Weld joint shape follow-up local heat treatment method and device
By using a weld-shaped local heat treatment device on curved thin plate metal parts, and using high-energy pulse current to quickly heat the weld, the problem of difficulty in local heat treatment of the welds of curved thin plate parts is solved, and efficient and low-cost weld heat treatment is achieved , avoiding the tissue roughening and performance losses caused by overall heat treatment.
Patent Information
- Application Number
- CN202410997090.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-24
- Publication Date
- 2024-11-26
AI Technical Summary
The prior art is difficult to realize local heat treatment of welds of curved thin plate metal parts, resulting in post-weld deformation, stress cracking, decreased strength, low efficiency and high cost.
Using a weld-shaped local heat treatment device and method, a mobile platform arranged up and down and an automatically telescopic electrode rod is used to form a closed circuit with a DC pulse power supply through flexible electrodes and conductive copper tapes to realize the high-energy pulse current butt weld. Rapid heating to avoid tissue roughening and performance losses caused by overall heat treatment.
It realizes efficient heat treatment in the weld area, avoids roughening of the structure and weakening of performance, retains the beneficial state of the substrate area, reduces cost and energy consumption, and solves the local heat treatment problem of curved thin plate parts.
Smart Images

Figure CN119020582A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of heat treatment of welded components and relates to a method and device for local heat treatment of weld seams in accordance with their shape. Background Art
[0002] Thin plate welding is an important metal material processing and parts manufacturing process, which is widely used in aerospace, shipbuilding, rail transportation, automobile industry, and various engineering equipment. The welding process mainly includes tungsten inert gas arc welding (TIG welding), metal inert gas welding (MIG welding), laser welding, plasma arc welding, etc. based on the principle of fusion welding, and stir friction welding and diffusion welding based on the principle of solid phase welding. Among them, in the process of fusion welding, metal materials will undergo a heating-melting-solidification process. In some solid phase welding, such as stir friction welding, metal materials will undergo severe plastic deformation-high temperature-cooling process, resulting in thermal stress, solidification segregation, and strengthening phase back dissolution in the local area of the weld, which can easily cause deformation, stress cracking, strength reduction and other quality problems of thin plate parts after welding. Therefore, after the metal sheet is welded, the weld area needs to be subjected to necessary heat treatment.
[0003] At present, most metal parts weld heat treatment still adopts the overall heating method in the furnace. First, the heating efficiency is low, and long-term heat preservation may lead to deterioration of the weld area structure and weakening of performance; second, large-scale heating furnaces are required for large welded parts, which are inefficient and costly; third, non-weld substrates are areas that do not require heat treatment, and microstructure changes will inevitably occur during the weld heat treatment process, which can easily lead to overall performance loss of the parts; fourth, curved thin plate parts are very easy to deform during the heat treatment process, and the curved spatial structure cannot be used for local heat treatment of the weld area. Therefore, it is difficult to achieve local heat treatment of curved thin plate parts with existing technologies, and it is urgent to carry out innovations based on new heat treatment principles and new process designs to meet the current technical requirements for local heat treatment of curved thin plate metal parts welds. Summary of the invention
[0004] In view of this, an object of the present invention is to provide a method and device for local heat treatment of welds in accordance with the shape of the welds, so as to solve the problem that welds of curved thin-plate metal parts are difficult to be locally heat treated.
[0005] In order to achieve the above object, the present invention provides the following technical solutions:
[0006] A weld conformal local heat treatment device comprises two movable platforms arranged in an upper and lower manner, two rows of electrode rods which can be automatically extended and retracted are arranged on opposite sides of the two movable platforms, and the two rows of electrode rods located in the upper direction are distributed in a mirror image with the two rows of electrode rods located in the lower direction, wherein any two rows of electrode rods which are not distributed in a mirror image in the upper and lower direction are connected with an electrode clamping plate so that a single row of electrode rods forms a conductor through the electrode clamping plate, the two electrode clamping plates are respectively connected with the positive and negative poles of a direct current pulse power supply through conductive copper strips, and the direct current pulse power supply is a high-current and low-voltage power supply; the two rows of electrode rods connected with the direct current pulse power supply are in contact with the workpiece through two flexible electrodes respectively located on both sides of the weld of the workpiece, so as to realize heating of the weld through a closed loop formed among the weld of the workpiece, the flexible electrodes, the electrode rods, the electrode clamping plate, the conductive copper strip and the direct current pulse power supply.
[0007] Optionally, the conductive copper strip is formed by stacking a red copper bar or multiple layers of red copper foil, and the conductive cross-sectional area of the conductive copper strip is not less than the conductive cross-sectional area of the weld processing area.
[0008] Optionally, the flexible electrode is formed by stacking multiple layers of copper foil, the thickness of the copper foil is 50 to 200 μm, and the stacking thickness is 2 to 5 mm.
[0009] Optionally, the electrode rods are arranged evenly or unevenly along the length of the weld; the electrode rods include an electrode rod body, the electrode rod body is connected to a cylinder via an insulating joint, the cylinder is mounted on a mobile platform, and the electrode rod body has a curved end at one end away from the cylinder.
[0010] Optionally, the voltage of the DC pulse power supply is not greater than 24V. The DC pulse power supply adjusts the pulse current frequency, pulse duty cycle and current intensity according to the type of metal material, the size of the processing area and the heat treatment effect. The average current density corresponding to the aluminum alloy is 8 to 30A / mm 2 The average current density of magnesium alloy is 5-20A / mm 2 The average current density of titanium alloy is 5-10A / mm 2 The average current density of steel is 5-15A / mm 2 .
[0011] Optionally, the mobile platform is mounted on a multi-axis platform so as to move freely with the multi-axis platform to meet the positioning requirements of the weld heat treatment area.
[0012] Optionally, the electrode clamping plate includes two copper plates arranged opposite to each other, the opposite surfaces of the two copper plates are provided with limiting grooves matching the electrode rod, and the two copper plates are locked by a mechanical locking structure to clamp the electrode rod.
[0013] A method for local heat treatment of weld seam conformation is provided, providing a device for local heat treatment of weld seam conformation as described above, comprising the following steps:
[0014] S1 preparation stage: fix the workpiece and remove the oxide scale on both sides of the weld;
[0015] S2 flexible electrode arrangement: flexible electrodes are placed near the weld on the upper and lower sides of the workpiece;
[0016] S3 electrode rod positioning: The electrode rod moves with the mobile platform to a position close to the flexible electrode;
[0017] S4 electrode rod extension and contact: driven by the cylinder, the electrode rod extends to contact the flexible electrode, and the flexible electrode conforms to the workpiece;
[0018] S5 clamping and circuit closing: After all electrode rods are in contact with the flexible electrode, the cylinder drives the electrode rod to apply a certain pressure to the flexible electrode to ensure that the electrode rod is in close contact with the flexible electrode; then, the electrode clamping plate is clamped to connect the electrode rod, so that the workpiece weld forms a closed circuit through the flexible electrode and the electrode rod, the electrode clamping plate, the conductive copper belt, and the DC pulse power supply;
[0019] S6 Heating treatment: Start the DC pulse power supply, and the temperature of the weld will rise rapidly under the action of Joule heat. After the heat treatment is completed, turn off the DC pulse power supply;
[0020] S7 repeat processing: move the flexible electrode to the next position of the weld to be processed, and repeat steps S2 to S8 until the heat treatment of the entire weld is completed;
[0021] S8 Take out the workpiece: take out the workpiece after the heat treatment is completed.
[0022] Optionally, in step S2, the distance between the inner side of the flexible electrode and the edge of the weld is determined according to the width of the heat affected zone of the weld; the wider the heat affected zone of the weld, the greater the distance between the inner side of the flexible electrode and the edge of the weld; the distance between the inner side of the flexible electrode and the edge of the weld is 1 to 30 mm.
[0023] Optionally, the order of extending the electrode rods in each row is from the middle to both sides; under the action of the electrode rods, the average pressure of the flexible electrodes on the metal sheet is 0.5MPa to 1.5MPa to ensure good conductive contact.
[0024] The beneficial effects of the present invention are:
[0025] 1. The present invention uses high-energy pulse current to act on the weld area to achieve heat treatment, which has the advantages of high heating efficiency, short processing time, and concentrated processing area, and can avoid coarsening of the weld area structure and weakening of performance.
[0026] 2. The present invention only performs heat treatment on the weld, thereby retaining the beneficial state of the pre-treatment of the substrate area, avoiding performance loss in the non-weld area of the part, and increasing the flexibility of the part process design.
[0027] 3. The present invention solves the problem that the weld of a metal sheet part with curved spatial structure characteristics is deformed during overall heat treatment and cannot be subjected to local heat treatment.
[0028] 4. The present invention does not require a large heat treatment furnace, and has low cost and low energy consumption.
[0029] Other advantages, objectives and features of the present invention will be described in the following description to some extent, and to some extent, will be obvious to those skilled in the art based on the following examination and study, or can be taught from the practice of the present invention. The objectives and other advantages of the present invention can be realized and obtained through the following description. BRIEF DESCRIPTION OF THE DRAWINGS
[0030] In order to make the purpose, technical solutions and advantages of the present invention more clear, the present invention will be described in detail below in conjunction with the accompanying drawings, wherein:
[0031] Figure 1 It is a schematic diagram of a weld conformal local heat treatment device;
[0032] Figure 2 is a schematic diagram of the weld shape;
[0033] Figure 3 is a schematic diagram of the structure of the electrode rod;
[0034] Figure 4 It is a structural schematic diagram of the electrode clamping plate;
[0035] Figure 5 Schematic diagram of the structure of the flexible electrode;
[0036] Figure 6 Schematic diagram of the extension sequence of the electrode rods;
[0037] Figure 7 This is the straight line projection weld part drawing of TIG welding of 7 series aluminum alloy curved thin plate;
[0038] Figure 8 This is the microstructure diagram of the TIG weld of 7 series aluminum alloy curved thin plate before and after high temperature annealing heat treatment;
[0039] Fig. 9 It is the laser welding curve projection weld part drawing of 2 series aluminum alloy curved thin plate;
[0040] Fig.10 This is the microstructure diagram of the laser weld of 2 series aluminum alloy curved thin plate before and after annealing heat treatment;
[0041] Fig.11 It is the curve projection weld part drawing of 420 stainless steel flat plate friction stir weld;
[0042] Fig.12 This is the microstructure diagram of 420 stainless steel flat plate friction stir weld before and after annealing heat treatment.
[0043] Figure numerals: DC pulse power supply 1, conductive copper belt 2, moving platform 3, electrode rod 4, electrode clamping plate 5, flexible electrode 6, welding sheet 7, cylinder 41, insulating joint 42, electrode rod body 43, arc surface end 44. DETAILED DESCRIPTION
[0044] The following describes the embodiments of the present invention by specific examples, and those skilled in the art can easily understand other advantages and effects of the present invention from the contents disclosed in this specification. The present invention can also be implemented or applied through other different specific embodiments, and the details in this specification can also be modified or changed in various ways based on different viewpoints and applications without departing from the spirit of the present invention. It should be noted that the illustrations provided in the following embodiments only illustrate the basic concept of the present invention in a schematic manner, and the following embodiments and features in the embodiments can be combined with each other without conflict.
[0045] Among them, the drawings are only used for illustrative explanations, and they only represent schematic diagrams rather than actual pictures, and should not be understood as limitations on the present invention. In order to better illustrate the embodiments of the present invention, some parts of the drawings may be omitted, enlarged or reduced, and do not represent the size of actual products. For those skilled in the art, it is understandable that some well-known structures and their descriptions in the drawings may be omitted.
[0046] The same or similar numbers in the drawings of the embodiments of the present invention correspond to the same or similar parts; in the description of the present invention, it should be understood that if the terms "upper", "lower", "left", "right", "front", "back" and the like indicate directions or positional relationships, they are based on the directions or positional relationships shown in the drawings, which are only for the convenience of describing the present invention and simplifying the description, rather than indicating or implying that the device or element referred to must have a specific direction, be constructed and operated in a specific direction. Therefore, the terms describing the positional relationship in the drawings are only used for illustrative purposes and cannot be understood as limiting the present invention. For ordinary technicians in this field, the specific meanings of the above terms can be understood according to specific circumstances.
[0047] See also Figures 1 to 12A weld conformal local heat treatment device comprises two movable platforms 3 arranged in an upper and lower manner, two rows of automatically retractable electrode rods 4 are arranged on opposite sides of the two movable platforms 3, and the two rows of electrode rods located above are distributed in a mirror image with the two rows of electrode rods located below, wherein any two rows of electrode rods distributed in a non-mirror image manner up and down are connected with an electrode clamping plate 5 so that a single row of electrode rods forms a conductor through the electrode clamping plate 5, and the two electrode clamping plates 5 are respectively connected to the positive and negative poles of a DC pulse power supply 1 through a conductive copper belt 2, and the DC pulse power supply 1 is a high-current and low-voltage power supply; the two rows of electrode rods 4 connected to the DC pulse power supply 1 are in contact with the workpiece through two flexible electrodes 6 located on both sides of the weld of the workpiece, so as to realize heating of the weld through a closed loop formed among the weld of the workpiece, the flexible electrode 6, the electrode rod 4, the electrode clamping plate 5, the conductive copper belt 2, and the DC pulse power supply 1.
[0048] The welds applicable to the device include but are not limited to the welds of metal parts with curved thin plate features, and the shapes of the welds are as follows: Figure 2 As shown, (a) - flat thin plate straight weld, (b) - flat thin plate curved weld, (c) - curved thin plate straight projection weld, (d) - curved thin plate curved projection weld. The thickness of the metal sheet is 1 to 10 mm, and the welding types of the welds include tungsten inert gas arc welding (TIG welding), metal inert gas welding (MIG welding), laser welding, plasma arc welding, stir friction welding, etc. The metal materials are aluminum alloy, magnesium alloy, titanium alloy, steel, etc.
[0049] The DC pulse power supply 1 is a high-current low-voltage power supply with a voltage not greater than 24. The pulse current frequency, pulse duty cycle, current intensity, etc. can be adjusted according to the type of metal material, the size of the processing area, the heat treatment effect and other conditions. Preferably, the average current density of the aluminum alloy is 8-30A / mm 2 , the average current density of magnesium alloy is 5~20A / mm 2 , the average current density of titanium alloy is 5~10A / mm 2 , steel average current density 5~15A / mm 2 .
[0050] The conductive copper strip 2 is formed by stacking a copper strip or multiple layers of copper foil, which is selected according to the specific situation. The conductive cross-sectional area of the copper strip is generally not less than the conductive cross-sectional area of the weld processing area.
[0051] The mobile platform 3 is installed on a multi-axis platform (≥3 axes) and can move freely with the multi-axis platform to meet the positioning requirements of the weld heat treatment area. Generally, the mobile platform 3 moves to a height of 10 to 50 mm from the lower end of the electrode rod to the weld surface.
[0052] The electrode rods 4 are distributed in a mirror image on both sides of the metal sheet, and two rows of electrode rods on each side are arranged on both sides of the weld. The number of electrode rods in each row depends on the length of the weld for a single heat treatment, the size of the electrode rods, and the arrangement method. Along the length direction of the weld, the electrode rods can be arranged evenly or unevenly to achieve the purpose of current density control. Figure 3 As shown, the electrode rod 4 includes an electrode rod body 43, which is connected to a cylinder 41 through an insulating joint 42. The cylinder 41 is installed on the mobile platform 3, and the end of the electrode rod body 43 away from the cylinder 41 has an arc end 44. The rear end of each electrode rod body 43 is connected to an independent cylinder 41, and the electrode rod body 43 and the cylinder 41 are connected through an insulating joint 42 made of ceramic, bakelite, etc. The cylinder 41 is fixed to the mobile platform 3 in an array according to the shape of the weld, and the cylinder 41 can independently control the extension and contraction of the electrode rod body 43. The electrode rod body 43 is composed of a vertical rod body and an arc end 44. The cross-section of the rod body is circular (diameter is generally 8 to 20 mm), rectangular (width does not exceed the width of the flexible electrode 6), etc. The rod body is made of copper, tungsten copper alloy, and the arc end 44 is made of tungsten copper alloy. After the electrode rod body 43 is extended, it contacts and presses the flexible electrode 6 to ensure that the flexible electrode 6 is in close contact with the metal sheet.
[0053] like Figure 4 As shown, the electrode clamping plate 5 includes two copper plates arranged opposite to each other, and the opposite surfaces of the two copper plates are provided with limiting grooves matching the electrode rod 4, and the two copper plates are locked by a mechanical locking structure to clamp the electrode rod 4. After the electrode rod is in place, the two copper plates are connected and mechanically clamp the electrode rod, the shape of the limiting groove is consistent with the cross-sectional shape of the electrode rod, and the position of the limiting groove corresponds to the position of the electrode rod, ensuring that the copper plate is in close contact with the electrode rod.
[0054] The flexible electrode 6 is formed by stacking multiple layers of copper foil. Figure 5 As shown, the copper foil has a thickness of 50 to 200 μm and a stacking thickness of 2 to 5 mm. The copper foil is in the shape of a long strip with a width of 10 to 20 mm. The length is determined according to the length of the weld processed in a single process, generally 100 to 500 mm. The specific shape in the length direction matches the curved shape of the weld. The flexible electrode 6 can be bent to achieve a close fit with the curved surface of the part under the pressure of the electrode rod.
[0055] The present invention also provides a weld conformal local heat treatment method, comprising the following steps:
[0056] (1) Fix the curved thin-plate metal parts with welds and grind off the oxide scale on both sides of the welds;
[0057] (2) The flexible electrodes 6 are placed close to the two sides of the weld, with two flexible electrodes 6 on each side of the thin plate, in a mirror-image distribution;
[0058] (3) The mirror array telescopic electrode rods 4 are symmetrically installed on the upper and lower mobile platforms 3 in a mirror distribution, and move with the mobile platform 3 to the position of the flexible electrode 6;
[0059] (4) The two rows of telescopic electrode rods on both sides of the thin plate extend synchronously in a mirrored manner under the driving action of the cylinder and contact the upper flexible electrode 6, which conforms to the curved surface of the part;
[0060] (5) After all electrode rods are in contact with the upper flexible electrode 6, the cylinder drives the electrode rod to apply a certain pressure to the flexible electrode 6 to ensure that the flexible electrode 6 is in close contact with the curved surface of the part;
[0061] (6) The electrode clamping plates 5 on both sides of the weld are clamped and connected to the electrode rods;
[0062] (7) The conductive copper tape 2 connects the electrode clamping plate 5 and the DC pulse power supply 1 to form a closed loop;
[0063] (8) Turn on the power supply. Under the action of Joule heat, the temperature of the weld seam rises rapidly and the heat treatment is completed. Then turn off the power supply.
[0064] (9) moving the flexible electrode 6 along the weld to the next untreated position, and repeating steps (2) to (8) until the heat treatment of the entire weld is completed;
[0065] (10) Take out the metal sheet parts and complete the local heat treatment of the welds of the parts.
[0066] Optionally, in step (2), after the flexible electrode 6 is placed, the distance between its inner side and the edge of the weld is generally 1 to 30 mm, depending on the width of the heat affected zone of the weld. The wider the heat affected zone, the greater the distance.
[0067] Optionally, in step (4), the order of extending the electrode rods in each column is generally from the middle to both sides, such as Figure 6 As shown, (a)-(b)-(c)-(d).
[0068] Optionally, in step (8), the types of heat treatment include but are not limited to annealing, solution treatment, aging, etc.
[0069] Traditional processes cannot meet the local heat treatment requirements of metal sheet welds, especially welds with curved surface features. The only way to heat treat the parts with welds is to place them in a furnace as a whole. This is not only inefficient, energy-intensive, and time-consuming, but also easy to cause changes in the structure of the weld and the entire part, leading to performance loss. The present invention solves the above problems very well. The present invention adopts a combination of a mirror array telescopic electrode rod and a flexible electrode to achieve a tight fit between the electrode and the curved surface of the part, and then uses the Joule heat of the electric current to achieve rapid heating of the weld, solving the industry problem that it is difficult to perform local heat treatment on curved thin-plate metal parts welds, and overcoming the defects of the prior art.
[0070] Example 1
[0071] A weld conformal local heat treatment method is used to treat aluminum alloy welds. The welds are 7 series aluminum alloy TIG welds. The thickness of the aluminum alloy sheet is 3 mm. The welds are curved thin plate straight line projection welds. The weld width is 7 mm. The size of the 7 series aluminum alloy curved thin plate TIG welding parts is as follows: Figure 7 As shown, the weld is now subjected to high temperature annealing heat treatment in order to eliminate welding stress and coarse solidified phase at grain boundaries. The steps are as follows:
[0072] (1) Fix the 7 series aluminum alloy curved thin plate TIG welding parts and grind off the oxide scale on both sides of the weld;
[0073] (2) 50 layers of copper foil with a size of 200 mm × 10 mm and a thickness of 100 μm are stacked to form a single flexible electrode. The flexible electrodes are placed at the positions close to the start of one end of the weld, with the inner side of the flexible electrode 5 mm away from the edge of the weld. Two flexible electrodes are placed on each side of the upper and lower sides of the thin plate, in a mirror-image distribution.
[0074] (3) The mirror array telescopic electrode rods are symmetrically installed on the upper and lower mobile platforms in a mirror distribution, and move to the flexible electrode position with the mobile platform. The electrode rod cross-section is circular, the rod diameter is 10 mm, the electrode rod material is copper, the end shape is a hemispherical arc surface, and the distance between the lower end of the electrode rod and the upper and lower surfaces of the thin plate is no more than 20 mm;
[0075] (4) The two rows of telescopic electrode rods on both sides of the thin plate extend synchronously from the middle to both sides in a mirror-image manner under the driving action of the cylinder and contact the upper flexible electrode, which conforms to the curved surface of the part;
[0076] (5) After all electrode rods are in contact with the upper flexible electrode, the cylinder drives the electrode rod to apply pressure to the flexible electrode. The pressure of the flexible electrode on the thin plate is 0.8 MPa, ensuring that the flexible electrode is in close contact with the surface of the part;
[0077] (6) Clamp the electrode clamping plates on both sides of the weld and connect the electrode rods;
[0078] (7) The conductive copper tape connects the electrode clamping plate and the DC pulse power supply to form a closed loop;
[0079] (8) Start the power supply and adjust the current parameters to: pulse current frequency 100 Hz, pulse duty cycle 50%, current intensity 20 A / mm 2 , under the action of Joule heat, the temperature of the weld is raised to 450±5℃ within 20s, and the heat treatment is completed for 5 minutes, and the power is turned off;
[0080] (9) moving the flexible electrode along the weld to the next untreated position, and repeating steps (2) to (8) until the heat treatment of the entire weld is completed;
[0081] (10) Take out the metal sheet parts and complete the local heat treatment of the welds of the parts.
[0082] After heat treatment, the thin plate parts are not deformed, the matrix structure and performance remain the same as before treatment, and the weld grain structure is as follows: Figure 8 As shown, it can be seen that after short-time pulse current high-temperature annealing treatment, the grain structure of the weld and the substrate did not coarsen, and the coarse solidified eutectic phase at the grain boundary was eliminated, and the grain boundary became clearer.
[0083] Example 2
[0084] A weld conformal local heat treatment method is used to treat aluminum alloy welds. The welds are 2 series aluminum alloy laser welds. The thickness of the aluminum alloy sheet is 2 mm. The welds are curved thin plate curved projection welds. The weld width is 3 mm. The size of the 2 series aluminum alloy curved thin plate laser welded parts is as follows: Fig. 9 As shown, the weld is now subjected to stress relief annealing heat treatment to eliminate welding stress. The steps are:
[0085] (1) Fix the laser-welded parts of the 2 series aluminum alloy curved thin plate and grind off the oxide scale on both sides of the weld;
[0086] (2) 30 layers of copper foil with a size of 100 mm × 10 mm and a thickness of 100 μm are stacked to form a single flexible electrode. The flexible electrodes are placed at the positions close to the start of one end of the weld. The inner side of the flexible electrode is 2 mm away from the edge of the weld. Two flexible electrodes are placed on the upper and lower sides of the thin plate in a mirror-image distribution.
[0087] (3) The mirror array telescopic electrode rods are symmetrically installed on the upper and lower mobile platforms in a mirror distribution, and move to the flexible electrode position with the mobile platform. The electrode rod cross-section is circular, the rod diameter is 10 mm, the electrode rod material is copper, the end shape is a hemispherical arc surface, and the distance between the lower end of the electrode rod and the upper and lower surfaces of the thin plate is no more than 20 mm;
[0088] (4) The two rows of telescopic electrode rods on both sides of the thin plate extend synchronously from the middle to both sides in a mirror-image manner under the driving action of the cylinder and contact the upper flexible electrode, which conforms to the curved surface of the part;
[0089] (5) After all electrode rods are in contact with the upper flexible electrode, the cylinder drives the electrode rod to apply pressure to the flexible electrode. The pressure of the flexible electrode on the thin plate is 0.8 MPa, ensuring that the flexible electrode is in close contact with the surface of the part;
[0090] (6) Clamp the electrode clamping plates on both sides of the weld and connect the electrode rods;
[0091] (7) The conductive copper tape connects the electrode clamping plate and the DC pulse power supply to form a closed loop;
[0092] (8) Start the power supply and adjust the current parameters to: pulse current frequency 50 Hz, pulse duty cycle 25%, current intensity 15 A / mm 2 , under the action of Joule heat, the temperature of the weld is raised to 350±5℃ within 45s, and the heat treatment is completed for 3 minutes, and the power is turned off;
[0093] (9) moving the flexible electrode along the weld to the next untreated position, and repeating steps (2) to (8) until the heat treatment of the entire weld is completed;
[0094] (10) Take out the metal sheet parts and complete the local heat treatment of the welds of the parts.
[0095] After heat treatment, the thin plate parts are not deformed, and the weld grain structure is as follows: Fig.10 As shown, it can be seen that after short-time pulse current annealing treatment, the weld grain structure did not coarsen.
[0096] Example 3
[0097] A weld conformal local heat treatment method is used to treat aluminum alloy welds. The welds are 420 stainless steel friction stir welding welds. The thickness of the stainless steel sheet is 2 mm. The welds are plane thin plate curved projection welds. The weld width is 12 mm. The size of the 420 stainless steel friction stir welding parts is as follows: Fig.12 As shown, the weld is now subjected to annealing heat treatment. The steps are:
[0098] (1) Fix the 420 stainless steel friction stir welding parts and grind off the oxide scale on both sides of the weld;
[0099] (2) 50 layers of copper foil with a size of 100 mm × 10 mm and a thickness of 100 μm are stacked to form a single flexible electrode. The flexible electrodes are placed at the positions close to the start of one end of the weld, with the inner side of the flexible electrode 5 mm away from the edge of the weld. Two flexible electrodes are placed on each side of the upper and lower sides of the thin plate, in a mirror-image distribution.
[0100] (3) The mirror array telescopic electrode rods are symmetrically installed on the upper and lower moving platforms in a mirror distribution, and move to the flexible electrode position with the moving platform. The electrode rod cross-section is circular, the rod diameter is 10 mm, the electrode rod material is tungsten copper alloy, the end shape is a hemispherical arc surface, and the distance between the lower end of the electrode rod end and the upper and lower surfaces of the thin plate is no more than 20 mm;
[0101] (4) The two rows of telescopic electrode rods on both sides of the thin plate extend synchronously from the middle to both sides in a mirror-image manner under the driving action of the cylinder and contact the upper flexible electrode, which conforms to the curved surface of the part;
[0102] (5) After all electrode rods are in contact with the upper flexible electrode, the cylinder drives the electrode rod to apply pressure to the flexible electrode. The pressure of the flexible electrode on the thin plate is 1.5 MPa, ensuring that the flexible electrode is in close contact with the surface of the part;
[0103] (6) Clamp the electrode clamping plates on both sides of the weld and connect the electrode rods;
[0104] (7) The conductive copper tape connects the electrode clamping plate and the DC pulse power supply to form a closed loop;
[0105] (8) Start the power supply and adjust the current parameters to: pulse current frequency 100 Hz, pulse duty cycle 50%, current intensity 8 A / mm 2 , under the action of Joule heat, the temperature of the weld is raised to 800±5℃ within 60s, and the heat treatment is completed by keeping the temperature for 3 minutes, and then the power is turned off;
[0106] (9) moving the flexible electrode along the weld to the next untreated position, and repeating steps (2) to (8) until the heat treatment of the entire weld is completed;
[0107] (10) Take out the metal sheet parts and complete the local heat treatment of the welds of the parts.
[0108] After heat treatment, the thin plate parts are not deformed, and the weld grain structure is as follows: Fig.12 As shown, it can be seen that after short-time pulse current annealing treatment, the weld grain structure did not undergo refinement and coarsening.
[0109] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the purpose and scope of the technical solution, which should be included in the scope of the claims of the present invention.
Claims
1. A weld conformal local heat treatment device, characterized in that: The invention comprises two movable platforms (3) arranged vertically, two rows of automatically retractable electrode rods (4) are arranged on opposite sides of the two movable platforms (3), and the two rows of electrode rods located at the top are arranged in a mirror image with the two rows of electrode rods located at the bottom, wherein any two rows of electrode rods that are not arranged vertically in a mirror image are connected to an electrode clamping plate (5) so that a single row of electrode rods forms a conductor through the electrode clamping plate (5), and the two electrode clamping plates are respectively connected to the positive and negative electrodes of a DC pulse power supply (1) through conductive copper strips (2), and the DC pulse power supply (1) is a high-current, low-voltage power supply; Two rows of electrode rods (4) connected to a DC pulse power supply (1) contact a workpiece through two flexible electrodes (6) located respectively on both sides of a weld of the workpiece, so as to heat the weld through a closed loop formed among the weld of the workpiece, the flexible electrodes (6), the electrode rods (4), the electrode clamping plate (5), the conductive copper strip (2), and the DC pulse power supply (1).
2. The weld conformal local heat treatment device according to claim 1, characterized in that: The conductive copper strip (2) is formed by stacking a red copper strip or multiple layers of red copper foil, and the conductive cross-sectional area of the conductive copper strip (2) is not less than the conductive cross-sectional area of the weld processing area.
3. The weld conformal local heat treatment device according to claim 1, characterized in that: The flexible electrode (6) is formed by stacking multiple layers of copper foil, the thickness of the copper foil is 50 to 200 μm, and the stacking thickness is 2 to 5 mm.
4. The weld conformal local heat treatment device according to claim 1, characterized in that: The electrode rods are arranged evenly or unevenly along the length direction of the weld; the electrode rod (4) comprises an electrode rod body (43), the electrode rod body (43) is connected to a cylinder (41) via an insulating joint (42), the cylinder (41) is mounted on a movable platform (3), and the end of the electrode rod body (43) away from the cylinder has a curved end (44).
5. The weld conformal local heat treatment device according to claim 1, characterized in that: The voltage of the DC pulse power supply (1) is not greater than 24V. The DC pulse power supply (1) adjusts the pulse current frequency, pulse duty cycle and current intensity according to the type of metal material, the size of the treatment area and the heat treatment effect. The average current density corresponding to aluminum alloy is 8 to 30A / mm 2 The average current density of magnesium alloy is 5-20A / mm 2 The average current density of titanium alloy is 5-10A / mm 2 The average current density of steel is 5-15A / mm 2 .
6. The weld conformal local heat treatment device according to claim 1, characterized in that: The mobile platform (3) is installed on the multi-axis platform so as to move freely with the multi-axis platform to meet the positioning requirements of the weld heat treatment area.
7. The weld conformal local heat treatment device according to claim 1, characterized in that: The electrode clamping plate (5) comprises two copper plates arranged opposite to each other, the opposite surfaces of the two copper plates are provided with limiting grooves matching the electrode rod, and the two copper plates are locked by a mechanical locking structure to clamp the electrode rod (4).
8. A method for local heat treatment of weld seams, characterized in that: A weld conformal local heat treatment device as claimed in any one of claims 1 to 7 is provided, comprising the following steps: S1 preparation stage: fix the workpiece and remove the oxide scale on both sides of the weld; S2 flexible electrode arrangement: flexible electrodes (6) are placed near the weld on the upper and lower sides of the workpiece; S3 electrode rod positioning: the electrode rod (4) moves with the mobile platform (3) to a position close to the flexible electrode (6); S4: electrode rod extending and contacting: driven by the cylinder (41), the electrode rod (4) extends to contact the flexible electrode (6), and the flexible electrode (6) conforms to the workpiece; S5 clamping and circuit closing: after all electrode rods are in contact with the flexible electrode (6), the cylinder (41) drives the electrode rod (4) to apply a certain pressure to the flexible electrode (6) to ensure that the electrode rod (4) and the flexible electrode (6) are in close contact; then, the electrode clamping plate (5) is clamped to connect the electrode rod (4), so that the weld seam of the workpiece forms a closed circuit through the flexible electrode (6) and the electrode rod (4), the electrode clamping plate (5), the conductive copper strip (2), and the DC pulse power supply (1); S6 heating treatment: starting the DC pulse power supply (1), rapidly heating the weld under the action of Joule heat, and shutting off the DC pulse power supply (1) after the heat treatment is completed; S7 repeat processing: move the flexible electrode (6) to the next position of the weld to be processed, and repeat steps S2 to S8 until the heat treatment of the entire weld is completed; S8 Take out the workpiece: take out the workpiece after the heat treatment is completed.
9. The weld conformal local heat treatment method according to claim 8, characterized in that: In step S2, the distance between the inner side of the flexible electrode and the edge of the weld is determined according to the width of the heat affected zone of the weld; the wider the heat affected zone of the weld, the greater the distance between the inner side of the flexible electrode and the edge of the weld; the distance between the inner side of the flexible electrode and the edge of the weld is 1 to 30 mm.
10. The weld conformal local heat treatment method according to claim 8, characterized in that: The order of extension of each row of electrode rods is from the middle to both sides; under the action of the electrode rods (4), the average pressure of the flexible electrodes (6) on the metal sheet is 0.5MPa to 1.5MPa, so as to ensure good conductive contact.
Citation Information
Cited By
Non-uniform constitutive parameter characterization method of thick plate friction stir welding seam
CN119375225A
Pulse discharge hot-pressing seal welding device and seal welding method for sheathing powder discharging pipe
CN120421829A