Stainless steel AOD furnace refining slag fluxing modifier, modification method and application

By using fluorine-containing, iron-containing, limestone and aluminum-containing fluorine-containing fluorine-containing, limestone and aluminum-containing fluorine-containing fluorine-containing fluorine-containing fluorine-containing fluorine-containing fluorine-containing fluorine-containing fluorine-containing fluorine-containing fluorine-containing fluorine-containing fluorine-containing fluorine-containing fluorine-containing fluorine-containing fluorine-containing fluorine-containing fluorine Reuse and reduction of environmental pollution.

CN119020555APending Publication Date: 2024-11-26WUHAN HAIYITONG SPECIAL MATERIAL TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411114649.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-14
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

During the cooling process of the stainless steel AOD furnace refining slag, tricalcium silicate decomposes to produce free calcium oxide. Dicalcium silicate transforms from high-temperature crystal form to low-temperature crystal form, resulting in a significant reduction in gelling activity and cannot be used in resource, resulting in environmental pollution and high maintenance. cost.

Method used

A stainless steel AOD furnace refining slag melting modifier, including fluorine-containing raw materials, iron-containing raw materials, limestone, aluminum-containing raw materials, binding agents and modification additives, is generated through reasonable iron-calcium ratio and thermodynamic conditions reaction. Low melting point calcium ferrite inhibits the crystalline transformation of calcium silicate and forms a highly active gelled material.

Benefits of technology

Without changing the smelting conditions and increasing material consumption, the free calcium oxide content is significantly reduced, volume expansion and powdering are avoided, gelling activity is improved, and the resource utilization of refined residue is achieved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119020555A_ABST
    Figure CN119020555A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of stainless steel smelting slag treatment, and particularly relates to a stainless steel AOD furnace refining slag fluxing modifier, a modification method and application. The fluxing modifier comprises the following components in parts by weight: 50-80 parts of a fluorine-containing raw material, 0-10 parts of an iron-containing raw material, 0-10 parts of limestone, 5-25 parts of an aluminum-containing raw material, 1-5 parts of a binding agent and 1-5 parts of a performance additive. On the premise of not changing smelting conditions, not increasing material consumption and not influencing the quality of molten steel, the fluxing modifier is adopted to replace traditional fluorite balls to serve as a fluxing material, meanwhile, in-furnace modification of the AOD refining slag is achieved, it is avoided that due to decomposition of tricalcium silicate, high free calcium oxide is caused, and due to conversion of dicalcium silicate, the gelation activity is reduced, and the service life of the AOD refining slag is prolonged. And a favorable material basis is provided for subsequent treatment. The modified refining slag is crushed and ground to a certain fineness, and the cementing material with high activity is obtained, so that resource reutilization is realized.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of stainless steel smelting slag treatment, and more specifically, relates to a stainless steel AOD furnace refining slag fluxing modifier, a modification method and an application thereof. Background Art

[0002] In recent years, with the increasing requirements for the development of metallurgical processes towards green and high environmental protection levels, the problems of stainless steel slag treatment and disposal, as a by-product produced in the stainless steel smelting process, have become increasingly prominent. Solving the environmental pollution problem caused by stainless steel slag has received attention and concern from various steel companies.

[0003] The composition of AOD furnace refined slag is mainly CaO and SiO2, and the rest is a small amount of Al2O3, MgO, FeO, Cr2O3, MnO, etc. Its main mineral phase is similar to cement clinker, mainly tricalcium silicate (C3S) and dicalcium silicate (C2S), which has a certain gelling activity. However, when cooling, tricalcium silicate (C3S) first decomposes to produce a large amount of free calcium oxide (f-CaO), and then dicalcium silicate (C2S) changes from high-temperature crystal form to low-temperature crystal form, resulting in volume expansion and pulverization, accompanied by a significant decrease in gelling activity. This change causes the performance of AOD refined slag to fail to meet the minimum requirements of GB / T 2847-1996 "Volcanic ash mixed materials used in cement", and the poor hydration stability makes it impossible to form effective utilization. As the smelting continues, the amount of AOD furnace refined slag continues to increase, and it has not been used as a resource, so it can only continue to increase the stockpile. Over the years, the land occupation has become larger and larger, the environmental pollution has become more and more serious, and the maintenance cost has become higher and higher. With the continuous production, the treatment and disposal of stainless steel slag is imminent. Summary of the invention

[0004] In view of the defects of the prior art, the purpose of the present invention is to provide a fluxing modifier, modification method and application of stainless steel AOD furnace refining slag, aiming to solve the technical problems of the prior art that tricalcium silicate (C3S) contained in the AOD furnace refining slag decomposes to produce a large amount of free calcium oxide (f-CaO) when cooling, and dicalcium silicate (C2S) transforms from a high-temperature crystal form to a low-temperature crystal form, resulting in volume expansion and pulverization, accompanied by a significant reduction in gelling activity, and cannot be recycled.

[0005] To achieve the above object, the present invention provides a flux modifier for stainless steel AOD furnace refining slag, which comprises, by weight, 50 to 80 parts of fluorine-containing raw materials, 0 to 10 parts of iron-containing raw materials, 0 to 10 parts of limestone, 5 to 25 parts of aluminum-containing raw materials, 1 to 5 parts of binders, and 1 to 5 parts of modification aids;

[0006] The main component of the fluorine-containing raw material is calcium fluoride, the main component of the iron-containing raw material is iron element and / or iron oxide, the main component of the aluminum-containing raw material is Na3AlF6, and the binder is a bonding agent; the modification aid is used to reduce the melting point of the flux modifier, modify the AOD furnace refining slag, and inhibit the crystal transformation of calcium silicate.

[0007] Preferably, the fluorine-containing raw material is one or more of fluorite ore, fluorite flotation powder, fluorine-containing sludge, and fluorine chemical by-products.

[0008] Preferably, the iron-containing raw material is one or more of iron scale, iron powder, iron concentrate, and steel mill scale.

[0009] Preferably, the aluminum-containing raw material is cryolite, and its main elements and their mass fractions are: F 48-53 parts, Al 0-25 parts, K+Na 0-30 parts, C 0-1.0 parts, S 0-0.5 parts, P 0-0.1 parts.

[0010] Preferably, the binder is one or more of vegetable gum or modified starch.

[0011] Preferably, the modification aid is one or more of boron oxide, boric acid or calcium borate.

[0012] According to another aspect of the present invention, a method for preparing the flux modifier is provided, wherein the ingredients are prepared according to the proportion of each component, granulated after uniform mixing, and the granulated particles are dried and cooled to room temperature to obtain the flux modifier.

[0013] According to another aspect of the present invention, there is provided an application of the flux modifier, which is used to perform furnace refining modification on stainless steel AOD furnace to obtain modified refined slag. The flux modifier does not change the traditional smelting process, does not increase material consumption, and does not affect the quality of molten steel when used.

[0014] According to another aspect of the present invention, a method for refining and modifying a stainless steel AOD furnace using the flux modifier to obtain modified refined slag is provided, wherein the flux used in the refining process of the stainless steel AOD furnace is replaced with the flux modifier, and the refining and modification is performed to obtain the modified refined slag.

[0015] In general, the above technical solution conceived by the present invention has the following technical advantages compared with the prior art:

[0016] The present invention adopts the flux modifier proposed by the present invention to replace the traditional fluorite ball as a flux material without changing the smelting conditions, increasing the material consumption and affecting the quality of molten steel, and at the same time realizes the in-furnace modification of AOD refined slag. Compared with the unmodified refined slag, the high-activity tricalcium silicate and dicalcium silicate phases are improved, the decomposition of tricalcium silicate (C3S) to form free calcium oxide is greatly reduced, and the transformation of dicalcium silicate (C2S) from a high-density and high-activity β-Ca2SiO4 crystal form to a low-density and low-activity γ-Ca2SiO4 crystal form is avoided, and the high free calcium oxide (f-CaO) generated after the refined slag is cooled, the gelling activity is reduced, and the volume expansion due to different crystal density forms pulverization is solved, providing a favorable material basis for subsequent processing. The modified refined slag is crushed and ground to a certain fineness, that is, a gelling material with high activity is obtained, thereby achieving resource recycling. BRIEF DESCRIPTION OF THE DRAWINGS

[0017] Figure 1 This is a photo of the refined slag obtained in the modified smelting process of Example 1 after cooling;

[0018] Figure 2 is a photograph of the refined slag obtained in the unmodified smelting process of Example 1 after cooling;

[0019] Figure 3 1 is the XRD diagram of the refined slag obtained in the unmodified and modified smelting processes of Example 1;

[0020] Figure 4 This is a photo of the refined slag obtained in the modified smelting process of Example 2 after cooling;

[0021] Figure 5 This is a photograph of the refined slag obtained in the unmodified smelting process of Example 2 after cooling;

[0022] Figure 6 These are the XRD diagrams of the refined slag obtained in the unmodified and modified smelting processes of Example 2, respectively.

[0023] Figure 7 This is a photo of the refined slag obtained in the modified smelting process of Example 3 after cooling;

[0024] Figure 8 is a photograph of the refined slag obtained in the unmodified smelting process of Example 3 after cooling;

[0025] Fig. 9 These are the XRD diagrams of the refined slag obtained in the unmodified and modified smelting processes of Example 3, respectively. DETAILED DESCRIPTION

[0026] In order to solve the technical problems of the prior art AOD furnace refining slag being seriously pulverized, having low gelling activity, and being unable to be utilized as resources, the present invention provides a flux modifier for stainless steel AOD furnace refining slag, which comprises, by weight, 50 to 80 parts of fluorine-containing raw materials, 0 to 10 parts of iron-containing raw materials, 0 to 10 parts of limestone, 5 to 25 parts of aluminum-containing raw materials, 1 to 5 parts of binders, and 1 to 5 parts of modifying aids; the main component of the fluorine-containing raw materials is calcium fluoride, and the main component of the iron-containing raw materials is iron element and / or iron oxide; the binder is a bonding agent, which is used to bond the components together to form a particle size that meets the specification requirements, and to form a strength sufficient to support transportation and use after drying; the main component of the aluminum-containing raw materials is Na3AlF6, and the modifying aid is used to reduce the melting point of the flux modifier, modify the AOD furnace refining slag, and inhibit the crystal transformation of calcium silicate.

[0027] The flux modifier proposed in the present invention generates low-melting calcium ferrite by reacting under thermodynamic and kinetic conditions in a smelting furnace through a reasonable iron-calcium ratio, and fuses the flux material with the modifying material, thereby having the functions of fluxing and modifying AOD refined slag. The test found that the stainless steel AOD furnace refined slag modified by the flux modifier of the present invention has a greatly reduced free calcium oxide (f-CaO) content compared with the unmodified refined slag, and the low-density, low-activity γ-Ca2SiO4 crystal form is not detected. It is speculated that the possible reason is that the modification aid of the present invention melts into the calcium silicate crystal phase at high temperature, avoiding the decomposition of tricalcium silicate (C3S) in the modified AOD refined slag to form free calcium oxide (f-CaO), and avoiding the high-density, high-activity β-Ca2SiO4 crystal form in dicalcium silicate (C2S) The phase is transformed into a low-density, low-activity γ-Ca2SiO4 crystal form as the temperature decreases, reducing the volume expansion caused by the density change caused by the crystal phase transformation, thereby avoiding the pulverization of the refined slag.

[0028] Preferably, the stainless steel AOD furnace refined slag flux modifier provided by the present invention comprises, by weight, 60 to 80 parts of fluorine-containing raw materials, 5 to 10 parts of iron-containing raw materials, 1 to 5 parts of limestone, 10 to 20 parts of aluminum-containing raw materials, 1 to 5 parts of binders, and 1 to 5 parts of modification aids.

[0029] In some embodiments, the fluorine-containing raw material is one or more of fluorite ore, fluorite flotation powder, fluorine-containing sludge, and fluorine chemical by-products; preferably, the main chemical components and their mass fractions contained in the fluorine-containing raw material are: CaF2 70.0-85.0 parts, CaCO3 0-15.0 parts, SiO2 0-15.0 parts, Al2O30-10 parts, K2O+Na2O 0-5.0 parts, S 0-1.0 parts, and P 0-0.1 parts.

[0030] Further preferably, the main chemical components and their mass fractions of the fluorine-containing raw material are: CaF2 70.0-85.0 parts, CaCO3 5-10.0 parts, SiO2 5-15.0 parts, Al2O3 2-5 parts, S 0.05-0.2 parts.

[0031] Preferably, the iron-containing raw material is one or more of iron scale, iron powder, iron concentrate, and steel rolling mill skin; preferably, the main chemical components of the iron-containing raw material and their mass fractions are: T.Fe50.0-80.0 parts, SiO2 0-15.0 parts, Al2O30-10 parts, MgO+CaO 0-10.0 parts, S 0-0.3 parts, and P 0-0.1 parts.

[0032] In some embodiments, the main chemical components of the iron-containing raw material and their mass fractions are: T.Fe55.0-65.0 parts, SiO2 5-10.0 parts, Al2O3 1-5 parts, MgO+CaO 0.5-5 parts, S 0.1-0.3 parts.

[0033] In some embodiments, the aluminum-containing raw material is cryolite, and its main element composition and its mass fraction are: F 48-53 parts, Al 0-25 parts, K+Na 0-30 parts, C 0-1.0 parts, S 0-0.5 parts, P0-0.1 parts. The aluminum-containing raw material of the present invention is cryolite, which can be natural cryolite or self-prepared cryolite, for example, recycled cryolite can be obtained by flotation of electrolytic aluminum slag.

[0034] In a preferred embodiment, the main elements and their mass fractions in the aluminum-containing raw material are: F 48-53 parts, Al 20-25 parts, K+Na 20-30 parts, S 0.1-0.5 parts.

[0035] Here, only the main components and mass fractions of fluorine-containing raw materials, iron-containing raw materials and aluminum-containing raw materials are listed. In fact, they may also contain other trace metal oxides and other components. T.Fe in iron-containing raw materials is the total content of iron, that is, all elemental iron, iron oxide, iron compounds, etc. are calculated as iron, which is the main indicator for evaluating iron ore.

[0036] The binder of the present invention includes but is not limited to one or more of plant gum or modified starch. In some embodiments, plant gum is a natural adhesive extracted from plants or an adhesive obtained by processing natural gum, such as xanthan gum, guar gum, carboxymethyl cellulose, etc. Modified starch is a derivative obtained by changing the molecular structure and physicochemical properties of natural starch through appropriate chemical or physical treatment, including but not limited to pregelatinized starch, oxidized starch, cross-linked starch, maltodextrin, etc.

[0037] In some embodiments, the modification aid is one or more of boron oxide, boric acid or calcium borate. The above modification aids can be industrial grade. In a preferred embodiment, the content of the main component of each modification aid is ≥ 99.5%. For example, the main component of the boron oxide modification aid is B2O3, the main component of the boric acid modification aid is H2BO3, and the main component of the calcium borate modification aid is CaBO3.

[0038] The present invention also provides a method for preparing the flux modifier, wherein the ingredients are prepared according to the proportion of each component, granulated after being evenly mixed, and the granulated particles are dried and cooled to room temperature to obtain the flux modifier;

[0039] In some embodiments, the granulated particles are heated to 80-150°C and 10000-30000m 3 After air drying for 0.5-2h at 400 °C / h, the mixture is naturally cooled to room temperature to obtain the flux modifier.

[0040] The flux modifier provided by the present invention can be used to perform furnace refining modification on a stainless steel AOD furnace to obtain modified refined slag. The content of free calcium oxide (f-CaO) in the obtained modified refined slag is greatly reduced, and low-density, low-activity γ-Ca2SiO4 crystals are not detected, thereby solving the technical problem of severe pulverization of the AOD furnace refined slag after cooling in the prior art.

[0041] The method of using the flux modifier of the present invention to refine and modify the stainless steel AOD furnace to obtain modified refined slag comprises the following steps: replacing the flux used in the refining process of the stainless steel AOD furnace with the flux modifier of the present invention, and refining and modifying to obtain modified refined slag. In some embodiments, the flux used in the refining process of the AOD furnace is fluorite balls. During the application process, the flux used in the refining process of the stainless steel AOD furnace is replaced with an equal amount of the flux modifier of the present invention.

[0042] In some embodiments, the method of refining and modifying a stainless steel AOD furnace using the flux modifier to obtain refined slag comprises the following steps:

[0043] (1) Calculate the amount of alloy and lime added according to the molten iron composition, temperature, scrap steel amount, and target molten steel composition, and determine the basic amount of fluorite balls added;

[0044] (2) The oxidation period is carried out according to the original process, and the temperature at the end of the oxidation period is 1650-1700°C;

[0045] (3) When entering the reduction period, various reducing alloys are added according to the original process. The flux modifier is added in an amount equal to the basic amount of fluorite balls, and no more fluorite balls are added. The side-blowing oxygen gun supplies oxygen for 1-3 minutes, and the temperature is appropriately supplemented depending on the temperature in the furnace;

[0046] (4) The rest is carried out according to the normal reduction process and steel tapping operation, and the temperature after reduction is 1550-1600°C.

[0047] Experimental results show that the flux modifier of the present invention is used to replace the fluorite balls used in the stainless steel AOD furnace refining process in the AOD smelting furnace, and the smelting thermodynamics and kinetic conditions are fully utilized to perform flux modification on the refined slag, and the modified quality is uniform and the effect is stable; the technical problem of serious pulverization of the AOD furnace refined slag after cooling in the prior art is cleverly solved. While performing flux modification on the refined slag, the flux modifier does not change the smelting process, does not increase material consumption, and does not affect the quality of molten steel.

[0048] In order to make the purpose, technical scheme and advantages of the present invention clearer, the technical scheme in the embodiment of the present invention will be clearly and completely described in conjunction with the embodiments of the present invention. It should be understood by those skilled in the art that the embodiments are only to help understand the present invention and should not be regarded as specific limitations of the present invention. Based on the embodiments in the present invention, all other embodiments obtained by ordinary technicians in the field without making creative work are within the scope of protection of the present invention.

[0049] The embodiments of the present invention are implemented on the premise of the technical solution of the present invention, and detailed implementation methods and processes are given, but the protection scope of the present invention is not limited to the following embodiments. The process parameters of the following embodiments that do not specify specific conditions are usually based on conventional conditions.

[0050] The endpoints and any values ​​of the ranges disclosed in the present invention are not limited to the precise ranges or values, and these ranges or values ​​should be understood to include values ​​close to these ranges or values. For numerical ranges, the endpoint values ​​of each range, the endpoint values ​​of each range and the individual point values, and the individual point values ​​can be combined with each other to obtain one or more new numerical ranges, which should be regarded as specifically disclosed in the present invention.

[0051] In the present invention, unless otherwise specified and / or described, the numerical values ​​of the percentage content of the components are "mass percentages". The process parameters in the following examples that do not specify specific conditions are usually based on conventional conditions.

[0052] The following are examples:

[0053] Example 1

[0054] The present embodiment discloses a stainless steel AOD furnace refining flux modifier, the ingredients of which are composed by weight: 65% fluorine-containing raw material, 7% iron-containing raw material, 3% limestone, 20% cryolite, 3% modification aid, and 2% binder.

[0055] Among them, the requirements for each raw material are as follows:

[0056] (1) The fluorine-containing raw material is a mixture of fluorite flotation powder and fluorine chemical by-products, and the chemical composition by weight percentage is: CaF2 77.0%, CaCO3 9.0%, SiO2 10.4%, Al2O3 3.5%, S 0.1%;

[0057] (2) The iron-containing raw material is iron concentrate, and the main chemical components by mass percentage are: T.Fe 62%, SiO2 7.7%, Al2O3 2.1%, CaO 1.3%, S 0.3%;

[0058] (3) The main chemical components of the limestone are as follows: CaO 52.3%, SiO2 4.8%, Al2O3 1.8% by weight;

[0059] (4) The main chemical composition of the cryolite is Na3AlF6, and the mass percentages of the main elements are: F 53%, Al22.3%, Na 24.5%, S 0.2%;

[0060] (5) The binder is pregelatinized starch;

[0061] (6) The modification aid is boric acid, and the main content of B2O3 is ≥99.5%.

[0062] The preparation method of the flux modifier is as follows:

[0063] (1) Add fluorine-containing raw materials, iron-containing raw materials, limestone, electrolytic aluminum slag, modification additives, and binders into a mixer according to the component ratio, and add 5% water for high-speed stirring to form a uniform mud material, so that it can be held in the hand and fall apart with a light touch;

[0064] (2) The above-mentioned sludge is evenly conveyed into a high-pressure roller granulator through a conveyor for granulation, and the particle size is controlled to be 5-50 mm after screening;

[0065] (3) Sent to the drying kiln, with hot air temperature of 150°C and air volume of 10,000m 3 / h for 1 hour and then naturally cooled to room temperature, thereby obtaining the flux modifier.

[0066] The chemical composition of the obtained flux modifier is: CaF2 50.1%, TFe 4.4%, CaO 5.0%, SiO2 7.5%, Al2O3 2.5%, Na3AlF6 19.8%, B2O3 1.7%, S 0.1%, and ignition loss 8.9%.

[0067] The flux modifier is added to the high-level silo of the AOD furnace and the original smelting process is followed:

[0068] (1) Calculate the amount of alloy and lime added according to the molten iron composition, temperature, scrap steel amount, and target molten steel composition, and determine the basic amount of fluorite balls to be 2000 kg;

[0069] (2) Add 2.5t lime when mixing steel, top lance oxygen flow rate 4669Nm 3 / h, main gun oxygen flow rate 5095Nm 3 / h, argon flow rate 790Nm 3 / h, after blowing for 10 minutes, add 12500kg of high carbon ferrochrome, 5000kg of scrap steel and 3085kg of steel grit, continue blowing for 13 minutes, lift the top gun and shake the furnace to remove 70-80% of the slag;

[0070] (3) Add 3 tons of lime, top lance oxygen flow rate 4595 Nm 3 / h, main gun oxygen flow rate 5068Nm 3 / h, argon flow rate 716Nm 3 / h, after blowing for 15 minutes, lift the top gun, add 2t of lime, 1562kg of high carbon ferromanganese, and adjust the oxygen flow rate of the main gun to 5103Nm 3 / h, argon flow rate 734Nm 3 / h, after blowing for 30 minutes, adjust the oxygen flow rate of the main gun to 1417Nm 3 / h, nitrogen flow rate 2044Nm 3 / h, argon flow rate 588Nm 3 / h, shake the furnace to take carbon samples to measure the temperature, and the temperature at the end of oxidation is measured to be 1690℃;

[0071] (4) When entering the reduction period, add 1600kg of low-carbon ferromanganese, 7580kg of medium-silicon ferromanganese, and the flux modifier of this embodiment in an amount equal to the amount of fluorite balls added to the base. No more fluorite balls are added. The oxygen flow rate of the main gun is adjusted to 1417Nm 3 / h, nitrogen flow rate 2044Nm 3 / h, the main gun was closed after blowing oxygen for 1.5 minutes, and nitrogen was blown for 7 minutes, and the furnace was shaken to take the reduction sample for temperature measurement. The temperature after reduction was measured to be 1590℃;

[0072] (5) According to the requirements of molten steel composition, add 130kg of copper plate and shake the furnace to drain more than 80% of the slag before tapping.

[0073] Among them, when step (4) uses fluorite balls, it is the original process, an unmodified smelting process, and an unmodified refined slag is obtained; in step (4), the fluorite balls are replaced with an equal amount of the flux modifier of Example 1, which is a modified smelting process, and a modified refined slag is obtained.

[0074] The experimental results show that according to this method, the flux modifier can completely replace the fluorite spheroidizing slag and modify the refined slag without changing the smelting process, increasing material consumption, and affecting the quality of molten steel. The modified refined slag is grayish white and does not pulverize after natural cooling. Figure 1 As shown in the figure, the refined slag obtained without modification is completely powdered after cooling, as shown in the figure. Figure 2 shown.

[0075] The chemical composition of modified and unmodified AOD furnace refined slag was analyzed in detail by X-ray fluorescence spectrometry, and the test results are shown in Table 1. The results show that the modified slag and unmodified slag have similar compositions, proving that the modification treatment has no significant effect on the refined slag.

[0076] Table 1 Main components of modified and unmodified slag

[0077]

[0078] X-ray diffraction (XRD) technology was used to identify the main mineral phases in the slag. Figure 3 shown.

[0079] Figure 3 The results show that the main phases of the unmodified slag and the modified slag are the same, namely tricalcium silicate, dicalcium silicate, periclase and calcite. The phases of each mineral in the modified slag and the unmodified slag are roughly the same, but the modified slag lacks the low-temperature γ-Ca2SiO4 crystal phase compared to the unmodified slag, indicating that the modification treatment preserves the original mineral phase and crystal form of the steel slag and inhibits the transformation of the high-temperature β-Ca2SiO4 crystal form to the low-temperature γ-Ca2SiO4 crystal form. β-Ca2SiO4 has high activity, while γ-Ca2SiO4 has extremely low activity. Inhibiting the crystal transformation means retaining the high-activity phase, which improves the gelling activity of the refined slag after cooling. At the same time, the density of β-Ca2SiO4 is 3.28g / cm 3 , the density of γ-Ca2SiO4 is 2.97g / cm 3 There is a 10% difference between the two, which inhibits the crystal transformation, that is, reduces the volume expansion and pulverization caused by the density difference. The modification treatment inhibits the crystal transformation, that is, solves the problem of reduced activity and pulverization of the refined slag at the same time.

[0080] The set process parameters and actual production data were strictly compared as shown in the following table. According to the on-site operation records and operator feedback, there was no abnormality. The composition of the modified molten steel is shown in Table 2. The results showed that the modification treatment had no effect on the smelting of the AOD furnace and the composition of the molten steel.

[0081] Table 2 Composition of modified molten steel

[0082]

[0083] The modified refined slag powder has the properties shown in Table 3 after crushing and grinding:

[0084] Table 3 Physical property test results of modified refined slag obtained after unmodified and modified smelting treatment in Example 1

[0085]

[0086]

[0087] As can be seen from Table 3, when the modifier of this embodiment is not used for modified smelting, the obtained refined slag has extremely low gelling activity, and the high free calcium oxide leads to unqualified hydration stability, which cannot meet the basic requirements for use as an active material. However, after the flux modifier of this embodiment is used for modified smelting, the gelling activity of the obtained modified refined slag is increased to >70%, the free calcium oxide is greatly reduced, the stability meets the qualified requirements, and the performance is greatly improved, meeting the requirements for use as an active material in cement and concrete production.

[0088] Example 2

[0089] The present embodiment discloses a stainless steel AOD furnace refining flux modifier, the ingredients of which are composed by weight: 75% of fluorine-containing raw material, 7% of iron-containing raw material, 1% of limestone, 10% of regenerated cryolite obtained by flotation of electrolytic aluminum slag, 5% of modification aid, and 2% of binder.

[0090] Among them, the requirements for each raw material are as follows:

[0091] (1) The fluorine-containing raw material is a mixture of fluorite ore and fluorine chemical by-products, and the chemical composition by weight percentage is: CaF281.0%, CaCO3 7.1%, SiO2 8.6%, Al2O3 3.2%, S 0.1%;

[0092] (2) The iron-containing raw material is iron scale, and the main chemical components by mass percentage are: T.Fe 62%, SiO2 7.7%, Al2O3 2.1%, %, CaO 1.3%, S 0.3%;

[0093] (3) The main chemical components of the limestone are as follows: CaO 52.3%, SiO2 4.8%, Al2O3 1.8% by weight;

[0094] (4) The main chemical composition of regenerated cryolite is Na3AlF6, and the mass percentages of the main elements are: F 53%, Al22.3%, Na 24.5%, S 0.2%;

[0095] (5) The binder is carboxymethyl cellulose;

[0096] (6) The modification aid is calcium borate, and the content of the main component CaBO3 is ≥99.5%.

[0097] The preparation method of the flux modifier is as follows:

[0098] (1) Add fluorine-containing raw materials, iron-containing raw materials, limestone, cryolite, modification aids, and binders into a mixer according to the component ratio, and add 5% water for high-speed stirring to form a uniform mud material, so that it can be held in the hand and fall apart with a light touch;

[0099] (2) The above-mentioned sludge is evenly conveyed into a high-pressure roller granulator through a conveyor for granulation, and the particle size after screening is controlled to be 5-50 mm;

[0100] (3) Sent to the drying kiln, with hot air temperature of 100°C and air volume of 30,000m 3 / h for 1 hour and then naturally cooled to room temperature, thereby obtaining the flux modifier.

[0101] The chemical composition of the obtained flux modifier is: CaF2 60.8%, TFe 4.4%, CaO 6.0%, SiO2 7.1%, Al2O3 2.6%, Na3AlF6 9.8%, B2O3 2.8%, S 0.1%, and ignition loss 6.4%.

[0102] The flux modifier is added to the high-level silo of the AOD furnace and the original smelting process is followed:

[0103] (1) Calculate the amount of alloy and lime added according to the molten iron composition, temperature, scrap steel amount, and target molten steel composition, and determine the basic amount of fluorite balls to be 1900 kg;

[0104] (2) 3.3t lime was added when mixing steel, and the top lance oxygen flow rate was 4386Nm 3 / h, main gun oxygen flow rate 5293Nm 3 / h, argon flow rate 706Nm 3 / h, after blowing for 10 minutes, add 15700kg of high carbon ferrochrome, 2000kg of scrap steel and 5100kg of steel sand, continue blowing for 16 minutes, lift the top gun and shake the furnace to remove 70-80% of the slag;

[0105] (3) Add 3 tons of lime, top lance oxygen flow rate 4541Nm 3 / h, main gun oxygen flow rate 5205Nm 3 / h, argon flow rate 663Nm 3 / h, after blowing for 14 minutes, lift the top gun, add 3t of lime, 2542kg of high carbon ferromanganese, and adjust the oxygen flow rate of the main gun to 5102Nm 3 / h, argon flow rate 667Nm 3 / h, after blowing for 36 minutes, adjust the oxygen flow rate of the main gun to 1418Nm 3 / h, nitrogen flow rate 2028Nm 3 / h, argon flow rate 725Nm 3 / h, shake the furnace to take carbon samples to measure the temperature, and the temperature at the end of oxidation is measured to be 1693℃;

[0106] (4) When entering the reduction period, add 350kg of low-carbon ferromanganese, 8000kg of medium-silicon ferromanganese, and a flux modifier equal to the amount of fluorite balls added to the base. No more fluorite balls are added. Adjust the oxygen flow rate of the main gun to 1418Nm 3 / h, nitrogen flow rate 2028Nm 3 / h, the main gun was closed after blowing oxygen for 1.5 minutes, and nitrogen was blown for 7 minutes, and the furnace was shaken to take the reduction sample for temperature measurement. The temperature after reduction was measured to be 1580℃;

[0107] (5) According to the requirements of molten steel composition, 140 kg of copper plate is added, and the furnace is shaken to discharge more than 80% of the slag before tapping the steel; wherein, when fluorite balls are used in step (4), it is the original process, an unmodified smelting process, and unmodified refined slag is obtained; and when the fluorite balls are replaced with an equal amount of flux modifier in step (4), it is a modified smelting process, and modified refined slag is obtained.

[0108] According to this method, the flux modifier can completely replace the fluorite spheroidized slag and modify the refined slag without changing the smelting process, increasing material consumption, or affecting the quality of molten steel. The refined slag modified by the flux modifier of this embodiment does not pulverize when cooled naturally and is gray-green. Figure 4 As shown; the unmodified refined slag is severely powdered, as shown Figure 5 shown.

[0109] The chemical composition of modified and unmodified AOD furnace refined slag was analyzed in detail by X-ray fluorescence spectrometry, and the test results are shown in Table 4. The results show that the modified slag and unmodified slag have similar compositions, proving that the modification treatment has no significant effect on the refined slag.

[0110] Table 4 Main components of modified and unmodified slag

[0111]

[0112] X-ray diffraction (XRD) technology was used to identify the main mineral phases in the slag. Figure 6 shown.

[0113] The main physical phases of the unmodified slag and the modified slag are the same, namely tricalcium silicate, dicalcium silicate, periclase and calcite. The results show that the physical phases of each mineral in the modified slag and the unmodified slag are roughly the same. Compared with the unmodified slag, the physical phase of the modified slag lacks the low-temperature γ-Ca2SiO4 crystal phase, indicating that the modification treatment preserves the original mineral phase and crystal form of the steel slag and inhibits the transformation of the high-temperature β-Ca2SiO4 crystal form to the low-temperature γ-Ca2SiO4 crystal form. β-Ca2SiO4 has high activity, while γ-Ca2SiO4 has extremely low activity. Inhibiting the crystal transformation means retaining the high-activity phase, which improves the gelling activity of the refined slag after cooling. At the same time, the density of β-Ca2SiO4 is 3.28g / cm 3 , the density of γ-Ca2SiO4 is 2.97g / cm 3 There is a 10% difference between the two, which inhibits the crystal transformation, that is, reduces the volume expansion and pulverization caused by the density difference. The modification treatment inhibits the crystal transformation, that is, solves the problem of reduced activity and pulverization of the refined slag at the same time.

[0114] The set process parameters and actual production data were strictly compared as shown in the following table. According to the on-site operation records and operator feedback, there were no abnormalities. The results are shown in Table 5, indicating that the modification treatment had no effect on the smelting of the AOD furnace and the composition of the molten steel.

[0115] Table 5 Composition of modified molten steel in Example 2

[0116]

[0117] After crushing and grinding, the unmodified and modified refined slag powders have the following properties:

[0118] Table 6 Physical property test results of modified refined slag obtained after unmodified and modified smelting treatment in Example 2

[0119]

[0120] As can be seen from Table 3, when the modifier of this embodiment is not used for modified smelting, the obtained refined slag has extremely low gelling activity, and the high free calcium oxide leads to unqualified hydration stability, which cannot meet the basic requirements for use as an active material. However, after the flux modifier of this embodiment is used for modified smelting, the gelling activity of the obtained modified refined slag is increased to >70%, the free calcium oxide is greatly reduced, the stability meets the qualified requirements, and the performance is greatly improved, meeting the requirements for use as an active material in cement and concrete production.

[0121] Example 3

[0122] The present embodiment discloses a stainless steel AOD furnace refining flux modifier, the ingredients of which are composed by weight: 78% of fluorine-containing raw material, 0% of iron-containing raw material, 0% of limestone, 15% of regenerated cryolite obtained by flotation of electrolytic aluminum slag, 3% of modification aid, and 4% of binder.

[0123] Among them, the requirements for each raw material are as follows:

[0124] (1) The fluorine-containing raw material is selected fluorite powder, and the chemical composition by weight is: CaF2 71.5%, CaCO3 11.3%, SiO2 14.0%, Al2O3 3.0%, S 0.2%;

[0125] (2) The main chemical composition of regenerated cryolite is Na3AlF6, and the mass percentage of elements is: F50%, Al 24.8%, Na 25%, S 0.2%;

[0126] (3) The binder is maltodextrin;

[0127] (4) The modification aid is boron oxide, and the content of the main component B2O3 is ≥99.5%.

[0128] The preparation method of the flux modifier is as follows:

[0129] (1) Add fluorine-containing raw materials, regenerated cryolite, modification aids, and binders into a blender according to the component ratio, and add 5% water for high-speed stirring to form a uniform mud material, so that it can be held in the hand and dispersed by light touch;

[0130] (2) The above-mentioned sludge is evenly conveyed into a high-pressure roller granulator through a conveyor for granulation, and the particle size after screening is controlled to be 5-50 mm;

[0131] (3) Sent to the drying kiln, with hot air temperature of 120℃ and air volume of 20000m 3 / h for 1 hour and then naturally cooled to room temperature, thereby obtaining the flux modifier.

[0132] The chemical composition of the obtained flux modifier is: CaF2 55.8%, CaO 5.45%, SiO2 10.88%, Al2O3 2.3%, Na3AlF6 14.7%, B2O3 2.9%, S 0.17%, and ignition loss 7.8%.

[0133] The flux modifier is added to the high-level silo of the AOD furnace and the original smelting process is followed:

[0134] (1) Calculate the amount of alloy and lime added according to the molten iron composition, temperature, scrap steel amount, and target molten steel composition, and determine the basic amount of fluorite balls to be 1800 kg;

[0135] (2) Add 2.5t lime when mixing steel, top lance oxygen flow rate 4270Nm 3 / h, main gun oxygen flow rate 5252Nm 3 / h, argon flow rate 919Nm 3 / h, after blowing for 10 minutes, add 12750kg of high carbon ferrochrome and 5100kg of steel bars, continue blowing for 12 minutes, lift the top gun and shake the furnace to remove 70-80% of the slag;

[0136] (3) Add 3 tons of lime, 2086 kg of steel sand, and 4560 Nm of top lance oxygen flow rate 3 / h, main gun oxygen flow rate 5359Nm 3 / h, argon flow rate 880Nm 3 / h, after blowing for 16 minutes, lift the top gun, add 2.5t of lime and 2082kg of high carbon ferromanganese, adjust the main gun oxygen flow rate to 5317Nm3 / h, and the argon flow rate to 808Nm 3 / h, after blowing for 26 minutes, adjust the oxygen flow rate of the main gun to 1435Nm 3 / h, nitrogen flow rate 2036Nm 3 / h, argon flow rate 890Nm 3 / h, shake the furnace to take carbon samples to measure the temperature, and the temperature at the end of oxidation is measured to be 1690℃;

[0137] (4) When entering the reduction period, add 1050kg of low-carbon ferromanganese, 7100kg of medium-silicon ferromanganese, and a flux modifier equal to the amount of fluorite balls added to the base. No more fluorite balls are added, and the oxygen flow rate of the main gun is adjusted to 1435Nm 3 / h, nitrogen flow rate 2036Nm 3 / h, the main gun was closed after blowing oxygen for 2.5 minutes, and nitrogen was blown for 7 minutes, and the furnace was shaken to take the reduction sample for temperature measurement. The temperature after reduction was measured to be 1596℃;

[0138] (5) According to the requirements of molten steel composition, 140 kg of copper plate is added, and the furnace is shaken to discharge more than 80% of the slag before tapping the steel; wherein, when fluorite balls are used in step (4), it is the original process, an unmodified smelting process, and unmodified refined slag is obtained; and when the fluorite balls are replaced with an equal amount of flux modifier in step (4), it is a modified smelting process, and modified refined slag is obtained.

[0139] According to this method, the flux modifier can completely replace the fluorite spheroidized slag and modify the refined slag without changing the smelting process, increasing material consumption, or affecting the quality of molten steel. The refined slag modified by the flux modifier of this embodiment does not pulverize when cooled naturally, and is grayish white or grayish green. Figure 7 As shown; the unmodified refined slag is severely powdered, as shown Figure 8 shown.

[0140] The chemical composition of modified and unmodified AOD furnace refined slag was analyzed in detail by X-ray fluorescence spectrometry, and the test results are shown in Table 7. The results show that the modified slag and unmodified slag have similar compositions, proving that the modification treatment has no significant effect on the refined slag.

[0141] Table 7 Main components of modified and unmodified slag

[0142]

[0143] X-ray diffraction (XRD) technology was used to identify the main mineral phases in the slag. Fig. 9 shown.

[0144] The main physical phases of unmodified slag and modified slag are the same, namely tricalcium silicate and dicalcium silicate. The results show that the physical phases of each mineral in modified slag and unmodified slag are roughly the same. Compared with unmodified slag, the physical phase of modified slag lacks the phase of low-temperature γ-Ca2SiO4 crystal form, indicating that the modification treatment preserves the original mineral phase and crystal form of steel slag and inhibits the transformation of high-temperature β-Ca2SiO4 crystal form to low-temperature γ-Ca2SiO4 crystal form. β-Ca2SiO4 has high activity, while γ-Ca2SiO4 has extremely low activity. Inhibiting the crystal transformation means retaining the high-activity phase, which improves the gelling activity of the refined slag after cooling. At the same time, there is a density difference of about 10% between β-Ca2SiO4 and γ-Ca2SiO4, which inhibits the crystal transformation, that is, reduces the volume expansion caused by the density difference and pulverization. The modification treatment inhibits the crystal transformation, that is, it solves the problem of reduced activity and pulverization of refined slag at the same time.

[0145] The set process parameters and actual production data were strictly compared as shown in the following table. According to the on-site operation records and operator feedback, there were no abnormalities. The results are shown in Table 8, indicating that the modification treatment had no effect on the smelting of the AOD furnace and the composition of the molten steel.

[0146] Table 8 Composition of modified molten steel in Example 3

[0147]

[0148] After crushing and grinding, the unmodified and modified refined slag powders have the following properties:

[0149] Table 9 Physical property test results of modified refined slag obtained after unmodified and modified smelting treatment in Example 3

[0150]

[0151] As can be seen from Table 9, when the modifier of this embodiment is not used for modified smelting, the obtained refined slag has extremely low gelling activity, and the high free calcium oxide leads to unqualified hydration stability, which cannot meet the basic requirements for use as an active material. However, after the flux modifier of this embodiment is used for modified smelting, the gelling activity of the obtained modified refined slag is increased to >70%, the free calcium oxide is greatly reduced, the stability meets the qualified requirements, and the performance is greatly improved, meeting the requirements for use as an active material in cement and concrete production.

[0152] The adjustment of the AOD furnace smelting process in different embodiments of the present invention is mainly related to the on-site smelting conditions, such as molten iron composition, temperature, alloy type, composition, reduction temperature, basicity, target molten steel composition and temperature requirements, and the smelting parameters are set as conventional adjustments within the process requirements. Since the flux modifier proposed in the embodiment of the present invention is a substitute for fluorite balls, the basic usage refers to the previous usage of fluorite balls.

[0153] It will be easily understood by those skilled in the art that the above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. A fluxing modifier for stainless steel AOD furnace refining slag, characterized in that: According to weight parts, it includes 50-80 parts of fluorine-containing raw materials, 0-10 parts of iron-containing raw materials, 0-10 parts of limestone, 5-25 parts of aluminum-containing raw materials, 1-5 parts of binders, and 1-5 parts of modification aids; The main component of the fluorine-containing raw material is calcium fluoride, the main component of the iron-containing raw material is iron element and / or iron oxide, the main component of the aluminum-containing raw material is Na3AlF6, and the binder is a bonding agent; the modification aid is used to reduce the melting point of the flux modifier, modify the AOD furnace refining slag, and inhibit the crystal transformation of calcium silicate.

2. The flux modifier according to claim 1, characterized in that The fluorine-containing raw material is one or more of fluorite ore, fluorite flotation powder, fluorine-containing sludge, and fluorine chemical by-products; Preferably, the main chemical components and their mass fractions of the fluorine-containing raw material are: CaF270.0-85.0 parts, CaCO3 0-15.0 parts, SiO2 0-15.0 parts, Al2O3 0-10 parts, K2O+Na2O0-5.0 parts, S 0-1.0 parts, and P 0-0.1 parts.

3. The flux modifier according to claim 1, characterized in that The iron-containing raw material is one or more of iron scale, iron powder, iron concentrate, and rolled steel skin; Preferably, the main chemical components of the iron-containing raw material and their mass fractions are: T.Fe50.0-80.0 parts, SiO2 0-15.0 parts, Al2O3 0-10 parts, MgO+CaO 0-10.0 parts, S 0-0.3 parts, P 0-0.1 parts.

4. The flux modifier according to claim 1, characterized in that The aluminum-containing raw material is cryolite, and its main elements and their mass fractions are: F 48-53 parts, Al 0-25 parts, K+Na 0-30 parts, C 0-1.0 parts, S 0-0.5 parts, P 0-0.1 parts.

5. The flux modifier according to claim 1, characterized in that The binder is one or more of plant gum or modified starch.

6. The flux modifier according to claim 1, characterized in that The modification aid is one or more of boron oxide, boric acid or calcium borate.

7. The method for preparing a flux modifier according to any one of claims 1 to 6, characterized in that: The ingredients are prepared according to the proportion of each group, mixed evenly and then granulated, and the granulated particles are dried and cooled to room temperature to obtain the flux modifier.

8. Use of the flux modifier according to any one of claims 1 to 6, characterized in that: It is used to carry out in-furnace refining and modification of stainless steel AOD furnace to obtain modified refined slag.

9. A method for refining and modifying a stainless steel AOD furnace using the flux modifier according to any one of claims 1 to 6 to obtain modified refined slag, characterized in that: The flux used in the stainless steel AOD furnace refining process is replaced with the flux modifier according to any one of claims 1 to 6, and the refining and modification are performed to obtain modified refined slag.