Large-thickness subsea pipeline steel plate and production method thereof

By optimizing the chemical composition and process of subsea pipeline steel, the composite steel plate is made by using five-stage heating and multi-stage rolling and cooling processes, which solves the high alloy content, small thickness and long stacking time of existing subsea pipeline steel. These problems have achieved high strength, low temperature toughness and low production costs.

CN119020565AActive Publication Date: 2024-11-26INST OF RES OF IRON & STEEL JIANGSU PROVINCE +2

Patent Information

Application Number
CN202410921456.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-05-28
Publication Date
2024-11-26
Estimated Expiration
2044-05-28

AI Technical Summary

Technical Problem

The existing subsea pipeline steel has high alloy content, small thickness, long stacking time, low strength, low toughness, high yield and strength ratio, etc., which lead to high production costs, slow production pace, long cycle and low safety, which limits subsea pipeline engineering. development.

Method used

The chemical composition of the steel plate using large thickness subsea pipeline is C: 0.031-0.061%, Si: 0.08-0.16%, Mn: 1.64-1.72%, P: 0.0090-0.0140%, S: 0.0015-0.0038%, Cr: 0.12-0.20 %, Ni: 0.12~0.20%, Mo: 0.07~0.13%, Nb: 0.054~0.064%, Ti: 0.011~0.019%, Alt: 0.021~0.049%, N: 0.0031~0.0051%, passed the five-stage heating and The crystallization area is subjected to low-temperature and large-pressure rolling, intermediate blank cooling, high-temperature and large-pressure rolling and multi-stage controlled cooling processes to make steel plates with composite phase structure.

Benefits of technology

The steel plate with low production cost, high strength, good low temperature toughness and yield strength ratio matching has been achieved. The yield strength of the steel plate is ≥500MPa, tensile strength ≥630MPa, elongation ≥35%, impact work KV2 ≥300J, -60℃ The impact work KV2≥250J, and the DWTT tough brittle transition temperature is lower than -20℃, which solves the problems of high alloy content, small thickness, and long stacking time.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119020565A_ABST
    Figure CN119020565A_ABST
Patent Text Reader

Abstract

The invention relates to a large-thickness subsea pipeline steel plate and a production method thereof, components of the steel plate are optimally designed through low-carbon and low-alloy components, and the production method adopts a matched special controlled rolling process of five-section heating, recrystallization zone low-temperature and high-pressure rolling, intermediate billet instant cooling and non-recrystallization zone high-temperature and high-pressure rolling. And a multi-stage control cooling process including high-temperature area air cooling redistribution, ferrite area cooling, temperature holding, bainite area cooling and air cooling self-tempering cooling is adopted. The proportion of acicular ferrite of the product steel plate is high, and the average grain size of the ferrite is small and is 3-6 microns, so that the steel plate has good obdurability matching, the steel plate strength is high, the yield strength is larger than or equal to 500 MPa, the tensile strength is larger than or equal to 630 MPa, and the impact energy KV2 at the temperature of 60 DEG C below zero is larger than or equal to 250 J.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a thick submarine pipeline steel plate and a production method thereof, belonging to the technical field of steel casting. Background Art

[0002] At present, onshore oil and gas fields around the world have gradually entered the middle and late stages of exploitation, with exploration and development becoming more difficult and more costly. However, the potential of offshore oil and gas resources is huge, and the prospect of exploration is good. The demand for submarine oil and gas pipelines is increasing. Submarine oil and gas pipelines are the fastest, most economical and most effective way to transport offshore oil and natural gas. They are an indispensable lifeline project for the development and production of offshore oil and gas fields, and will generate huge demand for submarine pipeline steel.

[0003] As submarine pipelines are in service in complex marine environments for a long time, they are subject to environmental loads such as wave currents outside the pipeline, seabed scouring and silting, and slippage, as well as fluid pressure and corrosion inside the pipeline. Once a submarine pipeline ruptures, it will cause catastrophic accidents such as economic losses, environmental pollution, and ecological damage. Therefore, higher requirements are put forward for submarine pipeline steel, such as large thickness, high strength, low yield ratio, excellent low-temperature toughness, and corrosion resistance.

[0004] Patent publication number CN117165870A is a hot-rolled steel plate for thick-walled submarine pipelines and a manufacturing method, providing a chemical composition of the hot-rolled steel plate by weight percentage: C: 0.03% to 0.05%, Si: 0.16% to 0.24%, Mn: 1.60% to 1.70%, P≤0.015%, S≤0.004%, Cr: 0.14% to 0.18%, Ni: 0.11% to 0.15%, Mo: 0.09% to 0.13%, Nb: 0.05% to 0.065%, Ti: 0.01% to 0.02%, Al: 0.02% to 0.05%, P cm ≤0.19%, the rest are Fe and impurity elements. Through KR desulfurization-BOF converter-LF refining-RH degassing-CCM continuous casting-slab reheating-rough rolling-intermediate billet waiting for temperature cooling-finishing rolling-accelerated cooling-hot straightening-natural cooling-warm straightening and cold straightening-off-line stack cooling and ultrasonic flaw detection-finishing process, it can meet the specification requirements of submarine pipeline X70 level and thickness specifications above 30mm.

[0005] Patent publication number CN104357766A is a kind of ultra-thick specification high-strength and high-toughness submarine pipeline steel for ultra-deep sea, providing the chemical composition of the steel by weight percentage: C: 0.020%~0.050%, Si≤0.10%, Mn: 1.00%~1.50%, P≤0.010%, S≤0.0010%, Cu: 0.10%~0.30%, Cr: 0.10%~0.25%, Ni: 0.31%~0.50%, Mo≤0.15%, Nb: 0.030%~0.065%, V: 0.015%~0.040%, Ti: 0.010%~0.025%, Al: 0.010%~0.050%, N≤0.008%, and the rest is Fe. The manufacturing method is as follows: 1) casting; 2) rough rolling; 3) finishing rolling; 4) cooling; 5) relaxation. Thickness of extra thick pipeline steel is ≥35mm. The finishing rolling start temperature is controlled at 820~900℃, and the cumulative reduction rate of finishing rolling is 60~75%; the final rolling temperature is 760~840℃; after rolling, the steel plate is cooled in two stages, with a cooling rate of 5~10℃ / s in stage I and a final cooling temperature of 720~750℃; the cooling rate of 20~40℃ / s in stage II and a final cooling temperature of 100~300℃; the yield strength (R t0.5) ≥485MPa, tensile strength (R m) ≥570MPa, yield strength ratio (R t0.5 / R m) ≤0.85, elongation (A 50mm) ≥40%, -20℃ KV8≥400J, -20℃ DWTT shear area fraction≥85%.

[0006] Patent publication number CN103451536B is a low-cost thick-gauge steel plate for submarine pipelines and its manufacturing method, providing the chemical composition weight percentage of the steel plate: C: 0.04% ~ 0.06%, Si: 0.15% ~ 0.20%, Mn: 1.43% ~ 1.47%, P ≤ 0.008%, S ≤ 0.003%, Ni: 0.10% ~ 0.15%, Nb: 0.030% ~ 0.040%, Ti: 0.012% ~ 0.023%, Al: 0.015% ~ 0.025%, N ≤ 0.006%, Nb + V + Ti ≤ 0.15%, the rest is iron and unavoidable impurities. The continuous casting slab is horizontally formed, the continuous casting slab is heated at low temperature, the low temperature is controlled to roll, and the relaxation and slow cooling control technology is adopted. The produced steel plate has a dual-phase microstructure, achieves high strength and low yield strength ratio, and has good toughness. When rolling in the recrystallization zone, the final rolling temperature is controlled at 990~1020℃, the total reduction is 65%~75%, and the final 3-pass reduction is 20%~30%; in the non-recrystallization zone, the total reduction is 60%~70%, and the final rolling temperature is 750~810℃; after rolling, the steel plate is relaxed and slowly cooled, and then the steel plate is quenched online using MULPIC, the cooling rate is controlled at 20~30℃ / s, and the final cooling temperature is controlled at 350~450℃. The thickness of the steel plate is 28.6~31.8mm.

[0007] Patent publication number CN102676925A discloses a thick-walled submarine pipeline steel plate and a production method of the steel plate, which discloses that the steel plate is composed of the following components in weight percentage: C: 0.05% to 0.07%, Si: 0.15% to 0.25%, Mn: 1.42% to 1.48%, P≤0.010%, S≤0.002%, Ni: 0.13% to 0.18%, Nb: 0.043% to 0.048%, Al: 0.020% to 0.040%, Ti: 0.014% to 0.024%, Mo: 0.13% to 0.18%, and the remainder is Fe and unavoidable impurities. The thickness of the thick-walled submarine pipeline steel plate is 25-30.2 mm. It is rolled using a two-stage rolling process of recrystallization zone + non-recrystallization zone. The rolling temperature in the first stage is 950-1100 ° C. The single-pass reduction in this stage is 10%-20%, and the cumulative reduction rate is 30%-50%; the rolling temperature in the second stage is 840-880 ° C, and the cumulative reduction rate is 30%-50%; the water entry temperature after rolling is 740-780 ° C, and the red-return temperature is 450-500 ° C to obtain the steel plate. Mechanical properties: yield strength is between 470-570 MPa, tensile strength is between 535-760 MPa, elongation>30%, -20 ° C impact energy>200 J, DWTT shear area fraction>75%, yield strength ratio<0.90.

[0008] Currently, there are many patents for submarine pipeline steel.

[0009] In terms of composition, some submarine pipeline steels adopt alloy component systems such as V and Cu, such as patents CN111979497A, CN109234487B, CN111607747A, CN110863145A, CN108504931B, CN105132833B, CN105132807B, CN104357766A, CN103993240A, CN101701315B, CN111748741B, etc., all of which are added with 0.015%~0.060% V and / or 0.10%~0.30% Cu, and their alloy content is relatively high, which leads to increased production costs.

[0010] In terms of technology, some submarine pipeline steels are produced by coil production lines to obtain pipeline steel coils or steel strips. Rough rolling is 1 to 2 stands, finishing rolling is 5 to 7 stands, and coiling is required after rolling, such as patents CN111979497A, CN113278880A, CN110578091B, CN111607747A, CN108504931B, etc. The submarine pipeline steel coils or steel strips produced by them have a small thickness, generally 3 to 20 mm, which is difficult to meet the needs of harsh submarine environment and pipeline high-pressure transportation. Some submarine pipeline steels are rolled by medium and thick plate or wide and thick plate mills. The steel plates are relatively thick, such as patents CN103993240A and CN106566991B, with a thickness of 20 to 48 mm. After being rolled into steel plates, they need to be stacked and slowly cooled for 12 to 48 hours. The long stacking time affects production efficiency.

[0011] In terms of performance, some patents for pipeline steel have low strength, such as patents CN109234487B, CN107988562A, etc., which are X65-grade submarine pipeline steels with low strength and yield strength ≥450MPa. Some patents have low toughness, such as patents CN105132807B, CN103834874B, etc., with -20℃ impact energy ≥250J, and no requirements for -40℃ impact energy. Some patents have high yield strength ratios, such as patents CN104357766A, CN103993240A, CN109234487B, CN111607747A, etc., with yield strength ratios ≤0.90, and most of them are between 0.85 and 0.90.

[0012] Existing submarine pipeline steel patents have problems such as high alloy content, small thickness, long stacking time, low strength, low toughness, and high yield strength ratio. These problems lead to high production costs, slow production pace, long cycle, and low safety of existing submarine pipeline steel, which restricts the development of the submarine pipeline engineering industry. Summary of the invention

[0013] In order to solve the above problems, the present invention discloses a thick submarine pipeline steel plate and a production method thereof, and the specific technical scheme thereof is as follows: A thick submarine pipeline steel plate, the chemical composition of which is calculated by mass percentage: C: 0.031-0.061%, Si: 0.08-0.16%, Mn: 1.64-1.72%, P: 0.0090-0.0140%, S: 0.0015-0.0038%, Cr: 0.12-0.20%, Ni: 0.12-0.20%, Mo: 0.07-0.13%, Nb: 0.054-0.064%, Ti: 0.01 1~0.019%, Alt: 0.021~0.049%, N: 0.0031~0.0051%, the rest are iron and unavoidable impurities, the chemical composition of the steel plate also meets the carbon equivalent CEV=C+Mn / 6+(Cr+Mo+V) / 5+(Cu+Ni) / 15 is 0.350~0.427, Pcm=C+Si / 30+(Mn+Cu+Cr) / 20+Ni / 60+Mo / 15+V / 10+5B is 0.127~0.174. The elements in the calculation formulas of CEV and Pcm are the values ​​of their mass percentage in the steel plate, without the percentage sign of mass percentage.

[0014] Furthermore, the continuous casting billet is successively subjected to a special controlled rolling process of five-stage heating, low-temperature large-reduction rolling in the recrystallization zone, intermediate billet cooling, high-temperature large-reduction rolling in the non-recrystallization zone, and a multi-stage controlled cooling process of air cooling and redistribution in the high-temperature zone after rolling, cooling in the ferrite zone, waiting for temperature, cooling in the bainite zone, and air cooling and self-tempering cooling to produce submarine pipeline steel plates.

[0015] Furthermore, the five-stage heating process is specifically as follows: placing the continuous casting billet in a walking beam heating furnace for heating, the length of the heating furnace is 55m, and a five-stage heating process of a heat recovery section, a preheating section, a first heating section, a second heating section and a soaking section is adopted, wherein the temperature of the heat recovery section is ≤850°C, the heating time of the heat recovery section is 0.37-0.41min / mm, the temperature of the preheating section is ≤950°C, the heating time of the preheating section is 0.32-0.35min / mm, the temperature of the first heating section is 1050±15°C, the heating time of the first heating section is 0.22-0.25min / mm, the temperature of the second heating section is 1150±15°C, the heating time of the second heating section is 0.17-0.20min / mm, the temperature of the soaking section is T1, T1≥T NbN , and T NbN ≤T1≤T NbN + 25℃, the heating time in the soaking section is 0.07~0.14min / mm, and the total heating time is 1.15~1.35min / mm, where lg(Nb×N)=3.7-10800 / (TNbN +273.15).

[0016] Further, the process of low-temperature large-reduction rolling in the recrystallization zone is specifically as follows: the starting rolling temperature is T2 -10°C ~ T2 + 30°C, and the final rolling temperature is T2 - 80°C ~ T2 - 40°C; in the low-temperature section within the temperature range of the recrystallization zone, a large-reduction rolling process is adopted, the pass reduction is ≥31mm, the total number of rough rolling passes is 4 to 6 passes, the temperature difference between adjacent passes is 12°C ~ 18°C, and the reduction of the previous pass is less than or equal to the reduction of the next pass, that is, R n ≤R n+1 , R n and R n+1 are the reductions of the nth pass and the n+1th pass respectively; the thickness of the intermediate billet after rolling is t z , satisfying 3.4t≤t z ≤4.4t, t is the thickness of the finished steel plate, where T2 is the recrystallization temperature, T2=887+464C+6445Nb-644 +890Ti+363Al-357Si.

[0017] Further, the intermediate billet is cooled: after the rolling in the austenite recrystallization zone is completed, the intermediate billet cooling device is immediately used for water cooling, the cooling manifold water pressure is 0.4~0.6MPa, the upper manifold water flow is 50~150m³ / h, the lower manifold water flow is 100~300m³ / h, the water flow ratio of the lower manifold to the upper manifold is ≥2, the cooling water temperature is 10~30℃, the intermediate billet is cooled back and forth in the cooling device, the roller speed of the cooling device is 0.4~6m / s, and it is cooled to the non-recrystallization rolling temperature range, that is, cooled to T2-240℃ ~ T2-220℃.

[0018] Further, the non-recrystallization zone high temperature and large reduction rolling: the starting rolling temperature is T2-240℃ ~ T2-220℃, and the final rolling temperature is T3 ~ T3 + 25℃; a large reduction rolling process is adopted in the high temperature section within the temperature range of the non-recrystallization zone, the high temperature section, that is, the temperature is T2-280℃ ~ T2-240℃, the number of rolling passes in the high temperature zone is 4 to 6 passes, the rolling speed is 3 to 5m / s, the pass reduction is ≥21mm, and the previous pass reduction is greater than or equal to the next pass reduction, that is, R m ≥R m+1 , R m and R m+1The reduction amounts are the mth pass and the m+1th pass respectively, and the thickness of the billet after rolling is t+3mm ~ t+12mm; a small reduction rolling process is adopted in the low temperature section within the temperature range of the non-recrystallization zone, and the temperature of the low temperature section is T3 +5℃ ~ T3 + 30℃, the number of rolling passes in the low temperature section is 1 to 2 passes, the rolling speed is 4 to 6m / s, the pass reduction amount is ≤6mm, and the thickness of the finished steel plate after rolling is t, t≥35mm; during the rolling process in the non-recrystallization zone, an intermediate billet cooling device is used for water cooling between passes, wherein T3 is the temperature at which the transformation of austenite to ferrite begins during cooling, T3=910-310C-80Mn-15Cr-80Mo.

[0019] Furthermore, the air cooling in the high temperature zone after rolling is redistributed: after rolling, the steel plate is air cooled on the conveyor roller, the conveyor roller length is 60m, the roller speed is 2-5m / s, the indoor temperature is 5-39°C, the steel plate is air cooled to T3-50°C ~ T3-30°C, and then enters the ultra-fast cooling system.

[0020] Furthermore, the ferrite zone is cooled: the steel plate enters the ultra-fast cooling system from the ultra-fast cooling inlet, the ultra-fast cooling system has a total of 24 groups of cooling headers, and the cooling length of each group of headers is 1m; 1 to 24 groups of headers are opened for cooling, the cooling rate is 10 to 20°C / s, the water pressure is 0.15 to 0.20MPa, the cooling water temperature is 10 to 30°C, the water flow rate of the upper and lower headers is 60 to 200m³ / h, the water flow rate ratio of the lower header to the upper header is 1.1 to 1.5, the cooling roller speed of the ultra-fast cooling system is 1.8 to 2.2m / s, and the temperature is cooled to T4+ 5°C to T4 + 25°C, where T4=830-270C-90Mn-37Ni-70Cr-83Mo.

[0021] Furthermore, the waiting for temperature is specifically as follows: after cooling to the intermediate temperature T4 + 5°C ~ T4 + 25°C, the upper and lower cooling water headers are closed, the steel plate exits the ultra-fast cooling system from the entrance of the ultra-fast cooling system, and is swung on the ultra-fast cooling entrance roller to wait for temperature, that is, it is swung back and forth on the roller at a speed of 0.5 to 1.5 m / s, the forward and backward moving distance is 5 to 10 m, and the waiting time is 8 to 15 seconds.

[0022] Furthermore, the cooling of the bainite zone is specifically as follows: the steel plate enters the ultra-fast cooling system again from the ultra-fast cooling inlet, with a total of 24 groups of cooling headers, and the cooling length of each group of headers is 1m; 1 to 24 groups of headers are opened for cooling, the water pressure is 0.30 to 0.50 MPa, the cooling rate is 8 to 20°C / s, the cooling water temperature is 10 to 26°C, the water flow rate of the upper and lower headers is 100 to 400 m³ / h, the water flow rate ratio of the lower header to the upper header is 1.2 to 1.4, the cooling roller speed of the ultra-fast cooling system is 0.6 to 1.4 m / s, and the temperature is cooled to T4 - 285°C to T4 - 265°C.

[0023] Furthermore, the air-cooling self-tempering cooling is specifically as follows: after cooling to T4 - 285°C ~ T4 - 265°C, the steel plate leaves the ultra-fast cooling system from the outlet of the ultra-fast cooling system; then straightening, and air-cooling self-tempering is performed on the cooling bed until it is cooled to room temperature; the air-cooling self-tempering conditions are that the cooling bed is airtight and windless, the cooling bed needs to be covered with hot steel plates, the spacing between the steel plates is 1 to 2m, and the steel plate temperature is T4 - 305°C ~ T4 - 105°C.

[0024] Furthermore, by using continuous casting billets with a thickness of ≤320 mm, the center segregation is not higher than level 0.5, and the inclusions of types A, B, C, and D are all not higher than level 1, a steel plate with a thickness of ≥35 mm is produced, and the compression ratio is ≤9.14.

[0025] The present invention also claims to protect the thick submarine pipeline steel plate produced by the above-mentioned thick submarine pipeline steel plate production method.

[0026] Furthermore, the structure of the thick submarine pipeline steel plate is a complex phase structure of quasi-polygonal ferrite + acicular ferrite + bainite + tempered bainite, the proportion of MA self-tempering decomposition in bainite is ≤20%, the average grain size of ferrite is 3~6μm, the proportion of quasi-polygonal ferrite is 5%~15%, the proportion of acicular ferrite is 25%~40%, the proportion of bainite is 25%~65%, the proportion of tempered bainite is 5%~20%, the yield strength of the steel plate is ≥500MPa, the tensile strength is ≥630MPa, the elongation is ≥35%, the yield strength ratio is ≤0.80, the impact energy KV2 at -40℃ is ≥300J, the impact energy KV2 at -60℃ is ≥250J, the hardness is ≤208HV10, the -10℃ DWTT drop hammer shear area fraction is 100%, the -20℃ DWTT drop hammer shear area fraction is ≥90%, and the DWTT ductile-brittle transition temperature is lower than -20℃.

[0027] The beneficial effects of the present invention are: (1) The chemical composition of the present invention does not contain expensive alloys such as V and Cu, and the content of alloy additions such as Ni and Mo is relatively low. Harmful elements such as P and S do not need to be controlled at ultra-low content, which makes steelmaking production easy and has a low production cost.

[0028] (2) The controlled rolling and controlled cooling process is adopted, which has the advantages of short process flow, low production cost and fast delivery, avoiding the problems of long production process, slow production rhythm and long delivery cycle caused by stacking. At the same time, the process of low-temperature large reduction rolling in the recrystallization zone + intermediate billet cooling + high-temperature large reduction rolling in the non-recrystallization zone is adopted to accurately control each rolling stage. The continuous casting billet with a thickness of ≤320mm is used to produce a steel plate with a thickness of ≥35mm, with a compression ratio of ≤9.14, fine structure, excellent toughness, an average ferrite grain size of 3~6μm, an impact energy KV2 of -60℃ ≥250J, and a DWTT ductile-brittle transition temperature below -20℃.

[0029] (3) The present invention adopts a multi-stage controlled cooling process, and adjusts and controls the finished product structure type and proportion according to the cooling parameters of each stage to obtain a complex phase structure. Quasi-polygonal ferrite is formed in the first stage of air cooling before ultra-fast cooling after rolling, acicular ferrite is formed in the second stage of cooling and the third stage of waiting for temperature, bainite is formed in the fourth stage of cooling, and tempered bainite is formed in the fifth stage of cooling. This complex phase structure can ensure the good matching of various mechanical properties such as steel plate strength, low temperature toughness, yield strength ratio, hardness, and drop hammer performance.

[0030] (4) The present invention has a complex structure of quasi-polygonal ferrite + acicular ferrite + bainite + tempered bainite through reasonable matching of chemical composition, five-stage heating, special controlled rolling process, and multi-stage controlled cooling process. The proportion of MA self-tempering decomposition in bainite is ≤20%, the proportion of quasi-polygonal ferrite is 5%-15%, the proportion of acicular ferrite is 25%-40%, the proportion of bainite is 25%-65%, and the proportion of tempered bainite is 5%-20%. The yield strength of the steel plate is ≥500MPa, the tensile strength is ≥630MPa, the elongation is ≥35%, the yield strength ratio is ≤0.80, the impact energy KV2 at -40℃ is ≥300J, the hardness is ≤208HV10, the -10℃ DWTT drop hammer shear area fraction is 100%, and the -20℃ DWTT drop hammer shear area fraction is ≥90%.

[0031] (5) The steel plate of the product of the present invention has a high proportion of needle-shaped ferrite and a fine average ferrite grain size of 3 to 6 μm, so that the steel plate has a good match between strength and toughness. The steel plate has a high strength, a yield strength of ≥500 MPa, a tensile strength of ≥630 MPa, and an impact energy KV2 of ≥250 J at -60°C. BRIEF DESCRIPTION OF THE DRAWINGS

[0032] Figure 1 2 is a metallographic structure diagram of an embodiment of the present invention. DETAILED DESCRIPTION

[0033] The present invention will be further described below in conjunction with specific embodiments. It should be understood that the following specific embodiments are only used to illustrate the present invention and are not used to limit the scope of the present invention.

[0034] Thick submarine pipeline steel plate and production method thereof, the chemical composition of the steel plate includes, by mass percentage: C: 0.031-0.061%, Si: 0.08-0.16%, Mn: 1.64-1.72%, P: 0.0090-0.0140%, S: 0.0015-0.0038%, Cr: 0.12-0.20%, Ni: 0.12-0.20%, Mo: 0.07-0.13%, Nb: 0.054-0.064%, Ti: 0 .011~0.019%, Alt: 0.021~0.049%, N: 0.0031~0.0051%, the rest are iron and inevitable impurities. The chemical composition of the steel plate also meets the carbon equivalent CEV=C+Mn / 6+(Cr+Mo+V) / 5+(Cu+Ni) / 15, which is 0.350~0.427, and Pcm=C+Si / 30+(Mn+Cu+Cr) / 20+Ni / 60+Mo / 15+V / 10+5B, which is 0.127~0.174.

[0035] The main functions of the chemical components in the present invention and the selection of their dosage are specifically analyzed and explained below: Carbon (C): Carbon is the most economical strengthening element in steel, which has a solid solution strengthening effect. At the same time, it forms carbides with Nb, Ti, Cr, Mo, etc., which has a precipitation strengthening effect. The increase in carbon content has a significant effect on improving the strength and hardness of pipeline steel, but too high carbon content will lead to poor low-temperature toughness and welding performance, and reduce the low-temperature drop hammer performance of pipeline steel. Therefore, the carbon content is selected to be 0.031% to 0.061%.

[0036] Silicon (Si): Silicon has a solid solution strengthening effect in steel, but too much silicon tends to produce Fe2SiO4 on the surface of the slab, which is not conducive to the control of the surface quality of the steel plate. Therefore, the silicon content is selected to be 0.08% to 0.16%.

[0037] Manganese (Mn): Manganese plays a role of solid solution strengthening in steel, improving the strength and hardness of steel. Reasonable manganese content can ensure the strength of pipeline steel at a low cost. It is the most economical strengthening element besides carbon. However, too much manganese will cause central segregation of the ingot, which will have a great damage to the toughness of the thick plate. At the same time, it is not conducive to the control of banded structure. Therefore, the manganese content is selected to be 1.64%~1.72%.

[0038] Phosphorus (P): Phosphorus is an impurity element in steel. Too high phosphorus content will easily cause segregation, which will significantly reduce the plasticity and toughness of the steel, especially under low temperature conditions. However, too low phosphorus content will greatly increase the cost of steelmaking. Therefore, the phosphorus content is selected to be 0.0090%~0.0140%.

[0039] Sulfur (S): Sulfur is an impurity element in steel. It not only increases the hot brittleness of steel, but also easily forms MnS inclusions with manganese, reducing the low-temperature toughness of steel. However, too low sulfur content will greatly increase the cost of steelmaking. Therefore, the sulfur content is selected to be 0.0015%~0.0038%.

[0040] Chromium (Cr): Chromium plays a role in solid solution strengthening in steel. At the same time, as a ferrite-forming element, chromium can obtain more acicular ferrite structure in high-niobium steel. However, when the chromium content is too high, the microhardness of pipeline steel will be increased and the low-temperature toughness will be reduced. Therefore, the chromium content is selected to be 0.12%~0.20%.

[0041] Nickel (Ni): Nickel plays a role in solid solution strengthening in steel, improving the strength of steel without significantly increasing the hardness of steel. At the same time, nickel is beneficial to low-temperature toughness, but when the nickel content is too high, the alloy cost increases. Therefore, the nickel content is selected to be 0.12%~0.20%.

[0042] Molybdenum (Mo): Mo can significantly improve the hardenability of steel, delay ferrite transformation, obtain acicular ferrite structure, and is beneficial to improving the strength and toughness of pipeline steel. However, Mo increases the number of MA components, which is not conducive to improving toughness. Moreover, when the Mo content is too high, the alloy cost increases significantly. Therefore, the Mo content is selected to be 0.07% to 0.13%.

[0043] Niobium (Nb): Niobium is an important grain-refining element in steel. During hot rolling, niobium strongly inhibits austenite recrystallization and its precipitation in austenite, pins austenite grain boundaries, and refines recrystallized grains. During cooling, the dissolved niobium can continue to precipitate in the form of niobium carbonitride, which significantly refines the structure of the material after phase transformation, further improving the strength and toughness of the steel. Adding too much niobium will, firstly, increase the alloy cost; secondly, niobium cannot be completely dissolved during normal heating; thirdly, the precipitation strengthening of niobium is not good for the yield strength ratio. Therefore, the niobium content is selected to be 0.054% to 0.064%.

[0044] Titanium (Ti): Titanium is a nitrogen-fixing element in steel. It can form dispersed titanium nitride particles, which inhibit the coarsening of austenite grains during the billet heating and rolling process. If the addition amount is too high, it is easy to form coarse carbon / nitride precipitation in the core of the billet, affecting the low-temperature toughness of the steel plate. Therefore, the titanium content is selected to be 0.011% to 0.019%.

[0045] Aluminum (Al): Aluminum is a deoxidizing element in steel. Too much aluminum can easily increase the Al2O3 inclusions in the steel, affecting the low-temperature toughness of the steel. On the basis of ensuring the deoxidation effect, the aluminum content should be reduced as much as possible. Therefore, the aluminum content is selected to be 0.021% to 0.049%.

[0046] Nitrogen (N): Nitrogen is an impurity element in steel, which reduces the plasticity and toughness of the steel plate. Too low nitrogen will increase the cost of steelmaking. Therefore, the nitrogen content is selected to be 0.0031% to 0.0051%.

[0047] Smelting is carried out according to the above chemical composition, and continuous casting billets with a thickness of ≤320mm are obtained by light pressure reduction at the end of continuous casting. The central segregation is not higher than level 0.5, and the inclusions of types A, B, C, and D are not higher than level 1.

[0048] The continuous casting billet is made into submarine pipeline steel plate through a special controlled rolling process of five-stage heating + low-temperature large-reduction rolling in the recrystallization zone + intermediate billet cooling + high-temperature large-reduction rolling in the non-recrystallization zone, and a multi-stage controlled cooling process of air cooling and redistribution in the high-temperature zone after rolling + cooling in the ferrite zone + waiting for temperature + cooling in the bainite zone + air cooling and self-tempering cooling. The specific process steps are as follows: (1) Five-stage heating process: A five-stage heating process consisting of a heat recovery section, a preheating section, a first heating section, a second heating section, and a soaking section is used, wherein the temperature of the heat recovery section is ≤850°C, the temperature of the preheating section is ≤950°C, the temperature of the first heating section is 1050±15°C, the temperature of the second heating section is 1150±15°C, and the temperature of the soaking section is T1, T1≥T NbN , and T NbN ≤T1≤T NbN + 25℃, the heating time in the soaking zone is 0.07~0.14min / mm, and the total heating time is 1.15~1.35min / mm. Among them, lg(Nb×N)=3.7-10800 / (T NbN + 273.15).

[0049] (2) Low-temperature and high-reduction rolling in the recrystallization zone: the starting rolling temperature is T2 - 10℃ ~ T2 + 30℃, and the final rolling temperature is T2 - 80℃ ~ T2 -40℃; in the low-temperature section within the temperature range of the recrystallization zone, a high-reduction rolling process is adopted, with a reduction of ≥31mm per pass, and the reduction of the previous pass is less than or equal to the reduction of the next pass, that is, R n ≤R n+1 , R n and R n+1 are the reductions of the nth pass and the n+1th pass respectively; the thickness of the intermediate billet after rolling is t z , satisfying 3.4t≤t z≤4.4t, t is the thickness of the finished steel plate. Among them, T2 is the recrystallization temperature, T2=887+464C+6445Nb-644 +890Ti+363Al-357Si.

[0050] (3) Intermediate billet cooling: After the rolling in the austenite recrystallization zone is completed, the intermediate billet cooling device is immediately used for water cooling to the non-recrystallization rolling temperature range, that is, cooled to T2-240℃ ~ T2-220℃.

[0051] (4) High temperature and large reduction rolling in the non-recrystallization zone: the starting rolling temperature is T2-240℃ ~ T2-220℃, and the final rolling temperature is T3 ~ T3 + 25℃; in the high temperature section within the temperature range of the non-recrystallization zone, a large reduction rolling process is adopted, with a reduction of ≥21mm per pass, and the reduction of the previous pass is greater than or equal to the reduction of the next pass, that is, R m ≥R m+1 , R m and R m+1 The reductions are the mth pass and the m+1th pass respectively; in the low temperature section within the non-recrystallization temperature range, a small reduction rolling process is adopted, and the pass reduction is ≤6mm; during the rolling process in the non-recrystallization zone, the intermediate billet cooling device is used for water cooling between passes. Among them, T3 is the temperature at which the austenite starts to transform into ferrite during cooling, T3=910-310C-80Mn-15Cr-80Mo.

[0052] (5) Air cooling and redistribution in the high temperature zone after rolling: After rolling, the steel plate is air cooled on the conveyor roller to T3 - 50℃ ~T3 - 30℃, and then enters the ultra-fast cooling system.

[0053] (6) Ferrite zone cooling: The steel plate enters the ultra-fast cooling system, with a total of 24 sets of cooling headers, each with a cooling length of 1m; open 1 to 24 sets of headers for cooling, cooling to T4 + 5℃ ~ T4 + 25℃, cooling rate of 10~20℃ / s, water pressure of 0.15~0.20MPa, ultra-fast cooling system cooling roller speed of 1.8~2.2m / s. Among them, T4=830-270C-90Mn-37Ni-70Cr-83Mo.

[0054] (7) Waiting for temperature: After cooling to the intermediate temperature of T4 + 5℃ ~ T4 + 25℃, the steel plate exits the ultra-fast cooling system from the ultra-fast cooling entrance and swings on the ultra-fast cooling entrance roller to wait for temperature. The waiting time is 8 to 15 seconds.

[0055] (8) Cooling of bainite zone: Open 1~24 sets of headers for cooling, cool to T4-285℃~T4-265℃, water pressure is 0.30~0.50MPa, cooling rate is 8~20℃ / s; the cooling roller speed of the ultra-fast cooling system is 0.6~1.4m / s.

[0056] (9) Air-cooling self-tempering cooling: After cooling to T4-285℃ ~ T4-265℃, the steel plate leaves the ultra-fast cooling system from the ultra-fast cooling outlet, is then straightened, and is air-cooled and self-tempered on the cooling bed until it cools to room temperature; the air-cooling self-tempering conditions are that the cooling bed is airtight and windless, the cooling bed must be covered with hot steel plates, the spacing between the steel plates is 1 to 2m, and the steel plate temperature is T4-305℃ ~ T4-105℃.

[0057] The heating, rolling and cooling processes of the present invention are described in detail below: In the heating process, a five-stage heating process is adopted, including a heat recovery section, a preheating section, a first heating section, a second heating section and a soaking section. The temperature of the heat recovery section is ≤850°C, the temperature of the preheating section is ≤950°C, the temperature of the first heating section is 1050±15°C, the temperature of the second heating section is 1150±15°C, and the temperature of the soaking section is T1, T1≥T NbN , and T NbN ≤T1≤T NbN + 25℃, the heating time in the soaking section is 0.07~0.13min / mm, and the total heating time is 1.15~1.35min / mm. The purpose is to make the billet evenly heated in the heating furnace. Secondly, when the billet is heated, the heating temperature and heating time are reasonably selected to ensure that the Nb precipitates in the steel are completely dissolved and the austenite grains do not grow excessively, so as to prepare for the precipitation in the subsequent recrystallization zone rolling process.

[0058] In the rolling process, a special controlled rolling process is adopted, which includes low-temperature and large reduction rolling in the recrystallization zone + cooling of the intermediate billet + high-temperature and large reduction rolling in the non-recrystallization zone. The first stage is low-temperature and large reduction rolling in the recrystallization zone, with the start rolling temperature of T2-10℃ ~ T2 +30℃ and the final rolling temperature of T2-80℃ ~ T2-40℃. The purpose is to ensure that the billet can be rolled in the recrystallization zone to avoid mixed crystals, and at the same time, cooperate with the precipitation of Nb compounds during the rolling process to prevent the growth of recrystallized grains and refine the recrystallized grains. In the low-temperature section within the temperature range of the recrystallization zone, a large reduction rolling process is adopted, with a reduction of ≥31mm per pass, and the reduction of the previous pass is less than or equal to the reduction of the next pass, that is, R n ≤R n+1 , R n and R n+1 are the reductions of the nth pass and the n+1th pass respectively; the thickness of the intermediate billet after rolling is t z, satisfying 3.4t≤t z ≤4.4t, t is the thickness of the finished steel plate. The purpose is to use large reduction rolling in the low temperature section of the recrystallization zone to fully break up the continuous casting structure and obtain refined recrystallized grains. The greater the total reduction and the single pass reduction, the more obvious the refinement effect on the austenite grains, and because the temperature is low, the grains will not grow excessively. In actual production, due to the limitations of billets, rolling mills, etc., the reduction cannot be infinite. According to the results of the present invention, the pass reduction is ≥31mm, and R n ≤R n+1 , which can achieve the purpose of effective grain refinement.

[0059] During the cooling of the intermediate billet, after the rolling of the austenite recrystallization zone is completed, the intermediate billet cooling device is immediately used for water cooling to cool to the non-recrystallization rolling temperature range, that is, to T2-240℃ ~ T2-220℃. The purpose is to obtain fine recrystallized grains after rolling in the recrystallization zone. During the growth process of the grains, they are quickly cooled to below the recrystallization temperature. On the one hand, the grain growth is avoided, and on the other hand, the waiting time is reduced to improve the rolling efficiency.

[0060] In the high temperature and large reduction rolling in the non-recrystallization zone, the starting rolling temperature is T2-240℃ ~ T2-220℃, and the final rolling temperature is T3~ T3 + 25℃; in the high temperature section within the temperature range of the non-recrystallization zone, a large reduction rolling process is adopted, the reduction in one pass is ≥21mm, and the reduction in the previous pass is greater than or equal to the reduction in the next pass, that is, R m ≥R m+1 . The purpose is that in the high temperature stage of the non-recrystallization zone, the temperature is high, and large reduction rolling can be achieved, which can deform and flatten the recrystallized equiaxed grains, form more deformation bands and accumulate more energy, preparing for the subsequent cooling phase transformation. In the low temperature section within the temperature range of the non-recrystallization zone, a small reduction rolling process is adopted, and the pass reduction is ≤6mm. The purpose is that the rolling temperature is low, and the low temperature rolling process will be unfavorable to the plate shape of the steel plate. Therefore, a small deformation rolling is adopted in the low temperature section to ensure the plate shape of the steel plate after rolling. During the rolling process in the non-recrystallization zone, the intermediate billet cooling device is used for water cooling between passes. The purpose is that, on the one hand, the temperature range of the non-recrystallization zone is large, and in order to match the high temperature zone rolling and the low temperature zone rolling of the non-recrystallization zone at the same time, cooling is required. On the other hand, through the rapid cooling and rolling of the non-recrystallization, the recovery time of the deformed austenite after rolling is reduced, and more energy is accumulated for the subsequent cooling phase transformation.

[0061] In the cooling process, a multi-stage controlled cooling process is adopted, which includes air cooling and redistribution in the high temperature zone after rolling + cooling in the ferrite zone + waiting for temperature + cooling in the bainite zone + air cooling and self-tempering cooling.

[0062] In the air cooling redistribution in the high temperature zone after rolling, after rolling, the steel plate is air cooled on the conveyor roller to T3 - 50℃ ~ T3 - 30℃, and then enters the ultra-fast cooling system. The purpose is to redistribute carbon during the air cooling process of the steel plate after rolling. When the temperature is T3 - 50℃ ~ T3 - 30℃, it is in the two-phase region, and carbon-rich austenite and polygonal ferrite structure are obtained.

[0063] During the cooling of the ferrite zone, the steel plate enters the ultra-fast cooling system and is cooled to T4+5℃ ~ T4 + 25℃, with a cooling rate of 10~20℃ / s, a water pressure of 0.15~0.20MPa, and a cooling roller speed of 1.8~2.2m / s in the ultra-fast cooling system. The purpose is to quickly reduce the temperature of the steel plate to the lowest part of the ferrite phase transformation range, obtain fine acicular ferrite structure, and ensure the yield strength and good low-temperature toughness of the steel plate.

[0064] In the temperature waiting process, after cooling to the intermediate temperature of T4 + 5℃ ~ T4 + 25℃, the steel plate exits the ultra-fast cooling system from the ultra-fast cooling entrance and swings on the ultra-fast cooling entrance roller to wait for temperature, and the waiting time is 8 to 15 seconds. The purpose is that when the temperature of the steel plate is at the lowest part of the ferrite phase transformation range, the acicular ferrite phase transformation begins. In order to obtain more fine ferrite structures, the steel plate needs to stay in this temperature range for a long time to fully transform. According to the results of the present invention, when the waiting time is 8 to 15 seconds, a certain proportion of fine acicular ferrite can be obtained, ensuring good strength and toughness matching of thick submarine pipeline steel plates.

[0065] In the cooling of the bainite zone, the temperature is cooled to T4 - 285℃ ~ T4 - 265℃, the water pressure is 0.30~0.50MPa, and the cooling rate is 8~20℃ / s; the cooling roller speed of the ultra-fast cooling system is 0.6~1.4m / s. The purpose is to quickly cool the steel plate (cooling rate is 8~20℃ / s) when the ferrite phase changes to a certain proportion, so that the bainite phase changes occur, ensuring that the steel plate has a higher tensile strength, thereby reducing the yield strength ratio of the steel plate.

[0066] In the air-cooling self-tempering cooling, after cooling to T4 - 285℃ ~ T4 - 265℃, the steel plate exits the ultra-fast cooling system from the ultra-fast cooling outlet, and then is straightened and air-cooled on the cooling bed for self-tempering until it cools to room temperature. The purpose is, on the one hand, to eliminate or weaken the internal stress of the thick steel plate during the self-tempering cooling process; on the other hand, during the bainite phase transformation process, the MA hard phase is generated, which is not conducive to the toughness of the steel plate and easily leads to high local hardness of the steel plate. Air-cooling self-tempering cooling can partially decompose MA and improve toughness and local hard points. The air-cooling self-tempering conditions are that the cooling bed is transparent and windless, the cooling bed needs to be covered with hot steel plates, the spacing between the steel plates is 1 to 2m, and the temperature of the steel plates is T4 - 305℃ ~ T4 - 105℃. The purpose is to control the flattening density of the steel plates on the cooling bed, the temperature of the cooling bed area, and the air-cooling cooling speed of the steel plates on the cooling bed through batch production, so that the pipeline steel plates on the cooling bed can produce air-cooling self-tempering effects.

[0067] Through the optimization design of low-carbon and low-alloy components, supplemented by the matching special controlled rolling process of five-stage heating + low-temperature and high-pressure rolling in the recrystallization zone + immediate cooling of the intermediate billet + high-temperature and high-pressure rolling in the non-recrystallization zone, and the multi-stage controlled cooling process of air cooling and redistribution in the high-temperature zone + cooling in the ferrite zone + waiting for temperature + cooling in the bainite zone + air cooling and self-tempering cooling, the continuous casting billet with a thickness of ≤320mm is used to produce a steel plate with a thickness of ≥35mm, with a compression ratio of ≤9.14, and the organization is quasi-polygonal ferrite + acicular ferrite + bainite + tempered bainite The composite structure of the steel plate is ≤500MPa, the tensile strength is ≥630MPa, the elongation is ≥35%, the yield strength ratio is ≤0.80, the impact energy KV2 at -40℃ is ≥300J, the impact energy KV2 at -60℃ is ≥250J, the hardness is ≤208HV10, the DWTT drop hammer shear area fraction at -10℃ is 100%, the DWTT drop hammer shear area fraction at -20℃ is ≥90%, and the DWTT ductile-brittle transition temperature is lower than -20℃.

[0068] The thick submarine pipeline steel applicable to the present invention is X70 grade, and the chemical composition of the steel plate includes, by mass percentage, C: 0.045%, Si: 0.12%, Mn: 1.68%, P: 0.0120%, S: 0.0022%, Cr: 0.16%, Ni: 0.16%, Mo: 0.10%, Nb: 0.060%, Ti: 0.016%, Alt: 0.035%, N: 0.0041%, and the rest is iron and unavoidable impurities, and the carbon equivalent CEV of the steel plate is 0.388, and Pcm is 0.150. According to the above chemical composition, smelting is carried out, and a continuous casting billet with a thickness of 320 mm is obtained by light pressure at the end of continuous casting, and the center segregation is 0.5 grade, and the A, B, C, and D classes are all 0.5 grade.

[0069] The specific process steps are: (1) Five-stage heating process: A five-stage heating process consisting of a heat recovery section, a preheating section, a first heating section, a second heating section, and a soaking section is used. The temperature of the heat recovery section is 840°C, the temperature of the preheating section is 950°C, the temperature of the first heating section is 1060°C, the temperature of the second heating section is 1155°C, and the temperature of the soaking section is T1, T1 ≥ T NbN , and T NbN ≤T1≤T NbN +25℃, by calculation, T NbN =1204°C. Therefore, 1204°C≤T1≤1229°C.

[0070] (2) Low temperature and large reduction rolling in the recrystallization zone: By calculation, T2=1121℃. The starting rolling temperature is T2-10℃~T2+30℃, and the final rolling temperature is T2-80℃~T2-40℃, that is, the starting rolling temperature is 1111℃~1151℃, and the final rolling temperature is 1041℃~1081℃. The large reduction rolling process is adopted, the reduction of one pass is ≥31mm, and the reduction of the previous pass is less than or equal to the reduction of the next pass, R n ≤R n+1 , that is, a total of 5 rolling passes, each pass reduction is 31mm, 33mm, 37mm, 40mm and 44mm respectively, the thickness of the intermediate billet after rolling is t z , 3.4t≤t z ≤4.4t, t is the thickness of the steel plate, that is, the thickness of the intermediate billet is 135mm, and the thickness of the finished steel plate t is 35mm.

[0071] (3) Intermediate billet cooling: After the recrystallization zone rolling is completed, the intermediate billet cooling device is immediately used for water cooling to T2-240℃ ~ T2-220℃, that is, 881℃ ~ 901℃.

[0072] (4) High temperature and large reduction rolling in the non-recrystallization zone: Through calculation, T2 is 1121℃ and T3=755℃. The starting rolling temperature is T2-240℃ ~ T2-220℃, and the final rolling temperature is T3~ T3 + 25℃, that is, the starting rolling temperature is 881℃ ~ 901℃, and the final rolling temperature is 755℃ ~ 780℃. During the rolling process in the non-recrystallization zone, the intermediate billet cooling device is used for water cooling between passes; in the high temperature section within the temperature range of the non-recrystallization zone, the pass reduction is ≥21mm, and a total of 4 passes are rolled, with each pass reduction of 21mm, 22mm, 25mm and 26mm respectively; in the low temperature section within the temperature range of the non-recrystallization zone, the pass reduction is 6mm, and the thickness of the finished steel plate is 35mm.

[0073] (5) Air cooling and redistribution in the high temperature zone after rolling: After rolling, the steel plate is air cooled on the conveyor roller to T3 - 50℃ ~T3 - 30℃, that is, 705℃ ~ 725℃, and then enters the ultra-fast cooling system.

[0074] (6) Ferrite zone cooling: The steel plate enters the ultra-fast cooling system and is cooled to T4 + 5 °C ~ T4 + 25 °C. By calculation, T4 = 641 °C, that is, cooled to 646 °C ~ 666 °C. The cooling rate is 18 °C / s, the water pressure is 0.20 MPa, and the cooling roller speed of the ultra-fast cooling system is 2.0 m / s.

[0075] (7) Waiting for temperature: After cooling to the intermediate temperature of 646℃ ~ 666℃, the steel plate exits the ultra-fast cooling system from the ultra-fast cooling entrance and swings on the ultra-fast cooling entrance roller to wait for temperature. The waiting time is 10 seconds.

[0076] (8) Cooling in the bainite zone: The steel plate enters the ultra-fast cooling system again and is cooled to T4 - 285℃ ~ T4 - 265℃. By calculation, T4 = 641℃, that is, it is cooled to 356℃ ~ 376℃. The water pressure is 0.40MPa, the cooling rate is 8~20℃ / s, and the cooling roller speed of the ultra-fast cooling system is 0.6~1.4m / s.

[0077] (9) Air-cooling self-tempering cooling: After cooling to a temperature of 356°C ~ 376°C, the steel plate leaves the ultra-fast cooling system from the ultra-fast cooling outlet, is then straightened, and is air-cooled and self-tempered on the cooling bed until it cools to room temperature; the air-cooling self-tempering conditions are that the cooling bed is airtight and windless, the cooling bed must be fully covered with hot steel plates, the spacing between the steel plates is 1.5m, and the steel plate temperature is T4 - 305°C ~ T4 - 105°C, that is, 336°C ~ 536°C.

[0078] The structure is a composite structure of quasi-polygonal ferrite + acicular ferrite + bainite + tempered bainite, the proportion of MA self-tempering decomposition in bainite is ≤20%, the average grain size of ferrite is 3~6μm, the proportion of quasi-polygonal ferrite is 5%~15%, the proportion of acicular ferrite is 25%~40%, the proportion of bainite is 25%~65%, the proportion of tempered bainite is 5%~20%, the yield strength of the steel plate is ≥500MPa, the tensile strength is ≥630MPa, the elongation is ≥35%, the yield strength ratio is ≤0.80, the impact energy KV2 at -40℃ is ≥300J, the impact energy KV2 at -60℃ is ≥250J, the hardness is ≤208HV10, the area fraction of DWTT drop hammer shear at -10℃ is 100%, the area fraction of DWTT drop hammer shear at -20℃ is ≥90%, and the ductile-brittle transition temperature of DWTT is lower than -20℃. Figure 1 shown.

[0079] Based on the above ideal embodiments of the present invention, the relevant staff can make various changes and modifications without departing from the technical concept of the present invention through the above description. The technical scope of the present invention is not limited to the contents of the specification, and its technical scope must be determined according to the scope of the claims.

Claims

1. Production method of thick submarine pipeline steel plate, It is characterized in that The continuous casting billet is successively subjected to a special controlled rolling process of five-stage heating, low-temperature and large-reduction rolling in the recrystallization zone, intermediate billet cooling, high-temperature and large-reduction rolling in the non-recrystallization zone, and a multi-stage controlled cooling process of air cooling and redistribution in the high-temperature zone after rolling, cooling in the ferrite zone, waiting for temperature, cooling in the bainite zone, and air cooling and self-tempering cooling to make submarine pipeline steel plates.

2. The method for producing thick submarine pipeline steel plate according to claim 1, It is characterized in that The five-stage heating process is specifically as follows: placing the continuous casting billet in a walking beam heating furnace for heating, the length of the heating furnace is 55m, and a five-stage heating process of a heat recovery section, a preheating section, a first heating section, a second heating section and a soaking section is adopted, wherein the temperature of the heat recovery section is ≤850°C, the heating time of the heat recovery section is 0.37-0.41min / mm, the temperature of the preheating section is ≤950°C, the heating time of the preheating section is 0.32-0.35min / mm, the temperature of the first heating section is 1050±15°C, the heating time of the first heating section is 0.22-0.25min / mm, the temperature of the second heating section is 1150±15°C, the heating time of the second heating section is 0.17-0.20min / mm, and the temperature of the soaking section is T 1 , T 1 ≥T NbN , and T NbN ≤T 1 ≤T NbN + 25℃, the heating time in the soaking section is 0.07~0.14min / mm, and the total heating time is 1.15~1.35min / mm, where lg(Nb×N)=3.7-10800 / (T NbN + 273.15).

3. The method for producing thick submarine pipeline steel plate according to claim 1, It is characterized in that The specific process of low temperature and large reduction rolling in the recrystallization zone is as follows: the starting rolling temperature is T 2 -10℃ ~ T 2 + 30℃, final rolling temperature is T 2 - 80℃ ~ T 2 - 40℃; In the low temperature section within the temperature range of the recrystallization zone, a large reduction rolling process is adopted, the pass reduction is ≥31mm, the total number of rough rolling passes is 4 to 6 passes, the temperature difference between adjacent passes is 12℃~18℃, and the reduction of the previous pass is less than or equal to the reduction of the next pass, that is, R n ≤R n+1 , R n and R n+1 are the reductions of the nth pass and the n+1th pass respectively; the thickness of the intermediate billet after rolling is t z , satisfying 3.4t≤t z ≤4.4t, t is the thickness of the finished steel plate, where T 2 is the recrystallization temperature, T 2 =887+464C+6445Nb-644 +890Ti+363Al-357Si.

4. The method for producing thick submarine pipeline steel plate according to claim 1, It is characterized in that The intermediate billet cooling: after the rolling of the austenite recrystallization zone is completed, the intermediate billet cooling device is immediately used for water cooling, the cooling header water pressure is 0.4-0.6MPa, the upper header water flow is 50-150m³ / h, the lower header water flow is 100-300m³ / h, the water flow ratio of the lower header to the upper header is ≥2, the cooling water temperature is 10-30°C, the intermediate billet is cooled back and forth in the cooling device, the roller speed of the cooling device is 0.4-6m / s, and it is cooled to the non-recrystallization rolling temperature range, that is, cooled to T 2 -240℃ ~ T 2 -220℃.

5. The method for producing thick submarine pipeline steel plate according to claim 1, It is characterized in that The non-recrystallization zone is rolled at high temperature and with large reduction: the rolling temperature is T 2 -240℃ ~ T 2 -220℃, final rolling temperature is T 3 ~ T 3 + 25℃; In the high temperature section of the non-recrystallization temperature range, a large reduction rolling process is used. The high temperature section is T 2 -280℃ ~ T 2 -240℃, the number of rolling passes in the high temperature zone is 4 to 6, the rolling speed is 3 to 5m / s, the pass reduction is ≥21mm, and the previous pass reduction is greater than or equal to the next pass reduction, that is, R m ≥R m+1 , R m and R m+1 The rolling reductions are the mth pass and the m+1th pass respectively. The thickness of the billet after rolling is t+3mm ~ t+12mm. The rolling process with small rolling reduction is adopted in the low temperature section within the temperature range of the non-recrystallization zone. The low temperature section is the temperature T 3 + 5℃ ~ T 3 + 30℃, the number of rolling passes in the low temperature section is 1 to 2, the rolling speed is 4 to 6 m / s, the pass reduction is ≤6 mm, and the thickness of the finished steel plate after rolling is t, t≥35 mm; during the rolling process in the non-recrystallization zone, the intermediate billet cooling device is used for water cooling between passes, where T 3 is the temperature at which the transformation from austenite to ferrite begins during cooling, T 3 =910-310C-80Mn-15Cr-80Mo.

6. The method for producing thick submarine pipeline steel plate according to claim 1, It is characterized in that The post-rolling high temperature zone air cooling redistribution: After rolling, the steel plate is air cooled on the conveyor roller, the conveyor roller length is 60m, the roller speed is 2-5m / s, the indoor temperature is 5-39℃, and the steel plate is air cooled to T 3 - 50℃ ~ T 3 - 30℃, then enter the ultra-fast cooling system.

7. The method for producing thick submarine pipeline steel plate according to claim 1, It is characterized in that The ferrite zone cooling: the steel plate enters the ultra-fast cooling system from the ultra-fast cooling inlet, the ultra-fast cooling system has a total of 24 groups of cooling headers, and the cooling length of each group of headers is 1m; 1 to 24 groups of headers are opened for cooling, the cooling rate is 10 to 20°C / s, the water pressure is 0.15 to 0.20MPa, the cooling water temperature is 10 to 30°C, the water flow of the upper header and the lower header is 60 to 200m³ / h, the water flow ratio of the lower header to the upper header is 1.1 to 1.5, the cooling roller speed of the ultra-fast cooling system is 1.8 to 2.2m / s, and the cooling is performed to T 4 + 5℃ ~ T 4 +25℃, where T 4 =830-270C-90Mn-37Ni-70Cr-83Mo.

8. The method for producing thick submarine pipeline steel plate according to claim 1, It is characterized in that The waiting temperature specifically includes cooling to an intermediate temperature T 4 + 5℃ ~ T 4 After the temperature reaches + 25℃, the upper and lower cooling water headers are closed, and the steel plate exits the ultra-fast cooling system from the entrance of the ultra-fast cooling system and swings on the ultra-fast cooling entrance roller to wait for temperature, that is, it swings back and forth on the roller at a speed of 0.5 to 1.5 m / s, the forward and backward moving distance is 5 to 10 m, and the waiting time is 8 to 15 seconds.

9. The method for producing thick submarine pipeline steel plate according to claim 1, It is characterized in that The bainite zone cooling is specifically as follows: the steel plate enters the ultra-fast cooling system again from the ultra-fast cooling inlet, there are 24 groups of cooling headers, and the cooling length of each group of headers is 1m; 1 to 24 groups of headers are opened for cooling, the water pressure is 0.30 to 0.50 MPa, the cooling rate is 8 to 20°C / s, the cooling water temperature is 10 to 26°C, the water flow rate of the upper header and the lower header is 100 to 400 m³ / h, the water flow rate ratio of the lower header to the upper header is 1.2 to 1.4, the cooling roller speed of the ultra-fast cooling system is 0.6 to 1.4 m / s, and the cooling is performed to T 4 - 285℃ ~ T 4 - 265°C.

10. The method for producing thick submarine pipeline steel plate according to claim 1, It is characterized in that The air-cooling self-tempering cooling is specifically: cooling to T 4 - 285℃ ~ T 4 - After 265℃, the steel plate leaves the ultra-fast cooling system from the outlet of the ultra-fast cooling system; then it is straightened and air-cooled and self-tempered on the cooling bed until it cools to room temperature; the air-cooled and self-tempered conditions are that the cooling bed is transparent and windless, the cooling bed needs to be covered with hot steel plates, the spacing between the steel plates is 1 to 2m, and the steel plate temperature is T 4 - 305℃ ~ T 4 - 105°C.

11. The method for producing thick submarine pipeline steel plate according to claim 1, It is characterized in that Using continuous casting billets with a thickness of ≤320mm, the center segregation is not higher than level 0.5, and the inclusions of types A, B, C, and D are all not higher than level 1. Steel plates with a thickness of ≥35mm are produced, and the compression ratio is ≤9.

14.

12. A thick submarine pipeline steel plate produced by the method for producing a thick submarine pipeline steel plate according to any one of claims 1 to 11.

Citation Information

Patent Citations

  • Manufacturing method of steel plate for extra-thick pipeline steel

    CN110629001A

  • Thick-specification pipeline steel and low-compression-ratio production process thereof

    CN111748741A

  • Anti-HIC and anti-scouring X80 pipeline steel plate for deep sea drilling riser and manufacturing method thereof

    CN112195396A

  • Low-yield-ratio high-toughness TMCP type bridge steel plate and production method thereof

    CN112322995A

  • Hot-rolled heavy H-shaped steel with yield strength of 560MPa and production method of hot-rolled heavy H-shaped steel

    CN115161440A

Cited By

  • Low-temperature toughness optimization method for short-process multi-stage phase change control of medium-thickness plate

    CN120350205A