Preparation method of high-strength and high-toughness wrought magnesium alloy

By regulating the composition and process of Mg-Al-Zn-based magnesium alloy, combined with hot extrusion and heat treatment, the problem of degradation of magnesium alloy at high temperatures is solved, and a deformed magnesium alloy with high strength and high toughness is achieved, suitable for high-performance products need.

CN119020648APending Publication Date: 2024-11-26WENXI COUNTY REGAL MAGNESIUM
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411135984.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-19
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

The β-Mg17Al12 phase in Mg-Al-Zn-based magnesium alloy is prone to soften and coarse at higher temperatures, which cannot effectively hinder dislocation slip, resulting in insufficient mechanical properties of room temperature and high temperature.

Method used

By regulating the alloy composition, combining hot extrusion and heat treatment processes, rare earth elements and Ca are added to refine grains, hinder dislocation movement, and homogenize and heat treatment to improve the mechanical properties of the alloy.

Benefits of technology

It has achieved a high-strength and high-toughness deformed magnesium alloy, with tensile strength of 288MPa, an elongation of 13%, and a simple process and low cost, which is suitable for industrial production.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention discloses a preparation method of a high-strength and high-toughness wrought magnesium alloy, and belongs to the technical field of alloy material preparation. The high-strength and high-toughness wrought magnesium alloy comprises the following components in percentage by mass: 5.8-6.2% of Al, 0.8-1.0% of Zn, 0.2-0.3% of Mn, 0.4-0.6% of La / Ce, 0-0.3% of Ca, less than or equal to 2% of other elements, less than or equal to 0.05% of impurity elements and the balance of Mg, the other elements comprise one or more of Si, Sn and Sb. The high-strength and high-toughness wrought magnesium alloy has excellent comprehensive mechanical properties, the tensile strength of the wrought magnesium alloy can reach 288MPa, and the ductility of the wrought magnesium alloy can reach 13%.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of alloy material preparation, and in particular to a method for preparing a high-strength and high-toughness deformable magnesium alloy. Background Art

[0002] Magnesium and its alloys have the advantages of low density, high specific strength, high specific stiffness and good casting properties. Compared with the common non-ferrous metal material aluminum alloy, they are also less prone to thermal fatigue. Therefore, the service life of magnesium alloy die castings is longer than that of aluminum alloys.

[0003] Mg-Al-Zn magnesium alloy (AZ series) is the most commonly used wrought magnesium alloy, which has excellent comprehensive mechanical properties, corrosion resistance and other advantages. However, the main strengthening phase β-Mg in AZ series alloy 17 Al 12 It tends to soften and coarsen at higher temperatures, and cannot play the role of pinning grain boundaries and hindering dislocation slip. Therefore, it needs to be optimized to further improve its mechanical properties at room temperature and higher temperatures. Summary of the invention

[0004] The purpose of the present invention is to provide a method for preparing a high-strength and high-toughness deformable magnesium alloy to solve the problems existing in the above-mentioned prior art. The present invention further improves the comprehensive mechanical properties of the Mg-Al-Zn magnesium alloy by regulating the alloy composition and combining hot extrusion (hot deformation) and heat treatment processes, so that the alloy has both good strength and toughness, providing material reserves for products with higher performance requirements.

[0005] To achieve the above object, the present invention provides the following solutions:

[0006] One of the technical solutions of the present invention: a high-strength and high-toughness deformable magnesium alloy, comprising the following components by mass percentage: Al 5.8-6.2%, Zn 0.8-1.0%, Mn 0.2-0.3%, La / Ce 0.4-0.6%, Ca0-0.3%, other elements ≤2%, impurity elements ≤0.05%, and the balance is Mg;

[0007] The other elements include one or more of Si, Sn, and Sb; the impurity elements include one or more of Fe, Cu, and Ni;

[0008] The La / Ce, in terms of mass percentage, includes the following components: 55% Ce, 25% La, 15-18% Nd, and the remainder is other rare earth metals.

[0009] The addition of rare earth elements and Ca elements can refine the grains and achieve grain refinement by hindering the movement of dislocations at grain boundaries.

[0010] Technical solution 2 of the present invention: A method for preparing the above-mentioned high-strength and high-toughness deformable magnesium alloy comprises the following steps:

[0011] The component raw materials are mixed, melted and cast to obtain alloy cast rods;

[0012] The alloy casting rod is subjected to homogenization treatment and hot extrusion in sequence to obtain the high-strength and high-toughness deformable magnesium alloy.

[0013] Furthermore, the smelting temperature is 715-733°C.

[0014] Furthermore, the casting conditions include: semi-continuous casting, a casting temperature of 705-715°C, a cooling water flow rate of 30m 3 / h, the casting speed is 120mm / min, and a 105mm diverter is used for drainage.

[0015] Furthermore, the temperature of the homogenization treatment is 410-420° C., and the insulation time is 10 hours.

[0016] Furthermore, the extrusion ratio of the hot extrusion is 35:1, the extrusion temperature is 380-400° C., and the extrusion speed is 0.3 mm / s.

[0017] Furthermore, a heat treatment step is also included after hot extrusion; the heat treatment can improve the concentrated distribution of the second phase in the alloy, especially the Al-Mn phase, and avoid the problem of stress concentration during deformation caused by the uneven distribution of the second phase.

[0018] The heat treatment includes solution heat treatment and / or aging heat treatment.

[0019] Furthermore, the temperature of the solution heat treatment is 350-420°C, and the time is 2 hours; the temperature of the aging heat treatment is 180-200°C, and the time is 24 hours.

[0020] Furthermore, the temperature of the solution heat treatment is 400°C and the time is 2h; the temperature of the aging heat treatment is 180°C and the time is 24h.

[0021] The present invention discloses the following technical effects:

[0022] The high-strength and high-toughness deformable magnesium alloy of the present invention has excellent comprehensive mechanical properties, and its tensile strength can reach 288MPa and its elongation can reach 13%.

[0023] The present invention further improves the comprehensive mechanical properties of Mg-Al-Zn magnesium alloy by regulating alloy composition and combining hot extrusion (hot deformation) and heat treatment processes, so that the alloy has both good strength and toughness. In addition, the method of the present invention has simple process, low cost, high production efficiency, and can realize industrial production, laying a foundation for practical production applications. DETAILED DESCRIPTION

[0024] Various exemplary embodiments of the present invention will now be described in detail. This detailed description should not be considered as limiting the present invention, but should be understood as a more detailed description of certain aspects, features, and embodiments of the present invention.

[0025] It should be understood that the terms described in the present invention are only for describing special embodiments and are not intended to limit the present invention. In addition, for the numerical range in the present invention, it should be understood that each intermediate value between the upper and lower limits of the scope is also specifically disclosed. Each smaller range between the intermediate value in any stated value or stated range and any other stated value or intermediate value in the described range is also included in the present invention. The upper and lower limits of these smaller ranges can be independently included or excluded in the scope.

[0026] Unless otherwise indicated, all technical and scientific terms used herein have the same meanings as those generally understood by those skilled in the art. Although the present invention describes only preferred methods and materials, any methods and materials similar or equivalent to those described herein may also be used in the implementation or testing of the present invention. All documents mentioned in this specification are incorporated by reference to disclose and describe the methods and / or materials associated with the documents. In the event of a conflict with any incorporated document, the content of this specification shall prevail.

[0027] It will be apparent to those skilled in the art that various modifications and variations may be made to the specific embodiments of the present invention description without departing from the scope or spirit of the present invention. Other embodiments derived from the present invention description will be apparent to the skilled artisan. The present invention description and examples are exemplary only.

[0028] The words “include,” “including,” “have,” “contain,” etc. used in this document are open-ended terms, meaning including but not limited to.

[0029] Example 1

[0030] A method for preparing a high-strength and high-toughness deformed magnesium alloy:

[0031] The high-strength and high-toughness wrought magnesium alloy is composed of the following components, by mass percentage: Al 6.04%, Zn 0.92%, Mn 0.26%, La / Ce 0.54%, Si 0.062%, Sn 0.073%, Sb 0.012%, Fe 0.0023%, Cu 0.0024%, Ni 0.0001%, and the balance is Mg.

[0032] Among them, La / Ce, in terms of mass percentage, consists of the following components: Ce 55%, La 25%, Nd 18%, Y 1.2%, and Sm 0.8%.

[0033] (1) Melting:

[0034] a. Magnesium melting: firstly dry pure magnesium (99.99%) and then melt it in a smelting furnace, and introduce Ar2 for protection during the melting process;

[0035] b. After the pure magnesium is completely melted, the temperature is raised to 720°C, and a mixture of preheated (preheating temperature is 270-280°C) pure Al (99.99%), pure Zn (99.99%), MnCl2 (containing 40wt.%) and RJ-5 flux (the amount of RJ-5 flux used is the same as the mass of MnCl2) is added;

[0036] c. After the alloy in the previous step is fully melted, when the temperature rises to 730°C, La / Ce rare earth is added;

[0037] d. Refining: After the alloy is fully melted, when the temperature drops to 720°C, add RJ-5 flux (the amount of RJ-5 flux is 2% of the total mass of the deformed magnesium alloy raw material), stir with argon, and then stand for 20 minutes (temperature is 720°C) to obtain alloy liquid;

[0038] e. Casting: The alloy liquid is cast to obtain alloy cast rods. The casting conditions are: semi-continuous casting, casting temperature is 710℃, cooling water flow rate is 30m 3 / h, the casting speed is 120mm / min, and a 105mm diverter is used for drainage.

[0039] (2) Hot extrusion process:

[0040] a. Homogenization treatment: The alloy casting rod is homogenized at a temperature of about 410-420°C for 10 hours, and then water-cooled to obtain a homogenized casting rod;

[0041] b. Hot extrusion: The homogeneous cast rod is hot extruded with an extrusion ratio of 35:1, an extrusion temperature of 386°C, and an extrusion speed of 0.3 mm / s to obtain a high-strength and high-toughness deformed magnesium alloy.

[0042] The room temperature mechanical properties of the high-strength and high-toughness wrought magnesium alloy prepared in this embodiment are as follows: tensile strength is 276.54 MPa, yield strength is 166.35 MPa, and elongation is 14.05%.

[0043] Example 2

[0044] The same as Example 1, except that the high-strength and high-toughness wrought magnesium alloy is composed of the following components, by mass percentage: Al 6.04%, Zn 0.92%, Mn 0.26%, La / Ce 0.54%, Ca 0.23%, Si0.062%, Sn 0.073%, Sb 0.012%, Fe 0.0023%, Cu 0.0024%, Ni 0.0001%, and the balance is Mg.

[0045] The room temperature mechanical properties of the high-strength and high-toughness wrought magnesium alloy prepared in this embodiment are as follows: tensile strength is 285.06 MPa, yield strength is 168.33 MPa, and elongation is 9.73%.

[0046] Example 3

[0047] The same as Example 1, the only difference is that the alloy obtained after hot extrusion is heat treated. The process is as follows: the alloy obtained after hot extrusion is subjected to solution heat treatment. The temperature of the solution heat treatment is 400° C. and the holding time is 2 h to obtain a high-strength and high-toughness deformable magnesium alloy.

[0048] The room temperature mechanical properties of the high-strength and high-toughness wrought magnesium alloy prepared in this embodiment are as follows: tensile strength is 277.52 MPa, yield strength is 170.85 MPa, and elongation is 12.26%.

[0049] Example 4

[0050] The same as Example 1, the only difference is that the alloy obtained after hot extrusion is heat treated. Process: the alloy obtained after hot extrusion is subjected to aging heat treatment, the aging heat treatment temperature is 180°C, the holding time is 24h, and a high-strength and high-toughness deformable magnesium alloy is obtained.

[0051] The room temperature mechanical properties of the high-strength and high-toughness wrought magnesium alloy prepared in this embodiment are as follows: tensile strength is 286.27 MPa, yield strength is 171.43 MPa, and elongation is 11.68%.

[0052] Example 5

[0053] The same as Example 1, the only difference is that the alloy obtained after hot extrusion is heat treated, the process: the alloy obtained after hot extrusion is subjected to solid solution aging heat treatment, the solid solution heat treatment temperature is 400°C, the holding time is 2h, the aging heat treatment temperature is 180°C, the holding time is 24h, to obtain a high-strength and high-toughness deformable magnesium alloy.

[0054] The room temperature mechanical properties of the high-strength and high-toughness wrought magnesium alloy prepared in this embodiment are as follows: tensile strength is 288.53 MPa, yield strength is 173.25 MPa, and elongation is 13.06%.

[0055] Comparative Example 1

[0056] Same as Example 1, except that La / Ce is replaced with Y of equal mass.

[0057] The room temperature mechanical properties of the alloy prepared in this comparative example are as follows: tensile strength is 263.6 MPa, yield strength is 172 MPa, and elongation is 9.74%.

[0058] The price of the La / Ce rare earth used in the embodiment of the present invention is much lower than that of the rare earth Y element. When the mechanical properties are not much different, the cost performance is greatly improved.

[0059] Comparative Example 2

[0060] Same as Example 5, except that the temperature of the solution heat treatment is 350° C., and the holding time is 2 h; the temperature of the aging heat treatment is 180° C., and the holding time is 24 h.

[0061] The room temperature mechanical properties of the alloy prepared in this comparative example are as follows: tensile strength is 243.6 Mpa, yield strength is 166.a Mpa, and elongation is 8.73%.

[0062] The embodiments described above are only descriptions of the preferred modes of the present invention, and are not intended to limit the scope of the present invention. Without departing from the design spirit of the present invention, various modifications and improvements made to the technical solutions of the present invention by ordinary technicians in this field should all fall within the protection scope determined by the claims of the present invention.

Claims

1. A high-strength and high-toughness deformable magnesium alloy, characterized in that: The composition includes the following components by mass percentage: Al 5.8-6.2%, Zn 0.8-1.0%, Mn 0.2-0.3%, La / Ce 0.4-0.6%, Ca 0-0.3%, other elements ≤2%, impurity elements ≤0.05%, and the balance is Mg; The other elements include one or more of Si, Sn, and Sb; The La / Ce, in terms of mass percentage, includes the following components: 55% Ce, 25% La, 15-18% Nd, and the remainder is other rare earth metals.

2. A method for preparing a high-strength and high-toughness deformable magnesium alloy according to claim 1, characterized in that: The following steps are involved: The component raw materials are mixed, melted and cast to obtain alloy cast rods; The alloy casting rod is subjected to homogenization treatment and hot extrusion in sequence to obtain the high-strength and high-toughness deformable magnesium alloy.

3. The preparation method according to claim 2, characterized in that: The casting conditions include: casting temperature of 705-715°C, cooling water flow rate of 30m 3 / h, the casting speed is 120mm / min.

4. The preparation method according to claim 2, characterized in that: The temperature of the homogenization treatment is 410-420° C., and the insulation time is 10 hours.

5. The preparation method according to claim 2, characterized in that: The extrusion ratio of the hot extrusion is 35:1, and the extrusion temperature is 380-400°C.

6. The preparation method according to claim 2, characterized in that: A heat treatment step is also included after hot extrusion; The heat treatment includes solution heat treatment and / or aging heat treatment.