Fluorescent powder compound, fluorescent layer, fluorescent film and coating method

By using phosphor composite and temperature-controlled fluorescent layer process in Mini LED backlight technology, the problems of insufficient dispersion and settlement of phosphors are solved, the light utilization efficiency and color reproducibility are improved, the production process is simplified and the cost is reduced.

CN119020016APending Publication Date: 2024-11-26YANTAI BRIGHT OPTOELECTRONIC MATERIALS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411118942.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-15
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

In Mini LED backlight technology, insufficient dispersion of phosphor in the resin leads to inconcentration of light distribution, affecting light utilization efficiency and color reproducibility, and traditional spraying technology is difficult to avoid the problem of sedimentation of phosphor particles.

Method used

Using phosphor composite, acrylic resin is used to form hydrogen bonds with the phosphor surface by in-situ generation, which enhances its dispersion performance in the resin, and the fluorescent layer is in a semi-cured state at room temperature through temperature control, which facilitates uniform coating.

Benefits of technology

It effectively improves the dispersion and transparency of phosphor particles, improves the concentration and luminous efficiency of light distribution, simplifies the production process, and reduces costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119020016A_ABST
    Figure CN119020016A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of fluorescent films, and relates to a fluorescent powder compound, a fluorescent layer, a fluorescent film and a coating method, and the fluorescent powder compound comprises fluorescent powder and matrix resin and has a structure shown in a general formula I. According to the fluorescent powder compound, the dispersing performance of fluorescent powder particles in resin is promoted, the problem that solid-phase fluorescent powder particles are partially settled when the fluorescent powder compound is placed for a long time is effectively solved, and the transparency can also be effectively improved; a fluorescent layer prepared from the fluorescent powder compound has the characteristics that the fluorescent layer is in a semi-cured state at room temperature and can flow when the temperature rises, and when a fluorescent film is coated, the fluorescent layer can flow by increasing the temperature, so that the fluorescent film is uniformly coated on a light-emitting element, and compared with a traditional dispensing and spraying process, the fluorescent powder compound has the advantages that the production efficiency is greatly improved. The production efficiency is effectively improved, the cost is reduced, and the luminous efficiency and the light distribution concentration ratio of the product are greatly improved. # imgabs0 #
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of fluorescent films, and relates to a fluorescent powder composite, a fluorescent layer, a fluorescent film and a coating method. Background Art

[0002] Mini LED backlight technology is highly competitive in the high-end display field, with high cost performance, and is the driving force of future technology. However, there are still many technical breakthroughs in Mini LED backlight technology. With the requirements of Mini LED backlight technology in energy saving and emission reduction, in order to improve light utilization efficiency and color reproducibility, it is proposed to use a wavelength conversion layer containing phosphors such as potassium fluorosilicate (KSF) and silicates (SILICATE) as luminescent materials.

[0003] Phosphor refers to a 0-dimensional semiconductor crystal with a diameter of less than tens of nanometers. It is a substance that can emit multiple colors of light by itself, even without other devices, depending on the size and voltage of the crystal. It consists of a central core and a shell that wraps it. Different colors can be reflected according to the size of the core, that is, it controls the light absorption wavelength or emission wavelength by changing the size of the phosphor. By dispersing these processed phosphors on resin to obtain a phosphor film that can convert wavelengths, there is a significant improvement in light utilization efficiency and color reproducibility, and it can be arranged between the backlight and the liquid crystal panel for use.

[0004] When applying the fluorescent powder, a dispensing process is generally used, that is, the fluorescent particles are dispersed in a highly heat-resistant, light-transmitting resin, and micro-droplets are sprayed through a nozzle of a certain diameter to apply the fluorescent body to the entire chip. In this process, in order to better spray the micro-droplets, the resin viscosity needs to be reduced, which will cause partial sedimentation of the inorganic fluorescent particles. Partial sedimentation of the inorganic fluorescent particles may occur in the tube of the device that stores the micro-droplets, or after dispensing and before the process of curing the fluorescent paste, which reduces the dispersibility of the fluorescent particles in the resin, thereby affecting the concentration of the light distribution. Summary of the invention

[0005] In view of the deficiencies of the above-mentioned prior art, the present invention provides a phosphor composite, a phosphor layer, a phosphor film and a coating method. The specific technical solutions are as follows:

[0006] The first object of the present invention is to provide a phosphor composite, comprising phosphor and matrix resin, having a structure shown in the following general formula I:

[0007]

[0008]

[0009] R1 is selected from methyl or hydrogen, R2 is selected from alkyl and its derivatives, such as alkylamine, olefin group, alkyl glycidyl ether, alkyl hydrazine group, or aromatic group and its derivatives, such as C=C with aromatic amine, C=C with aromatic group, glycidyl ether with aromatic group, glycidyl ester with aromatic group, or R2 is selected from hydrogen atom, alkyl with 1-6 carbon atoms, alkyl with 6-15 carbon atoms and aromatic group, or the same group as R1;

[0010] X is a halogen atom, O or N.

[0011] The surface of the phosphor composite of the present invention is an in-situ generated acrylic resin, which is in full contact with the phosphor surface and forms strong hydrogen bonds with oxygen in the phosphor particles, thereby enhancing the binding ability and promoting the dispersion performance of the phosphor particles in the resin, effectively solving the problem of partial sedimentation of solid-phase phosphor particles when placed for a long time, and can also effectively improve transparency.

[0012] Furthermore, the phosphor is one or two or more of the following: Garnet series phosphors (YAG, TAG, LuAG), silicate series phosphors (SILICATE), nitride phosphors (NITRIDE), fluoride phosphors (KSF), and oxide phosphors.

[0013] Furthermore, the method for preparing the phosphor composite comprises the following steps:

[0014] The phosphor is acidified with an acidic substance, filtered and dried to obtain the acidified phosphor; the acidified phosphor is subjected to a substitution reaction with (meth)acrylic acid, after the acidic substance is substituted, a catalyst and at least one (meth)acrylate derivative with different functional groups are added to the surface of the phosphor to perform an in-situ reaction to generate an acrylic resin, thereby obtaining a phosphor composite.

[0015] Furthermore, the acidic substance is an inorganic acid, an organic acid or an acid salt, the inorganic acid is hydrochloric acid, nitric acid, sulfuric acid or carbonic acid, etc., and the organic acid is acetic acid, nitric acid, picric acid or citric acid, etc.

[0016] Furthermore, the acidification temperature is 10-150°C, preferably 20-130°C, more preferably 40-100°C, and the acidification time is 0.5-72h, preferably 1-48h, more preferably 2-24h.

[0017] Furthermore, the acidified solvent is a protic polar solvent or an aprotic polar solvent, the protic polar solvent is water, ethanol or methanol, etc., and the aprotic polar solvent is DMSO, DMF or NMP, etc.

[0018] Furthermore, the temperature of the substitution reaction is 10-150°C, preferably 20-130°C, more preferably 40-100°C, and the time of the substitution reaction is 0.1h-72h, preferably 1-48h, more preferably 2-24h.

[0019] Furthermore, the solvent for the substitution reaction is one or more of a non-aqueous protic polar solvent such as ethanol or methanol, or an aprotic polar solvent such as DMSO, DMF or NMP, or a non-polar solvent such as PGME or PGMEA.

[0020] Furthermore, the reaction temperature of the in-situ generated acrylic resin is 10-150°C, preferably 20-130°C, more preferably 40-100°C, and the reaction time of the in-situ generated acrylic resin is 0.5-72h, preferably 1-48h, more preferably 2-24h.

[0021] Further, the reaction solvent for in-situ generation of acrylic resin is a non-aqueous protic polar solvent such as ethanol and methanol, or a non-protic polar solvent such as DMSO, DMF, NMP, or one or more non-polar solvents such as PGME and PGMEA, specifically including propylene glycol monomethyl ether acetate, cyclohexanone, dipropylene glycol dimethyl ether, ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, ethylene glycol n-propyl ether, propylene glycol monomethyl ether, propylene glycol monoethyl ether, propylene glycol mono-n-propyl ether, One or more of ethylene glycol monomethyl ether acetate, ethylene glycol monoethyl ether acetate, diethylene glycol dimethyl ether, tetrahydrofuran, methyl ethyl ether, 2-heptanone, 3-heptanone, ethyl acetate, n-propyl acetate, isopropyl acetate, n-butyl acetate, isobutyl acetate, n-pentyl formate, isopentyl acetate, n-butyl propionate, ethyl butyrate, n-propyl butyrate, isopropyl butyrate, n-butyl butyrate, N,N-dimethylformamide, N-dimethylacetamide, 3-methoxybutanol and cyclopentanone.

[0022] Furthermore, the methacrylate derivative is a polymerizable compound having an ethylenically unsaturated bond.

[0023] Further, the methacrylate derivative is ethylene glycol di(meth)acrylate, trimethylolpropane di(meth)acrylate, trimethylolpropane tri(meth)acrylate, pentadienol ester, pentaerythritol tetrahydroacrylate, acryloyl acrylate with 2 to 14 acryloyl groups, methyl(meth)acrylate, ethyl(meth)acrylate, butyl(meth)acrylate, dimethylpropane tetraacrylate, cyanurate (2-oxyethyl acrylate) isocyanate, ethylene glycol phthalate, Ester, ethylene phthalate, propylene glycol propylene glycol ester, ethylene oxide trimethyl propane melamine, ethylene diphthalate, propylene diphthalate, trimethanol propylene glycol triacrylate, and compounds obtained by esterification of polyvalent alcohols such as ethylene phthalate (meth)acrylate and ethylene phthalate (meth)acrylate with α, β-unsaturated carboxylic acid esters, trimethylolpropane triethylene glycol ether (meth)acrylate derivatives, and bisphenol A dipropylene glycol ether (meth)acrylate derivatives.

[0024] Furthermore, the reaction catalyst for in-situ generation of acrylic resin is an azo compound, a peroxide compound, an acetophenone compound, an α-amino ketone compound or an α-hydroxy ketone compound.

[0025] Further, the reaction catalyst for in-situ generation of acrylic resin is 2,2'-azobis(2,4-dimethylvaleronitrile), 2,2'-azobis(2,4-dimethylbutyronitrile), 2,2'-azobis(4-methoxy-2,4-dimethylvaleronitrile), 2,2'-azobis[N-(2-propenyl)-2-methylpropionamide], 2,2'-azobis(2-methylbutyronitrile), 2,2'-azobis[2-(2-imidazoline-2-yl)propane], 1,1,1-tri(p-hydroxyphenyl)ethane and 1,2-naphthoquinonediazide-5-sulfonyl chloride condensate, benzoyl peroxide, tert-butyl benzoyl peroxide, methyl ethyl ketone peroxide, 2-benzyl The α-hydroxy ketone compound is preferably any one of 1-phenyl-2-hydroxy-2-methylpropane-1-one, 1-(4-dipropylphenyl)-2-hydroxy-2-methylpropane-1-one, 4-(2-hydroxyethoxy)phenyl-(2-hydroxy-2-propyl)ketone or 1-hydroxycyclohexyl phenyl ketone, tert-butyl peroxide, isophenyl hydroperoxide, etc.

[0026] The second object of the present invention is to provide a fluorescent layer prepared from the above fluorescent powder composite.

[0027] The fluorescent layer prepared by the fluorescent powder composite of the present invention has a modulus value greater than 150Mpa and less than 450Mpa in the temperature range of 0-25°C; greater than 0.5Mpa and less than 3Mpa in the temperature range of 60-80°C; and less than 3Mpa in the temperature range above 80°C. The fluorescent layer is in a semi-cured state at room temperature and can flow when the temperature rises. The fluorescent layer can flow by increasing the temperature, so that it can be evenly coated on the light-emitting element. The method is simple and easy to operate, which effectively improves production efficiency and reduces costs; and greatly improves the luminous efficiency and light distribution concentration of the product.

[0028] Furthermore, the fluorescent layer also includes a matrix resin layer, the matrix resin layer is made of the matrix resin, and the matrix resin layer is one layer, two layers or more.

[0029] The base resin layer can meet the requirements of high adhesion, high light transmittance, high heat resistance, high light refractive index, moisture resistance, etc.

[0030] Furthermore, when the matrix resin layer is greater than 1, the matrix resins of adjacent layers have different viscosities and / or mechanical strengths to meet different requirements.

[0031] The third object of the present invention is to provide a fluorescent film, comprising a base film and at least one fluorescent layer as described above.

[0032] Furthermore, the fluorescent layer is provided with a receiving hole, and the base film is provided with a through hole corresponding to the receiving hole.

[0033] Furthermore, the shape of the fluorescent layer is adapted to the shape of the base film.

[0034] Furthermore, the fluorescent layer is composed of a plurality of fluorescent sheets, and the plurality of fluorescent sheets are arrayed on the base film.

[0035] Furthermore, the base film is made of any one of PVC, polyacryl fluoride, PET and PI.

[0036] The above base films are made of stretchable polymer materials, which facilitates the preparation of fluorescent films in different forms.

[0037] Furthermore, the fluorescent film also includes a cover film.

[0038] Furthermore, the shape of the cover film matches the shape of the base film, that is, the shape of the cover film matches the shape of the fluorescent layer.

[0039] When the fluorescent layer is formed on the base film by a uniform array of multiple fluorescent sheets, the cover film may be a continuous sheet matching the shape of the base film, or may be composed of multiple cover film sheets matching the size of the fluorescent sheets.

[0040] Furthermore, the material of the cover film is any one of PVC, polyacryl fluoride, PET, and PI.

[0041] Furthermore, an adhesive layer is provided between the fluorescent layer and the cover film.

[0042] The adhesive layer may be a temporary adhesive layer, which allows the fluorescent layer to maintain adhesion and adhere tightly to the base film. In the packaging process, in order to coat the fluorescent layer on the LED chip, the adhesion is easily weakened when the fluorescent layer is peeled off from the base film. As the temporary adhesive layer, a material based on a mixture of a polymer resin and an ultraviolet curing polymer may be used, which has the characteristic that the adhesion is weakened by ultraviolet irradiation. The thickness of the temporary adhesive layer may be in the range of several to several tens of microns.

[0043] A fourth object of the present invention is to provide a method for coating the above fluorescent film, comprising the following steps:

[0044] The light-emitting element to be coated is placed on a heating platform, and the fluorescent layer is placed above the light-emitting element; the heating platform is heated, and the temperature rises to cause the fluorescent layer to generate fluidity, and the fluorescent layer flows to the upper surface of the light-emitting element and is coated around the light-emitting element.

[0045] Furthermore, the fluorescent film coating method specifically comprises the following steps:

[0046] Step 1: The fluorescent film is output through a supply reel, and a pickup head and a push rod are placed on the upper and lower sides of the fluorescent film respectively; the push rod presses the base film from bottom to top, and the pickup head picks up the fluorescent layer;

[0047] Step 2: Place the light-emitting element to be coated on the heating platform, and place the fluorescent layer on top of the light-emitting element by a pick-up head;

[0048] Step 3: The heating platform is heated, and the temperature rises to make the fluorescent layer fluid, and the fluorescent layer flows to the upper surface of the light-emitting element and is coated around the light-emitting element;

[0049] Step 4: The remaining base film is recovered through a recovery reel.

[0050] Furthermore, another coating method of the fluorescent film specifically comprises the following steps:

[0051] Step 1: placing the light-emitting element to be coated on a heating platform, and placing the fluorescent film on top of the light-emitting element;

[0052] Step 2: Remove the cover film on the fluorescent layer and place the fluorescent layer toward the light-emitting element;

[0053] Step 3: A pressure roller is provided above the fluorescent film, and pressure is applied to the back side of the base film in sequence through the pressure roller;

[0054] Step 4: The heating platform is heated. When the temperature rises, the fluorescent layer becomes fluid. The fluorescent layer flows to the upper surface of the light-emitting element and is coated around the light-emitting element.

[0055] The beneficial effects of the present invention are:

[0056] The phosphor composite of the present invention promotes the dispersion performance of phosphor particles in resin, effectively solves the problem of partial sedimentation of solid-phase phosphor particles when placed for a long time, and effectively improves transparency; the fluorescent layer prepared by using the phosphor composite of the present invention has the characteristics of being in a semi-cured state at room temperature and being able to flow when the temperature rises. When coating the fluorescent film, the fluorescent layer can flow by increasing the temperature, so that it can be evenly coated on the light-emitting element. Compared with traditional dispensing and spraying processes, it effectively improves production efficiency, reduces costs, and greatly improves the luminous efficiency and light distribution concentration of the product. BRIEF DESCRIPTION OF THE DRAWINGS

[0057] Figure 1 This is a schematic diagram of the structure of a fluorescent film containing a single fluorescent layer of the present invention;

[0058] Figure 2 This is a schematic diagram of the structure of the fluorescent film containing a double fluorescent layer of the present invention;

[0059] Figure 3 The schematic diagram of the structure of the fluorescent film of the present invention includes a single fluorescent layer (upper) and a single matrix resin layer (lower);

[0060] Figure 4 The schematic diagram of the structure of the fluorescent film of the present invention includes a single fluorescent layer (lower) and a single matrix resin layer (upper);

[0061] Figure 5 It is a schematic diagram of the receiving hole structure of the fluorescent film of the present invention;

[0062] Figure 6 for Figure 5 AA section view;

[0063] Figure 7 is a schematic structural diagram of a light-emitting element of the present invention;

[0064] Figure 8 It is a schematic diagram of the structure of the fluorescent film 2 of the present invention;

[0065] Fig. 9 A schematic diagram of a supply reel for storing fluorescent film 2 of the present invention;

[0066] Fig.10 It is a schematic diagram of the structure of the fluorescent film 3 of the present invention;

[0067] Fig.11 Schematic diagram of the structure of the fluorescent film 4 of the present invention;

[0068] Fig.12 is a schematic diagram of the structure of the fluorescent film 5 of the present invention;

[0069] Fig.13 The present invention is Fig.12 BB cross-sectional view;

[0070] Fig.14 It is a schematic diagram of the formation process of the base film and the fluorescent layer of the fluorescent film 2 of the present invention;

[0071] Fig.15 This is a schematic diagram of the cutting process of the first cutting line of the fluorescent film 2 of the present invention;

[0072] Fig.16 This is a schematic diagram of the cutting process of the second cutting line of the fluorescent film 2 of the present invention;

[0073] Fig.17 Schematic diagram of the stretching process of the base film of the second fluorescent film of the present invention;

[0074] Fig.18 It is a schematic diagram of the structure of the fluorescent film 2 of the present invention;

[0075] Fig.19 This is a schematic diagram of the cutting process of the first cutting line of the fluorescent film 3 of the present invention;

[0076] Fig. 20 Schematic diagram of the stretching process of the base film of the fluorescent film 3 of the present invention;

[0077] Fig.21 This is a schematic diagram of the structure of the fluorescent film 3 of the present invention after the base film is stretched;

[0078] Fig. 22 The formation process of the cover film of the fluorescent film 3 of the present invention is shown in FIG. Figure 1 ;

[0079] Fig.23 A schematic diagram of the cutting process of the second cutting line of the fluorescent film 3 of the present invention;

[0080] Fig.24 Schematic diagram of the formation process of the base film and mask of the fluorescent film 3 of the present invention;

[0081] Fig.25 It is a schematic diagram of the process of forming the fluorescent layer of the fluorescent film 3 of the present invention;

[0082] Fig.26 It is a schematic diagram of the structure of the fluorescent layer of the fluorescent film 3 of the present invention;

[0083] Fig. 27 Schematic diagram of the cutting process of the base film of the fluorescent film 3 of the present invention;

[0084] Fig.28 The formation process of the cover film of the fluorescent film 3 of the present invention is shown in FIG. Figure 2 ;

[0085] Fig.29 Schematic diagram of the formation process of the cover film of the fluorescent film 3 of the present invention Figure 3 ;

[0086] Fig.30 This is a schematic diagram of the coating process of the fluorescent film 2 of the present invention;

[0087] Fig.31 It is a schematic diagram of the picking process of the second fluorescent layer of the fluorescent film of the present invention;

[0088] Fig.32 This is a schematic diagram of the process of adding two fluorescent layers to the fluorescent film of the present invention;

[0089] Fig.33 The structure of the light-emitting element after coating is shown in FIG. Figure 1 ;

[0090] Fig.34 The pickup head structure of the present invention is shown in FIG. Figure 1 ;

[0091] Fig.35 The pickup head structure of the present invention is shown in FIG. Figure 2 ;

[0092] Fig.36 Schematic diagram of the coating process of the fluorescent film 3 of the present invention Figure 1 ;

[0093] Fig.37 Schematic diagram of the coating process of the fluorescent film 3 of the present invention Figure 2 ;

[0094] Fig.38 The structure of the light-emitting element after coating is shown in FIG. Figure 2 ;

[0095] Fig.39 It is a schematic diagram of the pressure application method using a pressure roller in the present invention;

[0096] Fig.40 Schematic diagram of the coating process of the fluorescent film 4 of the present invention;

[0097] Fig.41 It is a schematic diagram of the heating method of the present invention;

[0098] Fig.42 The structure of the light-emitting element after coating is shown in FIG. Figure 3 ;

[0099] Fig.43 It is a schematic diagram of the process of coating the fluorescent film 5 of the present invention on the light-emitting element;

[0100] Fig.44 It is a schematic diagram of the heating process during the coating process of the fluorescent film 5 of the present invention;

[0101] Fig.45 It is a schematic diagram of the cutting process of the light-emitting element after the coating of the fluorescent film 5 of the present invention;

[0102] Fig.46 It is a schematic structural diagram of a light emitting element package equipped with a light emitting element according to the present invention.

[0103] The reference numerals are recorded as follows: 100, fluorescent film; 110, base film; 111, through hole; 120, temporary adhesive layer; 130, fluorescent layer; 130a, first fluorescent layer; 130b, second fluorescent layer; 130c, base resin layer; 130' base resin paste; 131, fluorescent sheet; 132, fluorescent powder particles; 135, base resin; 136, receiving hole; 150, cover film; 151, cover film sheet; 1', light emitting element package; 2, main body; 3. Lead frame; 4. Lead; 5. Sealing part; 10. Substrate; 20. Light-emitting element; 21. Electrode; 200. Fluorescent film 2; 300. Fluorescent film 3; 400. Fluorescent film 4; 500. Fluorescent film 5; RE, supply reel; RE1, supply reel 1; W, wafer; L1, first cutting line; L2, second cutting line; M, mask; H, pick-up head; PP, push pin; RE2, recovery reel; S, heating platform; PR, pressing head; RL, pressing roller. DETAILED DESCRIPTION

[0104] The principles and features of the present invention are described below in conjunction with the accompanying drawings. The examples given are only used to explain the present invention and are not used to limit the scope of the present invention.

[0105] 1. Preparation of phosphor composites

[0106] Preparation Example 1

[0107] 1g of YAG LED phosphor was added to an aqueous solution of acetic acid with a concentration of 5%, the temperature was raised to 60°C, heated for reaction for 24h, filtered, and dried to obtain acetic acid-acidified LED phosphor. The above acetic acid-acidified phosphor was added to 100mL of PGMEA (solvent), 1.72g of methacrylic acid (Mr=86.09, 20mmol) was added to the system, heated to 130°C for reaction for 15min, 0.1g of AIBN was added as a catalyst, and 4g of methacrylate (Mr=100.12, 40mmol) was added, and the mixture was reacted at 60°C for 48h to obtain a polymethacrylate-coated LED phosphor mixture, i.e., a phosphor composite, for later use.

[0108]

[0109] Preparation Example 2

[0110] 1 g of silicate LED phosphor was added to a 5% HCl aqueous solution, the temperature was raised to 30°C, heated for reaction for 72 hours, filtered, and dried to obtain a hydrochloric acid-acidified LED phosphor. The hydrochloric acid-acidified phosphor was added to 100 mL of ethyl acetate (solvent), 2.58 g of methacrylic acid (Mr=86.09, 30 mmol) was added to the system, heated to 150°C for reaction for 60 minutes, 0.15 g of 2-benzyl-2-dimethylamino-1-(4-morpholinophenyl)-butane-1-one was added as a catalyst, and 7.81 g of hydroxyethyl methacrylate (Mr=130.14, 60 mmol) was added, and the mixture was reacted at 100°C for 24 hours to obtain a polymethacrylate-coated LED phosphor mixture, i.e., a phosphor composite, for later use.

[0111]

[0112] 2. Preparation of fluorescent film

[0113] Figure 1 The structure of a fluorescent film 100 including a single fluorescent layer is shown, and the fluorescent film 100 includes a base film 110, a fluorescent layer 130 and a cover film 150 for protecting the fluorescent layer are formed on the base film 110. In this embodiment, a temporary adhesive layer 120 is provided between the base film 110 and the fluorescent layer 130. In this embodiment, the material of the base film 110 is PVC, and it can also be any one of polyamide fluoride, PET, and PI.

[0114] The fluorescent layer 130 includes fluorescent powder particles 132 and a matrix resin 135. Figure 2-Figure 4Schematic diagrams of fluorescent film structures of other fluorescent layer structures are shown, wherein the fluorescent layer 130 includes a first fluorescent layer 130a and a second fluorescent layer 130b, or the fluorescent layer 130 includes a first fluorescent layer 130a and a matrix resin layer 130c. The matrix resin materials of each layer of the fluorescent layer 130 may have different properties. For example, the matrix resin 135 constituting the first fluorescent layer 130a has a higher strength than the matrix resin 135 constituting the second fluorescent layer 130b, so that the fluorescent layer 130 can stably maintain its shape. In addition, the matrix resin 135 constituting the second fluorescent layer 130b has a higher adhesive force than the matrix resin 135 of the first fluorescent layer 130a, so that it is easy to bond with the light emitting element 20. Figure 3 As shown, it includes a first fluorescent layer 130a containing fluorescent powder particles 132, and a transparent layer matrix resin layer 130c without fluorescent powder particles 132, and the matrix resin layer 130c is below the first fluorescent layer 130a. Figure 4 As shown, the base resin layer 130c is above the first fluorescent layer 130a, and the base resin layer 130c is a transparent layer to allow light to pass through better.

[0115] The shape of the cover film 150 is matched with the shape of the base film 110 , and the shape of the cover film 150 is matched with the shape of the fluorescent layer 130 . In this embodiment, the material of the cover film 150 is PVC, and it can also be any one of polyamide fluoride, PET, and PI.

[0116] See also Figure 5-Figure 7 , a receiving hole 136 is provided on the fluorescent layer 130, and a through hole 111 is provided on the base film 110 corresponding to the receiving hole 136. The receiving hole 136 can be formed into a structure that passes through the fluorescent layer 130 corresponding to the position and structure of the electrode 21 of the light-emitting element 20. Therefore, even if the fluorescent layer 130 is placed on the light-emitting element 20 during the packaging process, the electrode 21 of the light-emitting element 20 is accommodated in the receiving hole 136 and is not covered by the fluorescent layer 130 but exposed to the outside. Thereafter, the wires can be stably combined with the wires, and therefore, the possibility of deformation of the wires during the packaging process can be avoided. Figure 6 As shown, when the receiving hole 136 is provided in the fluorescent layer 130, a through hole 111 corresponding to the receiving hole 136 is provided in the base film 110, so that a structure that penetrates the fluorescent film 100 as a whole can be formed. Figure 7In the embodiment, an example is given of forming an electrode 21 on the light emitting element 20, but this electrode structure is not limited thereto, and a plurality of electrodes 21 may be provided. In this case, the receiving hole 136 may be formed corresponding to the plurality of electrodes 21. The receiving hole 136 and the through hole 111 may be formed by punching or laser irradiation, or may be formed by etching. Here, the light emitting element 20 includes an LED chip having a semiconductor layer and an active layer, and the upper surface of the light emitting element 20 may have at least one electrode 21.

[0117] More spacers (not shown) can be added to the fluorescent layer 130. When the fluorescent layer 130 is applied to the target material, the spacers can help maintain the coating thickness, and the thickness of the spacers can be the same size as the thickness to be applied. In order to prevent the optical properties from being reduced, the spacers can use inorganic or organic materials with excellent light transmittance. Alternatively, when light is to be reflected on the surface of the spacer, an inorganic or organic material with a reflective layer having a high light reflectivity can be used.

[0118] Figure 8 The structure of the fluorescent film 200 of the present invention is shown. The fluorescent film 200 of this embodiment has a structure in which the fluorescent layer 130 is pre-cut according to a predetermined specification. That is, the fluorescent layer 130 is composed of a plurality of fluorescent sheets 131 having a predetermined size and spaced at predetermined intervals. Similarly, each fluorescent sheet 131 constituting the fluorescent layer 130 can be composed of a single layer or a plurality of layers. Figure 2-Figure 4 As shown. In addition, the cover film 150 is composed of a plurality of cover film sheets 151 of a size corresponding to the fluorescent sheet 131. The size of the fluorescent sheet 131 or the intervals therebetween is determined according to the object to which the fluorescent sheet 131 is to be coated. For example, when a plurality of light-emitting elements are applied to an arranged substrate, it can be determined according to the size of the light-emitting elements and the intervals therebetween. The plurality of fluorescent sheets 131 can be arranged one-dimensionally along a single direction or two-dimensionally. In addition, although not shown in the figure, the plurality of fluorescent sheets 131 can be respectively formed into corresponding to the positions of the electrodes arranged in the light-emitting elements. Figure 5 The receiving hole 136 is shown.

[0119] Fig. 9 Shows how to store Figure 8 In this embodiment, the fluorescent film 200 is in a strip shape, which is a structure that can be easily stored in a reel form. Fig. 9 The fluorescent film 200 of this embodiment is stored and kept by supplying a reel RE. When stored in this form at room temperature, the required number of fluorescent sheets 131 are heated and coated with a target substance when used. Although the fluorescent sheets 131 are shown to be arranged one-dimensionally on the fluorescent film 200, this is exemplary and is not limited thereto.

[0120] Fig.10The structure of the fluorescent film 300 of another embodiment of the present invention is shown. The fluorescent layer 130 of the fluorescent film 300 of this embodiment is composed of a plurality of fluorescent sheets 131 having a predetermined size and spaced at predetermined intervals, and the cover film 150 is composed of an integral film covering the plurality of fluorescent sheets 131. This is similar to the embodiment of the present invention. Figure 8 There are differences between the embodiments shown. In this embodiment, the fluorescent sheet 131 can be arranged in one dimension or in two dimensions. The fluorescent film 300 of this embodiment can also be arranged in a Fig. 9 The roll-type storage is shown in FIG. 1 , and the cover film 150 is separated from the fluorescent layer 130 when in use. Similarly, although not shown in the figure, the plurality of fluorescent sheets 131 can be as shown in FIG. Figure 2-Figure 4 As shown in FIG. 1 , the fluorescent sheet 131 is composed of multiple layers, and each fluorescent sheet 131 can be formed to correspond to the position of the electrode set in the light emitting element. Figure 6 The receiving hole 136 is shown.

[0121] Fig.11 FIG. 4 shows the structure of a fluorescent film 400 of another embodiment of the present invention. In this embodiment, the base film 110, the fluorescent layer 130 and the cover film 150 are respectively composed of an integral film. The fluorescent film 400 can have a strip shape and can have a shape that is easy to store in a roll-type manner, such as Fig. 9 Similarly, the fluorescent layer 130 can be as shown. Figure 2-Figure 4 As shown in FIG. 1 , the fluorescent layer 130 may be formed according to the position and arrangement interval of the LED chips, corresponding to the position of the electrodes set in each light-emitting element. Figure 3 The receiving hole 136 is shown. In addition, the cover film 150 is separated from the fluorescent layer 130 when in use.

[0122] Fig.12 and Fig.13 The structure of the fluorescent film 500 of another embodiment of the present invention is schematically shown. In this embodiment, the fluorescent film 500 has a shape corresponding to the wafer W as a whole, so that the plurality of light-emitting elements 20 grown on the wafer W by a CVD device or the like are uniformly covered in a horizontal state of the wafer W before being cut. In addition, according to the arrangement interval of the plurality of light-emitting elements 20 arranged on the wafer W, a plurality of receiving holes 136 may be provided corresponding to the positions of the electrodes 21 on each light-emitting element 20. Similarly, the fluorescent layer 130 may be as shown in FIG. Figure 2-Figure 4 As shown, the substrate 110 is composed of multiple layers. Through holes 111 corresponding to the receiving holes 136 formed on the fluorescent layer 130 can be formed on the base film 110. If a cover film 150 is provided, the cover film 150 will be used separately from the fluorescent layer 130.

[0123] Preparation Example 3

[0124] See also Figure 14-18, as shown in Figure 8 The method for preparing the fluorescent film 200 according to the embodiment of the present invention shown in the figure specifically comprises the following steps:

[0125] Step 1: first prepare a base film 110, form a fluorescent layer 130 on the base film 110, and form a cover film 150 on the fluorescent layer 130, see Figure 14-15 ;

[0126] Step 2: Cut the fluorescent layer 130 and the cover film 150 into blocks of a predetermined size; specifically, cut the fluorescent layer 130 along a plurality of first cutting lines L1 arranged in parallel in one direction on the fluorescent layer 130 and the cover film 150, and then cut along a second cutting line L2 perpendicular to the first cutting line L1, wherein the second cutting line L2 cuts the base film 110, the fluorescent layer 130 and the cover film 150 into strips, see Figure 15-16 ;

[0127] Step 3, see Fig.17 , the strip-shaped base film 110 is stretched along the length direction to obtain a fluorescent film, such as Fig.18 As shown, the fluorescent layer 130 of the fluorescent film 200 is divided into a plurality of fluorescent body sheets 131, and the cover film 150 is also divided into a plurality of cover film sheets 151. Fig. 9 As shown, the prepared fluorescent film 200 can be easily stored in a roll form.

[0128] Preparation Example 4

[0129] See also Fig.11 , Figure 19-Figure 23 , as shown in Fig.10 The method for preparing the fluorescent film 300 of the embodiment of the present invention shown in the figure specifically comprises the following steps:

[0130] Step 1: first prepare a base film 110, and then form a fluorescent layer 130 on the base film 110, see Fig.14 ;

[0131] Step 2, see Fig.19 , cutting the fluorescent layer 130 along a plurality of first cutting lines L1 arranged in parallel in one direction on the fluorescent layer 130;

[0132] Step three, such as Fig. 20 As shown, the base film 110 is stretched to the left and right sides. Fig.21 As shown, the fluorescent layer 130 of the fluorescent film 200 is divided into a plurality of regions by the first cutting line L1;

[0133] Step 4: Fig. 22 As shown, a cover film 150 is formed on the fluorescent layer 130 , and a temporary adhesive layer (not shown) may be further formed on the surface where the cover film 150 and the fluorescent layer 130 are combined.

[0134] Step 5: Fig.23 As shown, the substrate 110, the fluorescent layer 130 and the cover film 150 are cut along a second cutting line L2 which is perpendicular to the first cutting line L1. The second cutting line L2 cuts the base film 110, the fluorescent layer 130 and the cover film 150 in strips to prepare the substrate 110, the fluorescent layer 130 and the cover film 150. Figure 6 The fluorescent film 300 is shown. Fig. 9 As shown, the prepared fluorescent film 300 can be easily stored in a roll form.

[0135] Preparation Example 5

[0136] See also Figure 24-28 , as shown in Fig.10 Another method for preparing the fluorescent film 300 of the embodiment of the present invention shown in FIG. 1 specifically includes the following steps:

[0137] Step 1, see Fig.24 First, a base film 110 is prepared, and a mask M having a plurality of holes is provided on the base film 110, wherein the size and interval of the plurality of holes of the mask M are determined according to the size and interval of the fluorescent sheet to be manufactured;

[0138] Step 2, such as Fig.25 As shown, by printing a matrix resin paste 130' mixed with fluorescent particles in a plurality of holes of a mask M, a fluorescent layer 130 having a plurality of fluorescent sheets 131 is formed in the plurality of holes of the mask M, see Fig.26 ,exist Fig.26 FIG. 1 shows a single-layer fluorescent layer 130 formed by printing, but is not limited thereto. Figure 2-Figure 4 The fluorescent layer 130 having a multi-layer structure is shown;

[0139] Step three, such as Fig. 27 As shown, Fig.26 The structure shown is cut into strips;

[0140] Step 4: Fig.28 As shown in FIG. 1 , a cover film 150 is formed on the fluorescent layer 130. Fig. 9 As shown, the prepared fluorescent film 300 can be stored in a roll-up format.

[0141] In the above-mentioned fluorescent film preparation process, the order of step 3 and step 4 can be adjusted, such as Fig.29 As shown, you can first Fig.26 A cover film 150 is formed on the fluorescent layer 600 of the structure shown, and then cut into strips to form a fluorescent film three.

[0142] 3. Coating method of fluorescent film

[0143] Example 1

[0144] As Fig.18Taking the fluorescent film 200 as an example, the present invention provides a method for coating a fluorescent film, which specifically includes the following steps:

[0145] Step 1: The fluorescent film 200 is output through the supply reel RE1, the cover film 150 on the fluorescent layer 130 is peeled off, and the pickup head H and the push rod PP are placed on the upper and lower sides of the fluorescent film respectively;

[0146] See also Fig.30 , is a schematic diagram of the coating process of the fluorescent film 200 of this embodiment, wherein a supply reel 1 RE1 for supplying the fluorescent film 200, a base film 110, a pickup head H for picking up the fluorescent sheet 131 and the cover film 151, a push pin PP, and a recycling reel RE2 for the base film 110 are arranged. In addition, if a temporary adhesive layer is formed between the base film 110 and the fluorescent sheet 131, ultraviolet light irradiation can be used to weaken the adhesive force before the subsequent steps.

[0147] Step 2: See Fig.31 , the push rod PP presses the base film 110 upward from the bottom, and the pickup head H picks up the fluorescent layer 130 and the cover film 150;

[0148] A clamp C in contact with the object is installed on the pickup head H. A plurality of vacuum microtubes (not shown) can be formed on the surface of the clamp C, and the target object can be picked up by adsorption through the vacuum microtubes formed on the pickup head H. The clamp C can be made of materials such as rubber, metal, and heat-resistant engineering plastics.

[0149] Step 3: See Fig.32 , placing the substrate 10 with the wire-bonded light-emitting element 20 to be coated on the heating platform S, and the pickup head H places the fluorescent layer 130 above the light-emitting element 20;

[0150] Step 4: The heating platform S is heated, and the fluorescent layer 130 and the cover film 150 on the fluorescent layer 130 are close to the light-emitting element. The temperature is increased by the heating platform S, and the fluorescent layer 130 generates fluidity, such as Fig.33 As shown, the fluorescent layer 130 flows to the upper surface of the light emitting element 20 and is coated around the light emitting element 20;

[0151] Step 5: The remaining base film is recovered through a recovery reel.

[0152] Fig.34 and Fig.35 FIG. 2 shows an exemplary structure of different embodiments of a clamp C mounted on a pickup head H, which can be used in the above-mentioned embodiment 1. In the embodiment 1, the clamp C can be a flat type or a flat type. Fig.34 and Fig.35The same cavity type. This cavity acts as a frame to maintain a constant shape when picking up the cover film 151 and the fluorescent sheet 131. The depth of the cavity is greater than the thickness of the cover film 151, and can be less than the sum of the thickness of the cover film 151 and the fluorescent sheet 131. The inner wall of the cavity can be inclined at a right angle, such as Fig.34 As shown, it can also be an obtuse angle, such as Fig.35 shown.

[0153] See also Fig.41 The fluorescent sheet 131 of this embodiment can also be directly heated by the pickup head H, or indirectly heated by the heating platform S of the main body 2 on which the light-emitting element 20 is installed, so as to generate fluidity, and fall from the cover film 151 by its own weight, flow onto the light-emitting element 20, and coat the light-emitting element 20 including the wires.

[0154] See also Fig.42 The fluorescent layer 130 formed by the fluorescent sheet 131 on the light emitting element 20 is coated along the shape of the wire and has a shape corresponding to the shape of the wire. Fig.42 In the light emitting element package shown in , two electrodes are provided on the upper surface of the light emitting element 20, thereby showing a structure connected with two wires, but the number of electrodes and wires can be changed in various ways. In addition, a sealing portion (not shown) that covers and protects the light emitting element 20 having the fluorescent layer 130 can also be formed on the main body 2.

[0155] Example 2

[0156] As Fig.10 Take the fluorescent film 300 as an example, see Fig.36 The present invention provides a method for coating a fluorescent film, which adopts a method of directly applying pressure, and specifically comprises the following steps:

[0157] Step 1, providing the fluorescent film 300 from the supply reel 1 RE1, first removing the cover film 150, and arranging the fluorescent film 300 so that the fluorescent sheet 131 faces the light emitting element 20;

[0158] Step 2: Place the substrate 10 with the light emitting element 20 wire-bonded on a heating platform S, and apply pressure to the back of the base film 110 on which the fluorescent sheet 131 is placed by a pressing head PR;

[0159] Step 4: As the fluorescent sheet 131 approaches the light emitting element 20, heat causes the fluorescent sheet 131 to become fluid, and the fluorescent sheet 131 flows to the upper surface of the light emitting element 20 and is coated around the light emitting element 20. The base film 110 behind the fluorescent sheet 131 is recovered using the recovery reel RE2.

[0160] See also Fig.37 and Fig.38In this embodiment, a plurality of fluorescent sheets 131 can be simultaneously coated on a plurality of light emitting elements 20 by using a larger size pressing head PR, and the fluorescent film 300 can be Fig.36 Alternatively, the fluorescent film 300 can be arranged in a shape according to the shape of the light emitting element 20, and the cover film 150 can be peeled off from the fluorescent film 300 before use.

[0161] See also Fig.39 In this embodiment, the pressure roller RL can be used to replace Fig.36 and Fig.37 The pressing head PR shown in the figure applies pressure to the back side of the base film 110 in sequence through the pressing roller RL, so that the plurality of fluorescent sheets 131 are coated on the plurality of light-emitting elements 20 in sequence. The fluorescent film 300 can be as shown in FIG. Fig.36 Alternatively, the fluorescent film 300 can be arranged in a shape according to the shape of the light emitting element 20, and the cover film 150 can be peeled off from the fluorescent film 300 before use.

[0162] Example 3

[0163] As Fig.11 Take the fluorescent film 400 shown as an example, see Fig.40 , which is different from the second embodiment, a plurality of light emitting elements 20 can be coated by a pressing roller RL and a stamping method. In this embodiment, the fluorescent layer 130 is formed by Fig.11 The fluorescent film 29400 shown in the figure has the cover film 150 of the fluorescent film 29400 removed before coating. After the fluorescent layer 130 is coated in a form that surrounds the entirety of the plurality of light-emitting elements 20, it is cut into units of each light-emitting element 20. In this embodiment, it is also possible to coat around the plurality of light-emitting elements 20 at one time by directly applying pressure, and the rest is the same as in Embodiment 2 and will not be described in detail.

[0164] In the description of the above fluorescent layer coating method, a light-emitting element wire-bonded to a substrate is used as an example, but it is not limited thereto. The technical solution of the present invention is applicable to array-type, flip-chip structure and other light-emitting elements used in PCB applications.

[0165] Figure 43 to Figure 45 and Fig.46 The schematic diagram of the structure of the light-emitting element after coating according to other embodiments of the present invention is briefly described.

[0166] Fig.43 The stage of coating the fluorescent film 500 on the light emitting element 20 is shown. The fluorescent film 500 is coated on the light emitting element 20 so that each receiving hole 136 and the electrode 21 of each light emitting element 20 coincide with each other, so that the electrode 21 of each light emitting element 20 is connected through the corresponding receiving hole 136. Then, as shown in FIG. Fig.44As shown, the base film 110 is removed, the fluorescent layer 130 is made fluid by heating, and the fluid fluorescent layer 130 flows around the light emitting element 20 except the electrode 21, so that at least a portion of the upper surface and the side surface of the light emitting element 20 is covered by the fluorescent layer 130.

[0167] As described above, the fluorescent layer 130 is coated on a plurality of light emitting elements 20 together, and then cut into individual light emitting elements 20 coated with the fluorescent layer 130 by a cutting process, such as Fig.45 shown.

[0168] Fig.46 The light emitting device package 1' carrying the light emitting device 20 is shown. Fig.45 Each light emitting element 20 separated from the package is mounted on the lead frame 3 of the main body 2, and the electrode 21 not coated with the fluorescent layer 130 is electrically connected to the lead frame 3 through the lead 4. In addition, the light emitting element 20 and the lead 4 are manufactured into a light emitting element package 1' through a packaging process sealed by a sealing part 5.

[0169] The technical solution of the present invention is used to coat the fluorescent layer of the light-emitting element. Since there is no need to physically press the light-emitting element bonded by the wire, the possibility of deformation in the wire can be fundamentally eliminated, which has the advantage of improving the reliability of the light-emitting element. Since the fluorescent layer is formed to cover the upper surface of the light-emitting element and the side including the active layer, the occurrence of light leakage can be effectively prevented, thereby improving the light extraction efficiency. Since the fluorescent layer is manufactured and coated in the form of a film with a certain thickness, it has the advantages of reducing thickness deviation and reducing the dispersion distribution between products as a whole.

[0170] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.

Claims

1. A phosphor composite, characterized in that: The invention comprises phosphor and matrix resin, and has a structure shown in the following general formula I: Wherein, the base resin is 1≤a<20; 1≤b<20; R1 is selected from methyl or hydrogen, R2 is selected from alkyl and its derivatives, or R2 is selected from any one of hydrogen, alkyl with 1 to 6 carbon atoms, alkyl with 6 to 15 carbon atoms and aromatic group, or the same group as R1; X is a halogen atom, O or N.

2. The phosphor composite according to claim 1, characterized in that: The phosphor is one or two or more of a Garnet series phosphor, a silicate series phosphor, a nitride type phosphor, a fluoride type phosphor, and an oxide type phosphor.

3. The phosphor composite according to claim 1, characterized in that: The preparation method comprises the following steps: The phosphor is acidified with an acidic substance, filtered and dried to obtain the acidified phosphor; the acidified phosphor is subjected to a substitution reaction with methacrylic acid, after the acidic substance is substituted, a catalyst and at least one methacrylate derivative with different functional groups are added to the surface of the phosphor to perform an in-situ reaction to generate an acrylic resin, thereby obtaining a phosphor composite.

4. A fluorescent layer, characterized in that: The phosphor composite is prepared from the phosphor composite according to any one of claims 1 to 3.

5. The fluorescent layer according to claim 4, characterized in that: It also includes a base resin layer, which is prepared from the base resin, and the base resin layer is one layer, two layers or more.

6. A fluorescent film, characterized in that: It comprises a base film and at least one fluorescent layer as claimed in claim 4 or 5.

7. The fluorescent film according to claim 6, characterized in that: The fluorescent film further includes a cover film.

8. The fluorescent film according to claim 6, characterized in that: The fluorescent layer is provided with a receiving hole, and the base film is provided with a through hole corresponding to the receiving hole.

9. The fluorescent film according to claim 6, characterized in that: The fluorescent layer is composed of a plurality of fluorescent sheets, and the plurality of fluorescent sheets are arrayed on the base film.

10. A method for coating a fluorescent film, characterized in that: Using the fluorescent film as described in claims 6-9, comprising the following steps: The light-emitting element to be coated is placed on a heating platform, and the fluorescent layer is placed above the light-emitting element; the heating platform is heated, and the temperature rises to cause the fluorescent layer to generate fluidity, and the fluorescent layer flows to the upper surface of the light-emitting element and is coated around the light-emitting element.