parts by weight: 14 parts of polyacrylonitrile, 11 parts of polyvinylidene fluoride, 17 parts of polyimide, 21 parts of polypyrrole, 8 parts of polyaniline, 6 parts of polyvinyl alcohol, 21 parts of nano-silicon dioxide, 19 parts of carbon nanotubes, 18 parts of aziridine crosslinking agent, 11 parts of sodium stearate and 5 parts of polydimethylsiloxane, and set aside; Step S2: adding weighed polyacrylonitrile, polyvinylidene fluoride, polyimide, polypyrrole, polyaniline and polyvinyl alcohol into a reaction container, stirring and dissolving at a certain temperature to form a uniform polymer solution; Step S3: Slowly adding nano-silicon dioxide and nano-carbon tubes to the polymer solution under stirring, and continuing stirring for a period of time to ensure that the nano-filler is fully dispersed in the polymer solution; Step S4: adding aziridine crosslinking agent to the mixed solution, raising the temperature to an appropriate temperature, stirring and reacting for a certain period of time to allow the polymer to undergo a crosslinking reaction; Step S5: adding sodium stearate and continuing stirring at the same temperature for a period of time to improve the dispersion uniformity of the nanofiller in the system; Step S6: adding polydimethylsiloxane, stirring evenly, and then degassing the mixed solution; Step S7: coating the prepared adhesive solution on the silicon-carbon-based negative electrode material of the new energy battery, drying it at an appropriate temperature for a certain period of time to solidify the adhesive, thereby obtaining a high-performance silicon-carbon-based negative electrode adhesive.

[0028] Furthermore, in step S2, the temperature is set to 65°C, and the stirring time is set to 28 min. In step S3, the mixture is first stirred at room temperature for 3 h and then heated and stirred in a water bath. The speed of the stirrer is set to 280 r / min during stirring at room temperature, and the speed of the stirrer is set to 550 r / min during heating and stirring in a water bath. In step S4, the temperature is increased to 95°C, and the stirring time is set to 5 h. In step S5, the stirring speed is set to 140 r / min, and the stirring time is set to 75 min. In step S7, the temperature is set to 75°C, and the drying time is set to 3 h. Example

[0029] In this embodiment, a high-performance silicon-carbon-based negative electrode adhesive for new energy batteries is proposed, which includes the following raw materials in parts by weight: 15 parts of polyacrylonitrile, 12 parts of polyvinylidene fluoride, 18 parts of polyimide, 22 parts of polypyrrole, 9 parts of polyaniline, 6 parts of polyvinyl alcohol, 22 parts of nano-silicon dioxide, 20 parts of carbon nanotubes, 20 parts of aziridine crosslinking agent, 12 parts of sodium stearate and 6 parts of polydimethylsiloxane.

[0030] Furthermore, the preparation method of the high-performance silicon-carbon-based negative electrode adhesive for new energy batteries comprises the following steps: Step S1: weigh the following raw materials in parts by weight: 15 parts of polyacrylonitrile, 12 parts of polyvinylidene fluoride, 18 parts of polyimide, 22 parts of polypyrrole, 9 parts of polyaniline, 6 parts of polyvinyl alcohol, 22 parts of nano-silicon dioxide, 20 parts of carbon nanotubes, 20 parts of aziridine crosslinking agent, 12 parts of sodium stearate and 6 parts of polydimethylsiloxane, and set aside; Step S2: adding weighed polyacrylonitrile, polyvinylidene fluoride, polyimide, polypyrrole, polyaniline and polyvinyl alcohol into a reaction container, stirring and dissolving at a certain temperature to form a uniform polymer solution; Step S3: Slowly adding nano-silicon dioxide and nano-carbon tubes to the polymer solution under stirring, and continuing stirring for a period of time to ensure that the nano-filler is fully dispersed in the polymer solution; Step S4: adding aziridine crosslinking agent to the mixed solution, raising the temperature to an appropriate temperature, stirring and reacting for a certain period of time to allow the polymer to undergo a crosslinking reaction; Step S5: adding sodium stearate and continuing stirring at the same temperature for a period of time to improve the dispersion uniformity of the nanofiller in the system; Step S6: adding polydimethylsiloxane, stirring evenly, and then degassing the mixed solution; Step S7: coating the prepared adhesive solution on the silicon-carbon-based negative electrode material of the new energy battery, drying it at an appropriate temperature for a certain period of time to solidify the adhesive, thereby obtaining a high-performance silicon-carbon-based negative electrode adhesive.

[0031] Furthermore, in step S2, the temperature is set to 70°C and the stirring time is set to 30 min. In step S3, the mixture is first stirred at room temperature for 3 h and then heated and stirred in a water bath. The speed of the stirrer is set to 300 r / min during stirring at room temperature and to 600 r / min during heating and stirring in a water bath. In step S4, the temperature is increased to 100°C and the stirring time is set to 5 h. In step S5, the stirring speed is set to 150 r / min and the stirring time is set to 80 min. In step S7, the temperature is set to 80°C and the drying time is set to 4 h.

[0032] The viscosity, pH value, electrochemical peeling force and internal resistance of the high-performance silicon-carbon-based negative electrode adhesives prepared in Examples 1 to 5 above were tested, and the results are shown in the following table:

[0033] It can be seen from the above table that high viscosity is the key to the adhesive forming a stable and strong bonding layer on the surface of the silicon-carbon negative electrode, which helps to improve the overall performance of the battery; this neutral to weakly alkaline pH range allows the adhesive to maintain stable performance in a variety of battery preparation environments, avoiding performance degradation or failure caused by changes in pH; high peel force indicates that a strong interfacial bonding force is formed between the adhesive and the silicon-carbon negative electrode material, which helps to prevent the risk of active material shedding and internal short circuit of the battery; low internal resistance helps to reduce the energy loss of the battery during charging and discharging, improve the efficiency and service life of the battery, and Example 3 is the best example.

[0034] In the high-rate cycle test of 1C charge and 10C discharge, the high-performance silicon-carbon-based negative electrode adhesive prepared in Examples 1 to 5 has a capacity retention rate of up to 88.6% after 1000 cycles. This excellent cycle performance shows that the XYZ-100 adhesive can effectively alleviate the volume expansion problem of silicon-carbon negative electrode materials during the charge and discharge process and maintain the stability and integrity of the battery structure.

[0035] The appearance of the high-performance silicon-carbon-based negative electrode adhesive prepared in Examples 1 to 5 is a light yellow transparent liquid. This appearance feature not only facilitates the observation of the uniformity and stability of the adhesive, but also reflects its good transparency and purity.

[0036] The solid content of the high-performance silicon-carbon-based negative electrode adhesive prepared in Examples 1 to 5 is 12±0.5%. This precise control of the solid content ensures the consistency of the adhesive during use and the full utilization of the effective ingredients.

[0037] New energy batteries prepared using XYZ-100 silicon-carbon-based negative electrode adhesive have excellent performance stability and reliability: Stable and reliable performance: After multiple charge and discharge cycles, the battery capacity decays slowly, showing extremely high stability and reliability. This is mainly due to the excellent adhesion and electrochemical stability of XYZ-100 to the silicon-carbon negative electrode material, which ensures the integrity of the battery's internal structure and the efficient electrochemical reaction.

[0038] Improve energy density: The application of XYZ-100 further optimizes the internal structure of the battery, reduces the ineffective space, and enables the battery to store more energy in the same volume. This not only improves the energy density of the battery, but also meets the demand for high energy density batteries in new energy vehicles, drones and other fields.

[0039] Extended cycle life: Under high-rate charge and discharge conditions, the battery can maintain a high capacity retention rate, extending the overall service life of the battery. This is due to the XYZ-100 adhesive's effective control of the volume expansion of the silicon-carbon negative electrode material and its stabilizing effect on the battery structure.

[0040] Improve production efficiency: The use of XYZ-100 simplifies the battery preparation process and reduces the complexity and difficulty of the production process. At the same time, its good processing performance significantly reduces waste in the production process, further improving production efficiency and reducing production costs.

[0041] The above embodiments are only used to illustrate the technical solutions of the present application, rather than to limit it. Although the present application has been described in detail with reference to the aforementioned embodiments, a person skilled in the art should understand that the technical solutions described in the aforementioned embodiments can still be modified, or some of the technical features can be replaced by equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the spirit and scope of the technical solutions of the embodiments of the present application.

Claims

1. A high-performance silicon-carbon-based negative electrode adhesive for new energy batteries. It is characterized in that The invention comprises the following raw materials in parts by weight: 10-15 parts of polyacrylonitrile, 8-12 parts of polyvinylidene fluoride, 14-18 parts of polyimide, 20-22 parts of polypyrrole, 7-9 parts of polyaniline, 4-6 parts of polyvinyl alcohol, 18-22 parts of nano silicon dioxide, 15-20 parts of nano carbon tubes, 15-20 parts of aziridine crosslinking agent, 8-12 parts of sodium stearate and 2-6 parts of polydimethylsiloxane.

2. A high-performance silicon-carbon-based negative electrode adhesive for new energy batteries according to claim 1, It is characterized in that The invention comprises the following raw materials in parts by weight: 10 parts of polyacrylonitrile, 8 parts of polyvinylidene fluoride, 14 parts of polyimide, 20 parts of polypyrrole, 7 parts of polyaniline, 4 parts of polyvinyl alcohol, 18 parts of nano silicon dioxide, 15 parts of nano carbon tubes, 15 parts of aziridine crosslinking agent, 8 parts of sodium stearate and 2 parts of polydimethylsiloxane.

3. A high-performance silicon-carbon-based negative electrode adhesive for new energy batteries according to claim 1, It is characterized in that The invention comprises the following raw materials in parts by weight: 15 parts of polyacrylonitrile, 12 parts of polyvinylidene fluoride, 18 parts of polyimide, 22 parts of polypyrrole, 9 parts of polyaniline, 6 parts of polyvinyl alcohol, 22 parts of nano silicon dioxide, 20 parts of nano carbon tubes, 20 parts of aziridine crosslinking agent, 12 parts of sodium stearate and 6 parts of polydimethylsiloxane.

4. A high-performance silicon-carbon-based negative electrode adhesive for new energy batteries according to claim 1, It is characterized in that The preparation method of high-performance silicon-carbon-based negative electrode adhesive for new energy batteries comprises the following steps: Step S1: weigh the following raw materials in parts by weight: 10-15 parts of polyacrylonitrile, 8-12 parts of polyvinylidene fluoride, 14-18 parts of polyimide, 20-22 parts of polypyrrole, 7-9 parts of polyaniline, 4-6 parts of polyvinyl alcohol, 18-22 parts of nano-silicon dioxide, 15-20 parts of carbon nanotubes, 15-20 parts of aziridine crosslinking agent, 8-12 parts of sodium stearate and 2-6 parts of polydimethylsiloxane, and set aside; Step S2: adding weighed polyacrylonitrile, polyvinylidene fluoride, polyimide, polypyrrole, polyaniline and polyvinyl alcohol into a reaction container, stirring and dissolving at a certain temperature to form a uniform polymer solution; Step S3: Slowly adding nano-silicon dioxide and nano-carbon tubes to the polymer solution under stirring, and continuing stirring for a period of time to ensure that the nano-filler is fully dispersed in the polymer solution; Step S4: adding aziridine crosslinking agent to the mixed solution, raising the temperature to an appropriate temperature, stirring and reacting for a certain period of time to allow the polymer to undergo a crosslinking reaction; Step S5: adding sodium stearate and continuing stirring at the same temperature for a period of time to improve the dispersion uniformity of the nanofiller in the system; Step S6: adding polydimethylsiloxane, stirring evenly, and then degassing the mixed solution; Step S7: coating the prepared adhesive solution on the silicon-carbon-based negative electrode material of the new energy battery, drying it at an appropriate temperature for a certain period of time to solidify the adhesive, thereby obtaining a high-performance silicon-carbon-based negative electrode adhesive.

5. A high-performance silicon-carbon-based negative electrode adhesive for new energy batteries according to claim 4, It is characterized in that In step S2, the temperature is set to 50-70° C., and the stirring time is set to 20-30 min.

6. A high-performance silicon-carbon-based negative electrode adhesive for new energy batteries according to claim 4, It is characterized in that In step S3, stirring is performed at room temperature for 2 to 3 hours and then heating and stirring in a water bath. The speed of the stirrer is set to 200 to 300 r / min during stirring at room temperature and to 400 to 600 r / min during heating and stirring in a water bath.

7. A high-performance silicon-carbon-based negative electrode adhesive for new energy batteries according to claim 4, It is characterized in that In step S4, the temperature is raised to 80-100° C., and the stirring time is set to 3-5 hours.

8. A high-performance silicon-carbon-based negative electrode adhesive for new energy batteries according to claim 4, It is characterized in that In step S5, the stirring speed is set to 100-150 r / min, and the stirring time is set to 60-80 min.

9. A high-performance silicon-carbon-based negative electrode adhesive for new energy batteries according to claim 4, It is characterized in that In step S7, the temperature is set to 60-80° C., and the drying time is set to 2-4 hours.