TC16 titanium alloy rod wire material and processing method thereof

By optimizing the chemical composition and processing technology of TC16 titanium alloy, the problem of TC16 titanium alloy bars is solved, the degree of tissue refinement and performance of TC16 titanium alloy rods are improved, and high strength and high plasticity that meets national standards are achieved .

CN119020635AInactive Publication Date: 2024-11-26XIAN KEEN TITANIUM NEW MATERIAL TECH CO LTD

Patent Information

Application Number
CN202411137638.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-19
Publication Date
2024-11-26
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The existing TC16 titanium alloy rods are prone to mass defects such as prone to cracking and slipping during the upsetting process, and the structure is difficult to refine, which affects its performance.

Method used

By optimizing the chemical composition and processing technology of TC16 titanium alloy, including three vacuum consumable smelting, segmented forging, electric furnace rolling, cold rotary forging, electric straightening and grinding and polishing, adjusting grain structure and alloy element content, and improving materials Plasticity and tissue refinement.

Benefits of technology

It has achieved high annealing tensile strength and elongation of TC16 titanium alloy rods, reduced production costs, avoided cracking problems, and met the requirements of Class 1 standards of the national military standards.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119020635A_ABST
    Figure CN119020635A_ABST
Patent Text Reader

Abstract

The invention relates to a TC16 titanium alloy bar wire and a processing method thereof, TC16 components are improved, a forging and rolling process is further optimized, a mature titanium alloy cold processing technology is applied, crystal grains are refined through rotary forging of a rolled semi-finished product, so that the bar structure is close to the structure of the wire, and meanwhile, an original straightening machine is transformed, so that the quality of the TC16 titanium alloy bar wire is improved, and the quality of the TC16 titanium alloy bar wire is improved. And meanwhile, by means of the straightening mode, the internal stress of the material is reduced, and the problem that a product is prone to cracking after being upset is solved. And batch production is realized, the production efficiency is improved, and the cost is reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of titanium alloy material processing, in particular to a TC16 titanium alloy rod and wire material and a processing method thereof. Background Art

[0002] TC16 titanium alloy is a typical martensitic (α+β) two-phase titanium alloy. It belongs to the Ti-Al-Mo-V series of high-strength titanium alloys. It contains α-stabilizing element Al and isomorphous β-stabilizing elements Mo and V, which maintains high strength while also showing good plasticity. The alloy is mainly used in a heat-treated strengthened state, and its room temperature tensile strength limit is above 1100MPa. TC16 has good plasticity in the quenched state, and can obtain higher strength through enhanced heat treatment. It is particularly suitable for making fasteners with excellent performance and has been widely used in the aerospace field.

[0003] Conventional TC16 rods and wires are processed through the process of "melting → forging → billet rolling → finished product rolling → annealing → straightening → machining". Since the material needs to be cold-forged, the plasticity of the material is very high, which requires its microstructure to be more uniform and refined. The deformation rate of rods is smaller than that of wires, so the difficulty of refining the structure is greater, and the product will produce quality defects such as easy cracking and slipping during the upsetting process.

[0004] The invention with the publication (announcement) number CN117187723A discloses a processing method for TC16 titanium alloy bars for cold heading, wherein the selected bar blank is heated and then rolled through a flat square hole, air-cooled after rolling, peeled, heated at atmospheric pressure, straightened, ground and polished, and coated to provide large-size TC16 bars that meet the requirements of cold heading. The Chinese invention patent with the publication (announcement) number CN108067519B discloses a method for preparing TC16 titanium alloy wire with ultrafine grain structure, wherein the TC16 titanium alloy wire blank with α phase and β phase size of about 1 to 2 μm after hot working deformation is used, and after surface treatment, multiple passes of room temperature roller die drawing deformation are performed, and the cumulative deformation reaches 75% to 90%, and the deformation at room temperature has a significant effect on grain refinement. The invention with the publication (announcement) number CN103736727B discloses a temperature-controlled continuous rolling method for TC16 titanium alloy bars. Electromagnetic induction heating equipment and cooling bellows are added to the titanium alloy bar continuous rolling production line to respectively perform timely online compensation heating and spray cooling on the titanium bars, and the rolled pieces in the continuous rolling production are effectively temperature-controlled and rolled out titanium alloy bars of all specifications from Φ6 to Φ30 mm. The above-mentioned prior art has not been reported to improve the performance by optimizing the organizational composition of TC16 bars combined with cold heading process. Summary of the invention

[0005] The purpose of the present invention is to provide a TC16 titanium alloy rod and wire and a processing method thereof, by optimizing the internal grain structure of the TC16 rod, adjusting the content of alloy elements, improving the rod and wire production method, and improving the plasticity index of the rod, so as to meet the cold heading requirements and solve the quality defects of easy cracking and slipping generated in the upsetting process of the product.

[0006] To achieve the above object, the present invention provides the following technical solutions:

[0007] The chemical composition of the TC16 titanium alloy rod and wire provided by the present invention mainly includes, by mass fraction percentage, 2.4 to 3.6 Al, 4.5 to 5.3 Mo, 4.0 to 5.0 V; impurities include not more than 0.035 Fe, not more than 0.05 C, not more than 0.1 Zr, not more than 0.1 N, and not more than 0.012 O; the single content of other impurities is not more than 0.1, and the total content is not more than 0.4; the balance is Ti.

[0008] The annealed tensile strength of the TC16 titanium alloy rod and wire is above 830 MPa, the elongation is above 20%, and the shear strength is above 690 MPa.

[0009] The present invention also provides a method for processing TC16 titanium alloy rods and wires, using the above-mentioned TC16 titanium alloy components, comprising the following steps:

[0010] Step 1: After the TC16 titanium alloy components are subjected to three vacuum consumable melting processes to form an ingot, the ingot is peeled and turned to obtain an ingot;

[0011] Step 2: Forging treatment: The forging temperature is 100℃~200℃ above the phase change point. The forging requires three upsetting and three drawing, and the combination of β forging + two-phase zone upper forging is adopted; water cooling after forging;

[0012] Step 3: Rolling treatment: Use an electric furnace to heat in the α+β phase region, and the heating temperature is the phase transition point T β Below 50℃~100℃;

[0013] Step 4: Use a centerless lathe to remove surface defects of the blank by peeling; the blank specification is Φ4.0~Φ12, the peeling amount is 0.5mm; the blank specification is Φ13~Φ18, the peeling amount is 1.0mm; the blank specification is Φ19~Φ24, the peeling amount is 1.5mm; the blank specification is Φ25 or above, the peeling amount is 2.0mm;

[0014] Step 5: Use a cold rotary forging machine to perform 20-50% cold deformation rotary forging processing;

[0015] Step 6: Annealing heat treatment: The annealing temperature is 700℃~820℃, and after keeping warm for 120min, air-cooling and furnace-cooling are performed at 2℃~4℃ / min. When the temperature is below 550℃, the steel is taken out of the furnace and air-cooled;

[0016] Step 7: Use a vertical electric contact variable controllable straightening machine for straightening, and the straightness meets 3mm / m;

[0017] Step 8: Grinding and polishing with a carbon chloride medium-soft grinding wheel; polishing allowance 0.01mm-0.02mm; finally processing into finished rods and wires of Φ4.0-Φ20.

[0018] In the processing method of the above-mentioned TC16 titanium alloy rod and wire, in step 2, the forging treatment includes one-fire forging and two-fire forging; the first-fire forging is charged into the furnace at 800°C, preheated for 90 minutes, heated to 1000°C~1100°C and kept warm for 150 minutes, forged out of the furnace, and the final forging temperature is above 650°C; the second-fire forging is charged into the furnace at 820°C~900°C, kept warm for 120 minutes, forged out of the furnace, and the final forging temperature is controlled to be above 600°C.

[0019] In the processing method of the above-mentioned TC16 titanium alloy rod and wire, in step three, the rolling treatment includes one-fire rolling and two-fire rolling; one-fire rolling: charging the furnace at 800°C, the temperature rises to 820-870°C and starts to keep warm for 90 minutes, and then rolling out of the furnace; two-fire rolling: charging the furnace at 790°C, the temperature rises to 810-860°C and starts to keep warm for 60 minutes, and then rolling out of the furnace.

[0020] In the above-mentioned processing method of TC16 titanium alloy rod and wire, in step eight, in the grinding and polishing process, the single-pass grinding amount is ≤0.15mm; and the surface roughness Ra after polishing is ≤1.6μm.

[0021] In the processing method of the TC16 titanium alloy rod and wire, step six also includes strengthening heat treatment; the strengthening heat treatment temperature is 780°C-830°C, and the heat preservation is carried out for 120 minutes and then water-cooled. When the temperature is below 550°C, it is taken out of the furnace and air-cooled.

[0022] In the processing method of the above-mentioned TC16 titanium alloy rod and wire, in step six, the annealing heat treatment is replaced by double annealing; the double annealing includes a first stage and a second stage; the annealing temperature of the first stage is 700°C to 820°C, and after keeping warm for 120 minutes, air cooling and furnace cooling are performed at 2°C / min to 4°C / min, and when the temperature is below 550°C, the material is taken out of the furnace and air cooled; the annealing temperature of the second stage is 700°C to 820°C, and after keeping warm for 240 minutes, air cooling and furnace cooling are performed.

[0023] The beneficial effects of the present invention are:

[0024] The present invention improves the composition of TC16, further optimizes the forging and rolling process, uses mature titanium alloy cold processing technology, and refines the grains of the rolled semi-finished products by rotary forging, so that the bar structure is close to that of the wire material. At the same time, by modifying the original straightening machine, the high-efficiency straightening of the bar is achieved. At the same time, the straightening method reduces the internal stress of the material and improves the problem of easy cracking of the product during upsetting. It realizes batch production, improves production efficiency, and reduces costs.

[0025] The annealed tensile strength of the TC16 titanium alloy rod and wire prepared by the present invention is about 830MPa, the elongation is more than 20% and the shear strength is more than 690MPa. The high-power rating meets the national military standard GJB 2219A-2015 "Specifications for Titanium and Titanium Alloy Rods and Wires for Fasteners" Figure 1 Class 1 standard requirements. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] Figure 1 It is a schematic diagram of the heating process for forging of TC16 titanium alloy of the present invention;

[0027] Figure 2 This is a schematic diagram of the rolling and heating process of TC16 titanium alloy of the present invention;

[0028] Figure 3 It is a schematic diagram of the TC16 titanium alloy processing process flow of the present invention. DETAILED DESCRIPTION

[0029] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the accompanying drawings. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.

[0030] The element content range of the optimized and improved TC16 titanium alloy designed by the present invention is as shown in Table 3-1, and the chemical composition content conforms to the national standard GB / T 3620.1 "Titanium and Titanium Alloy Grades and Chemical Compositions". The formula adjustment plan is: the content of main elements and impurities is controlled, among which the main element Al is reduced by 6% compared with the upper limit of the standard; the main elements Mo and V are increased by 6% to 10% compared with the lower limit of the standard, and the contents of impurity elements C and N are reduced by 12.5% ​​and 10% respectively compared with the standard. The adjustment of chemical composition is beneficial to ensuring material performance indicators and consistency.

[0031] Table 3-1 TC16 titanium alloy composition comparison table

[0032]

[0033] The present invention optimizes the forging and rolling process by adjusting the chemical composition, adjusting the internal phase composition of the TC16 titanium alloy, improving the plasticity of the material, further refining the internal grains through the cold rotary forging process, and reducing the residual stress inside the material through an electric straightening method, thereby producing a TC16 titanium alloy bar with excellent plasticity index and good cold heading effect.

[0034] refer to Figures 1 to 3 The processing method of TC16 titanium alloy rod and wire of the present invention comprises the following steps:

[0035] Melting→forging→rolling→peeling→rotary forging→heat treatment→electric straightening→grinding and polishing→finished product inspection→warehousing.

[0036] 1) Melting

[0037] The key to alloy smelting is the composition design of alloy elements. According to the new design ratio, vacuum consumable smelting is performed three times to cast the ingot. After peeling and turning, the ingot is obtained.

[0038] 2) Forging:

[0039] The ingot that meets the composition design is ground, and the surface defects are removed before sawing. The key to forging is the heating temperature. In order to solve the problem of large lateral temperature difference and severe air absorption at high temperature caused by the low thermal conductivity of titanium alloy during heating, and considering the characteristic that the thermal conductivity of titanium alloy increases with the increase of temperature, the present invention adopts segmented electric furnace heating. In order to obtain a structure with fully broken α phase at the grain boundary, the principle of selecting the heating temperature should be to ensure that the thermal deformation starts in the β zone and ends in the two-phase zone, that is, the heating temperature should be above Tβ, but not too high. If the temperature is too high, the deformation may end in the β zone, which will cause the α phase at the grain boundary to be unable to be fully broken.

[0040] In summary, the TC16 forging heating process is formulated as follows Figure 1 As shown. The forging process includes one-time forging and two-time forging. For the first-time forging, the furnace is charged at 800℃, preheated for 90min, heated to 1000℃~1100℃ and kept warm for 150min, then forged out of the furnace, and the final forging temperature is above 650℃; for the second-time forging, the furnace is charged at 820℃~900℃, kept warm for 120min, then forged out of the furnace, and the final forging temperature is controlled above 600℃.

[0041] Practice shows that the process of microstructure formation in deformed two-phase alloys can be divided into two almost equivalent stages: microstructure formation under the influence of deformation and microstructure formation as a result of cooling after deformation.

[0042] The microstructure requirements of the final product are: fine grains and good uniformity of organization. In terms of deformation control, deformation greater than ≥70% will cause spheroidization of the lamellar organization and easily lead to uneven organization due to excessive deformation heat; deformation ≤30% will make it difficult to ensure sufficient refinement of the organization. After the billet is thermally deformed, the characteristics of the organization do not change. Considering the effect of later heat treatment, water cooling after forging can retain a large number of crystal defects caused by metal deformation, and these crystal defects will not only become nucleation sites in the subsequent heat treatment process, but also the distortion energy stored in the defects provides activation energy for element diffusion. In this regard, water cooling is used for cooling TC16 after forging.

[0043] The key parameter of the alloy forging is the heating temperature, which is controlled at 100℃ to 200℃ above the phase transformation point. Forging requires three upsetting and three drawing, and water cooling after forging. Since the total deformation rate of TC16 titanium alloy rods is smaller than that of wires, the degree of grain refinement is difficult to reach the level of wires. In order to refine the grains as much as possible, multiple upsetting and drawing are required during the forging process to refine the grains. At the same time, a forging process combining β forging + upper forging in the two-phase zone is used to reasonably adjust the tissue content while refining the grains.

[0044] 3) Rolling

[0045] The key parameter of rolling is the heating temperature. According to the analysis and selection principle of the heating method of the previous forging process, titanium and titanium alloys should be heated in an electric furnace during rolling. Considering the influence of deformation heat, the billet will have a certain temperature rise during rolling, which compensates or increases the temperature of the rolling strip. Therefore, the setting of the starting rolling temperature cannot be too high, which may cause the product to overheat and form a Widmanstätten structure. We choose to heat in the α+β phase region, and the temperature is controlled at 50℃~100℃ below the phase transformation point Tβ.

[0046] refer to Figure 2 The rolling process includes one-fire rolling and two-fire rolling; one-fire rolling: charging the furnace at 800℃, the temperature rises to 820℃-870℃ and starts to keep warm for 90 minutes, and then rolling out of the furnace; two-fire rolling: charging the furnace at 790℃, the temperature rises to 810℃-860℃ and starts to keep warm for 60 minutes, and then rolling out of the furnace.

[0047] The setting of the deformation amount of the rolling test is based on the principle of whether it can realize industrial production. The two-stage rolling deformation process is Φ110mm→Φ60mm in the first stage and Φ60mm→Φ9.5mm in the second stage. During deformation in the two-phase region, the changes in the shape of the α sheets in the grain and the α edges along the grain boundaries are determined by its initial orientation relative to the metal flow direction: the α sheets perpendicular to the metal flow direction are deformed the most, the α sheets parallel to this direction are elongated and flattened, and the α sheets in other directions are bent. As the deformation amount increases, all α sheets try to be distributed in line with the metal flow direction. Usually when the deformation amount exceeds 50%, the α edges of the original β grains are basically the same shape as the α sheets deformed within the grain, and it is difficult to distinguish them. Therefore, in production practice, we can regard the microstructure with clearly visible α edges as a manifestation of insufficient deformation. It is particularly noted that TC16 is K β = 0.8 martensitic high-strength heat-resistant alloy, when deformed in the two-phase region, there is no recrystallization at all deformation degrees

[0048] 4) Peeling:

[0049] The qualified billet after rolling is passed through a centerless lathe to remove surface defects of the billet. Generally, the peeling amount is based on the billet specifications. For Φ7.0~Φ12, the peeling amount is 0.5mm; for Φ13~Φ18, the peeling amount is 1.0mm; for Φ19~Φ24, the peeling amount is 1.5mm; for Φ25 and above, the peeling amount is 2.0mm.

[0050] 5) Rotary forging

[0051] The alloy bar can be processed by cold deformation of about 20%, using a cold rotary forging machine to achieve grain refinement and uniform structure. For example, Φ16 cold rotation → Φ13.5±0.5×L, the designed deformation is 25% to 35%. Cold deformation does not require the same large deformation rate as hot rolling to achieve the same effect of grain refinement.

[0052] 6) Heat treatment

[0053] The key to the heat treatment of this alloy lies in the selection of temperature, cooling method and cooling rate. Here, the performance requirements of TC16 bars for hot upsetting are taken as the target value. Considering the characteristics of the above-mentioned titanium and titanium alloys, the corresponding heat treatment test process is formulated according to the standard GJB3763A-2004 "Heat Treatment of Titanium and Titanium Alloys". Table 3-2 and Table 3-3 are the heat treatment processes of TC16 finished bars.

[0054] Table 3-2TC16 bar annealing process

[0055]

[0056] As can be seen from Table 3-2, this test has developed 4 annealing processes, a total of 2 categories: ordinary annealing, double annealing. The ordinary annealing temperature of the alloy bar is selected in the range of 700℃~820℃, and air cooling and furnace cooling are carried out after the holding time of 120min. When the temperature is below 550℃, it is taken out of the furnace and air cooled. Pay attention to controlling the furnace load. Double annealing, after ordinary annealing in the first stage, also includes the second annealing stage: the annealing temperature is selected in the range of 700℃~820℃, and air cooling and furnace cooling are carried out after the holding time of 240min.

[0057] Table 3-3TC16 bar strengthening heat treatment process

[0058]

[0059]

[0060] It can be seen from Table 3-3 that the strengthening heat treatment temperature of TC16 titanium alloy rod is 780-830℃. After keeping warm for 120 minutes, it is cooled by water. When the temperature is below 500-600℃, it is taken out of the furnace and air-cooled.

[0061] 7) Electrical straightening

[0062] The key to straightening the alloy lies in the design of straightening parameters. By upgrading the original straightening machine, the billet specification range is expanded to bars within Φ20mm, which can be straightened by electric straightening machines. For bars larger than Φ20mm, inclined rollers are used for straightening. The principle of electric straightening is to connect the heated workpiece to the circuit for heating, which is highly efficient. Its biggest advantage is that the workpiece is heated quickly and evenly, which can significantly prevent surface oxidation and grain growth. It is the most reasonable heating method for long products. The temperature control method includes various types of thermometers, and the temperature is adjusted by powering off the power supply by calculating the heating time through formulas.

[0063] The vertical electric contact variable controllable straightening machine device includes a base, a station bracket, a hydraulic device, a current controller, upper and lower clamps and other mechanisms. It is more suitable for bar straightening. The heating time of electric contact tension straightening is based on the surface temperature of the billet. It can be tested by high magnification and stretching, and it fully meets the standard requirements. The conventional heating inclined roller straightening and vertical electric contact variable controllable straightening machine are used to replace the previous electric straightening machine, expanding the straightening specification range while improving production efficiency.

[0064] 8) Grinding and polishing

[0065] The special characteristics of TC16 titanium alloy place high demands on equipment and great difficulty. The grinding wheel of the grinding machine is selected as a medium-soft grinding wheel. The fine grinding control retains a polishing allowance of 0.01mm to ensure that there is no obvious spiral pattern on the surface of the rod and wire. Finally, it is processed into finished rods and wires of Φ4.0-Φ20.

[0066] This embodiment selects three different TC16 titanium alloy compositions for illustration, see Table 3-4 for details.

[0067] Table 3-4 TC16 titanium alloy finished product composition specifications of the present invention

[0068]

[0069]

[0070] 1) Select the ingot with new composition, forging in the first fire: load the furnace at 800℃, preheat for 90min, heat up to 1000℃~1100℃ and keep warm for 150min, forge out of the furnace, upsetting from Φ275mm to Φ230mm, water cooling after forging, and the final forging temperature is controlled above 650℃. Forging in the second fire: load the furnace at 820℃~900℃, keep warm for 120min, forge out of the furnace, upsetting from Φ230 to Φ110, water cooling after forging, and the final forging temperature is controlled above 600℃;

[0071] 2) Rolling: First-fire rolling: Load the furnace at 800℃, and keep the temperature at 820-870℃ for 90min. Roll out of the furnace and roll from □110mm to Φ60mm mill bar through 13 passes. Grind to ensure there are no defects. Second-fire rolling: Load the furnace at 790℃, and keep the temperature at 810-860℃ for 60min. Roll out of the furnace and roll from Φ60mm to Φ12mm mill bar. Grind to ensure there are no defects.

[0072] 3) Cold rotary forging: The billet that has been rolled to Φ12mm is forged into a round shape to Φ11mm using a rotary forging machine.

[0073] 4) Stripping: The blank forged to Φ11mm is processed by a centerless lathe from Φ11mm×L→Φ10.0±0.1×L(mm)

[0074] 5) Annealing: The billet peeled to Φ10.0mm is subjected to 700-820℃ / 120min, furnace cooled to 550℃, and air cooled.

[0075] 6) Electric straightening: Use heated inclined roller straightening and vertical electric contact variable controllable straightening machine to straighten the blank, and the straightness meets 3mm / m.

[0076] 7) Grinding: The grinding amount per pass is not more than 0.15 mm. The straightened blank is ground to 9.51 mm, and the grinding pass is 2-3 times.

[0077] 8) Polishing The blank that has been ground to a near-finished product is polished, with a surface roughness of Ra ≤ 1.6 μm.

[0078] 9) Physical and chemical performance inspection of finished products: Select any 10 blanks from the blanks that have passed the appearance and size inspection, and cut a 300+10mm physical and chemical part from each blank, for a total of 10 parts / 5 sets; mark the brand and ingot number on each physical and chemical part.

[0079] Choose 4 out of 5 sets of physical and chemical parts for annealing:

[0080] ①700-820℃±10℃, 2h, furnace cool to 550℃ at 2~4℃ / min, air cool.

[0081] ②700-820℃±10℃, 2h, AC+600℃~700℃±10℃, 4h, AC;

[0082] Another set undergoes an enhanced heat treatment process;

[0083] Solution treatment: 800℃-850℃±10℃, 2h, water cooling;

[0084] Aging: 510℃-580℃±10℃, 6h~10h, air cooling.

[0085] Perform room temperature tensile, high magnification, shear and other performance tests respectively.

[0086] 10) The performance test results are shown in Table 3-5:

[0087] Table 3-5 Statistical table of test results of physical and chemical properties of finished products

[0088]

[0089] The present invention reduces the alloy smelting cost under the premise of ensuring the performance by using raw materials with adjusted chemical composition. At the same time, the forging and rolling selects reasonable temperature and deformation rate to make the blank structure more refined. Cold rotary forging further refines the alloy structure and reduces the difference between the rod structure and the wire structure. Electric straightening solves the problem of residual stress after straightening of Φ4.0mm~Φ20mm rod products. The precise grinding and polishing control method eliminates the quality problem of spiral lines on the surface of the current TC16 rod. The room temperature mechanical properties of the TC16 titanium alloy rods with specifications of Φ7.5 and Φ9.5 of the present invention are shown in Table 3-6.

[0090] Table 3-6 Room temperature mechanical properties of TC16 titanium alloy bars of the present invention with specifications of Φ7.5 and Φ9.5

[0091]

[0092] The annealed tensile strength of the TC16 titanium alloy rod and wire prepared by the present invention is about 830MPa, the elongation is more than 20% and the shear strength is more than 690MPa. The high-power rating meets the national military standard GJB 2219A-2015 "Specifications for Titanium and Titanium Alloy Rods and Wires for Fasteners" Figure 1 The surface roughness of the rod prepared by the present invention is ≤1.6μm, the straightness is ≤1.0mm / m, the dimensional deviation is -0.02mm, 0.

[0093] The present invention optimizes the chemical composition, improves the forging process, and adopts cold rotary forging, electric straightening and other technologies to fully refine the microstructure of the TC16 titanium alloy bar, effectively control the content of α and β structures, effectively improve the plasticity index of the TC16 titanium alloy bar, and effectively control the residual stress of the TC16 bar through processes such as electric straightening, avoiding the problem of cracking during cold heading of the material. The solution has a good foundation for industrial application, has been put into large-scale production and has been verified by customers to achieve good results.

[0094] What is described above is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.

Claims

1. A TC16 titanium alloy rod and wire, characterized in that: The chemical composition of the TC16 titanium alloy rod and wire is calculated by mass fraction, and the main components include: 2.4 to 3.6 Al, 4.5 to 5.3 Mo, 4.0 to 5.0 V; impurities include not more than 0.035 Fe, not more than 0.05 C, not more than 0.1 Zr, not more than 0.1 N, and not more than 0.012 O; the single content of other impurities is not more than 0.1, and the total content is not more than 0.4; the balance is Ti.

2. The TC16 titanium alloy rod and wire according to claim 1, characterized in that: The TC16 titanium alloy rod and wire have an annealed tensile strength of more than 830 MPa, an elongation of more than 20%, and a shear strength of more than 690 MPa.

3. A method for processing TC16 titanium alloy rod and wire, characterized in that: The TC16 titanium alloy composition according to any one of claims 1 to 2 is used, comprising the following steps: Step 1: After the TC16 titanium alloy components are subjected to three vacuum consumable melting processes to form an ingot, the ingot is peeled and turned to obtain an ingot; Step 2: Forging treatment: The forging temperature is 100℃~200℃ above the phase change point. The forging requires three upsetting and three drawing, and the combination of β forging + two-phase zone upper forging is adopted; water cooling after forging; Step 3: Rolling treatment: Use an electric furnace to heat in the α+β phase region, and the heating temperature is the phase transition point T β Below 50℃~100℃; Step 4: Use a centerless lathe to remove surface defects of the blank by peeling; For blanks with specifications of Φ4.0 to Φ12, the peeling amount is 0.5mm; for blanks with specifications of Φ13 to Φ18, the peeling amount is 1.0mm; for blanks with specifications of Φ19 to Φ24, the peeling amount is 1.5mm; for blanks with specifications of Φ25 or above, the peeling amount is 2.0mm; Step 5: Use a cold rotary forging machine to perform 20%-50% cold deformation rotary forging processing; Step 6: Annealing heat treatment: The annealing temperature is 700℃~820℃, and after keeping warm for 120min, air-cooling and furnace-cooling are performed at 2℃ / min~4℃ / min. When the temperature is below 550℃, the steel is taken out of the furnace and air-cooled. Step 7: Use a vertical electric contact variable controllable straightening machine for straightening, and the straightness meets 3mm / m; Step 8: Use medium-soft grinding wheel for grinding and polishing; polishing allowance 0.01mm; finally process into finished rods and wires of Φ4.0~Φ20.

4. The method for processing TC16 titanium alloy rod and wire according to claim 3, characterized in that: In step 2, the forging process includes one-time forging and two-time forging; the first-time forging is to load the furnace at 800°C, preheat for 90 minutes, heat to 1000°C-1100°C and keep warm for 150 minutes, forge out of the furnace, and the final forging temperature is above 650°C; the second-time forging is to load the furnace at 820°C-900°C, keep warm for 120 minutes, forge out of the furnace, and the final forging temperature is controlled above 600°C.

5. The method for processing TC16 titanium alloy rod and wire according to claim 3, characterized in that: In step three, the rolling treatment includes one-fire rolling and two-fire rolling; one-fire rolling: charging the furnace at 800°C, the temperature rises to 820°C-870°C and starts to keep warm for 90 minutes, and then rolling out of the furnace; two-fire rolling: charging the furnace at 790°C, the temperature rises to 810°C-860°C and starts to keep warm for 60 minutes, and then rolling out of the furnace.

6. The method for processing TC16 titanium alloy rod and wire according to claim 3, characterized in that: In step eight, during the grinding and polishing process, the grinding amount per pass is ≤0.15 mm; and the surface roughness Ra after polishing is ≤1.6 μm.

7. The method for processing TC16 titanium alloy rod and wire according to claim 3, characterized in that: Step six also includes enhanced heat treatment; the enhanced heat treatment temperature is 780°C-830°C, and the heat preservation is carried out for 90min-150min, followed by water cooling, and the aging temperature is 500°C-580°C / 4h-10h, and air cooling.

8. The method for processing TC16 titanium alloy rod and wire according to claim 3, characterized in that: In step six, the annealing heat treatment is replaced by double annealing; the double annealing includes a first stage and a second stage; the annealing temperature of the first stage is 700°C to 820°C, and after keeping the temperature for 120 minutes, the furnace is air-cooled at 2 to 4°C / min, and when the temperature is below 550°C, the furnace is taken out of the furnace and air-cooled; The second stage annealing temperature is 700℃~820℃, and after keeping warm for 240min, it is air-cooled and furnace-cooled.

Citation Information

Patent Citations

  • Preparation method and application of heat-resistant titanium alloy wires

    CN109355530A

  • Processing method of fine-grain superplastic TA15 titanium alloy medium-thickness plate

    CN111763850A

  • Processing method of TC16 titanium alloy bar for cold heading

    CN117187723A

  • Thermomechanical processing of alpha-beta titanium alloys

    US20140261922A1

  • Method of straightening wire rods of titanium and titanium alloy

    US6077369A

Cited By

  • Conductive corrosion-resistant titanium alloy product for battery system and preparation method thereof

    CN121852768A

  • Preparation method of Nb47Ti bar with uniform fine grains and small specification

    CN122517406A