Method for reducing C-type inclusions of strip steel through calcium treatment technology in argon station
By feeding calcium wire and carbon powder into the argon blowing process after the furnace in the smelting of low carbon steel strip, low-melting-point 3CaO·Al2O3 inclusions are generated, which solves the problem of silicate inclusions and improves the purity of molten steel and the quality of cold-rolled strip.
Patent Information
- Application Number
- CN202411129676.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-16
- Publication Date
- 2024-11-26
AI Technical Summary
Existing technologies are insufficient to effectively reduce Class C inclusions formed by silicate products during the smelting of low-carbon steel strip, leading to abnormal rolling quality of the steel.
In the smelting process of low carbon steel strip, calcium wire and carbon powder are fed in during the argon blowing process after the furnace. Ca reacts with O to generate CaO, forming 3CaO·Al2O3 with a low melting point, which promotes the floating of inclusions. CO2 is generated by blowing in carbon powder to reduce the presence of Si and Al oxides.
It effectively reduces Class C inclusions in molten steel, improves the purity of molten steel, reduces the risk of deformation and fracture during cold rolling, and improves the quality of cold-rolled premium strip.
Smart Images

Figure CN119020552A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of strip steel smelting using Si and Al for deoxidation during low-carbon steel strip steel smelting, and in particular to the field of reducing C-type inclusions during smelting. Background Art
[0002] Deoxidation is a reaction that reduces the oxygen content in steel during the steelmaking and casting process. It is an important process to ensure the quality of ingots (billets) and steel products. Oxygen exists in the molten steel in the form of dissolved or non-metallic inclusions. During the oxygen blowing steelmaking process, as the impurity content decreases, the [O] content in the molten steel increases. If the undeoxidized molten steel is poured out of the furnace, the oxygen dissolved in the molten steel will react with carbon during the condensation process, precipitate bubbles and boil; the characteristics of the precipitated gas vary significantly with the degree of deoxidation. The fully deoxidized molten steel has no bubbles precipitated during the condensation process, does not boil, and is calm, so it is called killed steel; the slightly deoxidized molten steel has carbon and oxygen react during the condensation process, precipitates bubbles, and has obvious boiling phenomenon, which is boiling steel; the partially deoxidized molten steel, after solidification for a period of time, the remaining oxygen reacts with carbon to produce a short-term boiling, which is semi-killed steel. Deoxidation of boiling steel, i.e. mild deoxidation, only slightly reduces the oxygen content in the molten steel, but still exceeds the content required for equilibrium with carbon. Deoxidation of semi-killed steel, i.e. partial deoxidation, can roughly make the oxygen content of the steel reach the content of equilibrium with carbon, so it is also called balanced steel. Deoxidation of killed steel, i.e. full deoxidation, makes the oxygen content of the steel much lower than the content of equilibrium with carbon. Although deoxidation of molten steel reduces the [O] content, if the deoxidation products are not floated and removed, but remain in the molten steel to form non-metallic inclusions in the steel, it will affect the quality of the steel; therefore, deoxidation products should be removed as much as possible during deoxidation. Therefore, deoxidation is to reduce the total oxygen content in the steel. However, no matter how the steelmaking technology develops and improves, there will always be inclusions remaining in the steel. Therefore, during deoxidation, the shape, size and distribution of the residual inclusions must be controlled to ensure the various properties of the steel.
[0003] Class C inclusions usually refer to silicate inclusions in molten steel, which is a type of non-metallic inclusions in molten steel. They mainly come from the deoxidation and alloying period of silicon-deoxidized steel, and Class C inclusions are mainly formed in this stage. Class C inclusions have the characteristics of irregular distribution and high ductility in silicon-deoxidized steel products. Therefore, in the subsequent steel rolling process, if the grade of Class C inclusions is too high, it will cause abnormal quality of steel rolling. Therefore, reducing Class C inclusions in molten steel is an important task.
[0004] When Si is dissolved in steel, it can increase the hardness and plasticity of the steel and reduce its toughness. At the same time, Si alloy also participates in the steelmaking process as a deoxidizer. Therefore, in the steelmaking process, if Si alloy is used as a deoxidizer and performance guarantee, Si will be oxidized to form SiO 2For example, Q195C steel is deoxidized with Al, and Al is oxidized to form Al 2 O 3 , SiO 2 Then with Al 2 O 3 Inclusions react to form silicates, so silicate production is a process that cannot be bypassed.
[0005] The existing method for treating silicate products without going through a refining furnace (reducing atmosphere refining process) is to blow argon through the argon station after the converter furnace, and use the characteristic that the silicate product has a lower density than molten steel to promote its floating. Under the conditions of this method, although some silicate products can be promoted to float, it is impossible to refine and shrink the silicate products. Therefore, although some silicate products float, the inclusion grade (diameter) is still relatively large. Summary of the invention
[0006] The technical problem to be solved by the present invention is: when the strip steel is low-carbon steel and Si and Al are used for deoxidation during the strip steel smelting, how to reduce the strip steel C-type inclusions composed of silicate products.
[0007] The technical scheme adopted by the present invention is: a method for reducing C-type inclusions in steel strip by using calcium treatment technology in an argon station. The steel strip is low-carbon steel and Si and Al are used for deoxidation during steel strip smelting. During steel strip smelting, calcium wire is fed into the argon blowing process after the furnace to make Ca in the molten steel react with O to produce CaO, and CaO reacts with Al 2 O 3 Formation of 3CaO.Al 2 O 3 , remove 3CaO.Al floating on the upper layer of molten steel 2 O 3 .
[0008] In the post-furnace argon blowing process, carbon powder is blown in to make the carbon content in the molten steel above the average of the upper and lower limits of the carbon content of the steel grade.
[0009] Calcium wire is fed into the post-furnace argon blowing process, and the molar ratio of calcium in the calcium wire to the molar ratio of Al added during deoxidation is 2 / 3-3 / 2.
[0010] The working principle of the present invention is that the present invention utilizes Al2O3 in molten steel to react with CaO to form 3CaO with low melting point. 2 O 3 ,3CaO.A 2 O 3 The inclusions float and are easy to remove, so the C-type inclusions in the molten steel can be reduced. In the present invention, carbon powder is blown in, and carbon combines with O at high temperature to form CO 2, thereby reducing the presence of Si and Al oxides in the molten steel, and also reducing the C-type inclusions composed of silicates. At the same time, the elemental Si can increase the hardness and plasticity of the steel and reduce toughness.
[0011] The beneficial effects of the present invention are as follows: the present invention can effectively reduce the C-type inclusions in molten steel, promote the improvement of the purity of molten steel, provide support for the subsequent improvement of the quality of cold-rolled high-quality strips, and reduce the risk of fracture caused by cold-rolled processing deformation. BRIEF DESCRIPTION OF THE DRAWINGS
[0012] Figure 1 This is a schematic diagram of type C inclusions in strip steel; Figure 2 It is a schematic diagram of a carbon powder blowing device; Among them, 1. argon gas tube, 2. funnel base, 3. funnel body, 4. conveying column with external spiral blades, 5. stepping rotary motor, 6. coupling, 7. carbon powder. DETAILED DESCRIPTION
[0013] The steel grade of the strip in this embodiment is Q195 (by mass percentage: C: 0.06-0.12%, Mn: 0.25-0.50%, Si: ≤0.30%, S: ≤0.050%, P≤0.045, and the rest are iron and indispensable impurities.), which is a carbon structural steel with a yield strength of 195MPa. This is a low-strength steel with good plasticity and toughness. The chemical composition of Q195 mainly includes carbon, manganese, silicon and other elements. The carbon content of Q195 steel is relatively low. The manganese content is used to increase the strength, and the silicon content helps to increase the hardness of the steel. In terms of mechanical properties, Q195 steel has a high elongation and good cold bending performance, which is suitable for the production of various structural parts. Its elongation is generally greater than 32%, and its cold bending performance is good. It is suitable as strip steel. When smelting using the existing production process, Si and Al are used for deoxidation, and Al is oxidized to form Al 2 O 3 , SiO 2 Then with Al 2 O 3 Inclusions such as MgO react to form silicates, so silicate products cannot be bypassed. When producing strip steel, the strip steel contains more C-type inclusions, such as Figure 1 As shown in Figure 2, Class C inclusions in silicon-deoxidized steel products have the characteristics of irregular distribution and high ductility. Therefore, in the subsequent steel rolling process, if the level of Class C inclusions is too high, it will cause quality abnormalities in steel rolling.
[0014] In this embodiment, a high calcium wire is fed into the argon blowing process after the furnace to make Ca in the molten steel react with O to produce CaO. CaO reacts with Al 2 O 3 Formation of 3CaO.Al2 O 3 ; Working principle: The argon station feeds high calcium wire to promote Al in molten steel 2 O 3 The CaO generated by the calcium treatment reaction forms 3CaO.Al with a low melting point 2 O 3 This method can reduce the SiO 2 With Al 2 O 3 The amount of silicate inclusions formed by the reaction.
[0015] Production operation: In the argon blowing process of the converter argon blowing station, a wire feeder is used to quickly feed 0.30kg / t high calcium wire into the molten steel at a speed of 3.5m / s, and then a soft blowing process is carried out to promote 3CaO.Al 2 O 3 Inclusions float up; Advantages of this process: The use of this process can improve the purity of molten steel, provide support for the subsequent improvement of the quality of cold-rolled high-quality strips, and reduce the risk of cold-rolled fractures due to processing deformation.
[0016] In one embodiment, during the post-furnace argon blowing process, carbon powder is blown in to make the carbon content in the molten steel equal to or higher than the average of the upper and lower limits of the carbon content of the steel grade, which is 0.11% by mass in this embodiment. Figure 2 As shown, it includes a funnel and an argon gas pipe 1. The stepping rotary motor 5 installed on the funnel cover drives the conveying column 4 with an outer spiral blade to rotate through the coupling 6. When the conveying column 4 with an outer spiral blade rotates, the carbon powder 7 in the funnel body 3 is driven to mix into the argon gas through the funnel base 2. The carbon powder is quickly mixed into the molten steel through the argon gas and combines with the O in the molten steel to form CO 2 , thereby reducing the presence of Si and Al oxides in the molten steel.
[0017] In one embodiment, in the post-furnace argon blowing process, on the one hand, carbon powder is blown into the argon gas to adjust the C mass percentage in Q195 (the current C mass percentage content needs to be measured before the post-furnace argon blowing process), and carbon powder is blown in so that the carbon content in the molten steel is above the average of the upper and lower limits of the carbon content of the steel grade, and the required amount of C is calculated, and then a carbon powder blowing device is used to blow it into the molten steel. After blowing C, the carbon content in the molten steel is 0.11% by mass. Subsequently, high calcium wire is fed, and in the argon blowing process of the converter argon blowing station, a wire feeder is used to quickly feed 0.30kg / t high calcium wire into the molten steel at a speed of 3.5m / s, and a soft blowing process is subsequently performed to promote 3CaO.Al 2 O 3 Inclusions float up, and then 3CaO.Al is removed 2 O 3 Inclusions.
[0018] When calculating the required amount of C, the total amount of molten steel is x (the upper limit of the carbon content of the steel grade is 0.12% - the current C mass percentage content of 0.09% needs to be measured before the argon blowing process after the furnace). In fact, some C is converted into carbon monoxide or carbon dioxide in the molten steel and discharged. The final carbon content must be less than the upper limit of the carbon content of the steel grade to meet the material requirements.
Claims
1. A method for reducing C-type inclusions in steel strip by calcium treatment technology using an argon station, wherein the steel strip is low carbon steel and Si and Al are used for deoxidation during steel strip smelting, characterized in that: During strip steel smelting, calcium wire is fed into the argon blowing process behind the furnace to make Ca in the molten steel react with O to produce CaO. CaO reacts with Al2O3 to form 3CaO.Al2O3, and the 3CaO.Al2O3 floating on the upper layer of the molten steel is removed.
2. The method of reducing C-type inclusions in steel strip by using calcium treatment technology in an argon station according to claim 1, characterized in that: In the post-furnace argon blowing process, carbon powder is blown in to make the carbon content in the molten steel above the average of the upper and lower limits of the carbon content of the steel grade.
3. The method of reducing C-type inclusions in steel strip by using calcium treatment technology in an argon station according to claim 1, characterized in that: Calcium wire is fed into the post-furnace argon blowing process, and the molar ratio of calcium in the calcium wire to the molar ratio of Al added during deoxidation is 2 / 3-3 / 2.