Novel high-entropy alloy material and preparation method thereof

By adjusting the molar ratio and process of high-entropy alloys, a new high-entropy alloy material with excellent comprehensive performance was prepared, which solved the problem of insufficient performance of traditional high-entropy alloys, and achieved high hardness, compressive strength, ductility and oxidation resistance. Improvement.

CN119020658APending Publication Date: 2024-11-26KUNMING UNIV OF SCI & TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411149603.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-21
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

The comprehensive use performance of traditional high-entropy alloy materials is limited and it is difficult to meet the growing industrial needs. A new high-entropy alloy material is needed to expand its application range.

Method used

By adjusting the molar ratio of AlCoCrFeNiZr high-entropy alloy, increasing the Fe and Ni content, adding an appropriate amount of Zr to suppress the formation of Laves phase, vacuum arc smelting and copper-absorbing rapid molding process were used to prepare high hardness, compressive strength and ductility. and oxidation resistance new high entropy alloy materials.

Benefits of technology

It significantly improves the microstructure stability of the alloy, reduces the brittle phase generation, and improves the comprehensive use performance of the alloy, especially the oxidation resistance and mechanical properties in high temperature environments.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119020658A_ABST
    Figure CN119020658A_ABST
Patent Text Reader

Abstract

The invention discloses a novel high-entropy alloy material and a preparation method thereof, and belongs to the field of metal materials. The high-entropy alloy material comprises a high-entropy alloy with the molar ratio of Al: Co: Cr: Fe: Ni: Zr being 3.3: 3.3: 3.3: 5: 5: 0.1, the high-entropy alloy material is prepared through raw material pretreatment, vacuum arc melting and alloy suction casting, and the high-entropy alloy with excellent comprehensive performance is obtained by controlling the content of alloy elements, so that the application range of the high-entropy alloy is widened.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of metal materials and relates to a new type of high entropy alloy material and a preparation method thereof. Background Art

[0002] With the acceleration of global industrialization, higher requirements are placed on the performance of alloy materials. Due to the limited performance of traditional alloy materials, it is difficult to meet the growing industrial needs.

[0003] The emergence of high entropy alloys has broken through the traditional alloy design concept and provided favorable support for industrial development. High entropy alloys, referred to as HEA, are alloys formed by five or more equal or approximately equal amounts of metals. Although high entropy alloys currently have certain advantages over traditional alloy materials, their comprehensive performance still has room for improvement. With the improvement of the comprehensive performance of high entropy alloy materials, they can meet a wider range of application scenarios. Therefore, it is of great significance to improve the comprehensive use of high entropy alloy materials.

[0004] Therefore, it is necessary to provide a new type of high entropy alloy material and a preparation method thereof, so as to obtain a high entropy alloy material with excellent comprehensive performance by preparing a new type of high entropy alloy material that is essentially different from traditional high entropy alloys, so as to further expand the application scope of high entropy alloy materials. Summary of the invention

[0005] In order to overcome the problems in the background technology, the present invention breaks through the traditional idea that high entropy alloys are composed of equal or approximately equal amounts of metals, and prepares a new type of high entropy alloy. The prepared high entropy alloy has high hardness, compressive strength, ductility, toughness and oxidation resistance, and the comprehensive performance of the alloy is relatively excellent.

[0006] In order to achieve the above object, the present invention is implemented by the following technical solutions:

[0007] On the one hand, the present invention proposes a new type of high entropy alloy material, the chemical expression of the high entropy alloy material is AlCoCrFeNiZr, wherein the molar ratio of Al, Co, Cr, Fe, Ni and Zr is Al:Co:Cr:Fe:Ni:Zr=3.3:3.3:3.3:5:5:0.1.

[0008] Preferably, the high entropy alloy material consists of FCC and BCC phases.

[0009] Another aspect of the present invention provides a method for preparing the novel high entropy alloy material, the preparation method comprising the following steps:

[0010] (1) Raw material pretreatment: grinding the raw metals Al, Co, Cr, Fe, Ni, and Zr with a grinding wheel and polishing with sandpaper in turn, then ultrasonically cleaning the raw metals with ethanol, and then drying the raw metals for later use;

[0011] (2) Vacuum arc melting: weighing the raw material metals pretreated in step (1) according to the molar ratio of the alloy components, placing the raw material metals in the order of Al, Ni, Co, Fe, Zr, and Cr from bottom to top into the crucible sub-tank of the vacuum arc furnace, then evacuating the vacuum arc furnace, and then filling the vacuum arc furnace with protective gas to normal pressure to melt the raw material metals;

[0012] (3) Alloy suction casting: The molten alloy liquid after smelting in the step (2) is sucked into a copper mold and cooled to form a high entropy alloy material.

[0013] Preferably, the raw metal purity is not less than 99.99%.

[0014] Preferably, in step (2), the smelting current intensity is 180-220A, and during the smelting process, the smelting is turned over once every 2-5 minutes, and the turning is repeated 6-7 times.

[0015] Preferably, in step (2), the protective gas is argon.

[0016] Preferably, in step (2), the vacuum is evacuated to 5×10 -3 Pa.

[0017] Beneficial effects of the present invention:

[0018] 1. The present invention increases the Fe and Ni contents in the alloy, and when the Fe and Ni contents are greater than the Al, Co, Zr, and Cr contents, thereby breaking through the limitations of traditional high entropy alloys, improving the stability of the alloy microstructure, reducing the generation of brittle phases, and improving the comprehensive performance of the alloy.

[0019] 2. The present invention achieves the purpose of improving the hardness of the alloy by adding a proper amount of Zr while suppressing the formation of Laves phase in the alloy and reducing the generation of brittle phase of the alloy. Thus, the hardness of the alloy is improved while reducing the brittleness of the alloy, so that the alloy has excellent comprehensive performance.

[0020] 3. The alloy prepared by the present invention not only has high hardness, toughness and ductility, but also has high compressive strength and oxidation resistance.

[0021] 4. By adopting a specific composition combination with high Fe, Ni content and moderate Zr content, the suction casting process significantly improves the compressive strength and toughness of the alloy during rapid prototyping. Compared with other composition combinations, the synergy of this process and specific components effectively improves microstructure control, and improves the high-temperature oxidation resistance and comprehensive mechanical properties of the alloy. Through rapid cooling and the high thermal conductivity of the copper mold, excessive grain boundary growth and brittle phase precipitation are suppressed, the alloy grains are refined, and the structure is uniform and stable. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 This is a picture of the alloy product prepared in Example 1 of the present invention;

[0023] Figure 2 The XRD diagram of the alloys prepared in Example 1 and the comparative example of the present invention;

[0024] Figure 3 The SEM images of the alloys prepared in Example 1 and the comparative example of the present invention are shown in FIG.

[0025] Figure 4 The Vickers hardness diagram of the alloys prepared in Example 1 of the present invention and the comparative example;

[0026] Figure 5 Compression diagrams of alloys prepared in Example 1 of the present invention and the comparative example;

[0027] Figure 6 The thermogravimetric curves of the alloys prepared in Example 1 and the comparative example of the present invention. DETAILED DESCRIPTION

[0028] The present invention is further described in detail below in conjunction with specific embodiments.

[0029] Example 1

[0030] In this embodiment, a high entropy alloy is prepared by the following method:

[0031] (1) The raw metals Al, Co, Cr, Fe, Ni, and Zr are sequentially ground with a grinding wheel and polished with sandpaper, and then the raw metals are ultrasonically cleaned with ethanol, and then the raw metals are dried.

[0032] (2) Raw metals with a molar ratio of Al:Co:Cr:Fe:Ni:Zr=3.3:3.3:3.3:5:5:0.1 were weighed and placed in the crucible sub-tank of a vacuum arc furnace in the order of Al, Ni, Co, Fe, Zr, and Cr from bottom to top. Meanwhile, a titanium sponge block was placed in the crucible main tank of the vacuum arc furnace. The furnace was evacuated to 5×10 -3Pa, and then filled with argon gas with a purity of 99.99% to normal pressure. First, the sponge titanium block was arc-melted for 3 minutes at a current intensity of 70A to absorb the residual oxygen in the furnace chamber and further reduce the oxidation behavior during the smelting process. Then, the raw metal was melted at a current intensity of 210A, and the melting was flipped every 3 minutes, and the flipping was repeated 7 times to ensure the uniformity of the alloy composition.

[0033] (3) The molten alloy obtained after the above smelting is sucked into a copper mold and cooled to form a rod-shaped sample. The alloy sample prepared in this embodiment is as follows: Figure 1 shown.

[0034] The alloy samples prepared in this example were subjected to XRD experiments, and the results are as follows: Figure 2 The alloy samples prepared in this example were subjected to SEM experiments, and the results were as follows: Figure 3 The alloy samples prepared in this embodiment were subjected to Vickers hardness test, and the results are shown in Figure 4 As shown; the compressive strength test of the alloy sample prepared in this embodiment is carried out, and the results are as follows Figure 5 Thermogravimetric analysis of the alloy samples prepared in this embodiment was performed, and the results are shown in Figure 6 shown.

[0035] Example 2

[0036] This embodiment adopts the same method as that of embodiment 1 to prepare alloy samples, except that: the current intensity during the smelting process of this embodiment is 180A, the smelting is turned over once every 5 minutes, and the turning over is repeated 7 times.

[0037] The performance of the alloy sample prepared in this example is similar to that of Example 1.

[0038] Example 3

[0039] This embodiment adopts the same method as that of embodiment 1 to prepare the alloy sample, except that: the current intensity during the smelting process of this embodiment is 220A, the smelting is turned over once every 2 minutes, and the turning over is repeated 6 times.

[0040] The performance of the alloy sample prepared in this example is similar to that of Example 1.

[0041] Comparative Example 1

[0042] The alloy sample was prepared in the same manner as in Example 1, except that the molar ratio of the alloy components in this comparative example was Al:Co:Cr:Fe:Ni=3.3:3.3:3.3:5:5

[0043] The alloy samples prepared in this comparative example were subjected to XRD experiments, and the results are as follows: Figure 2The alloy samples prepared in this comparative example were subjected to SEM experiments, and the results were as follows Figure 3 The alloy samples prepared in this comparative example were subjected to Vickers hardness test, and the results were as follows Figure 4 As shown; the compressive strength test of the alloy sample prepared in this comparative example was carried out, and the results are as follows Figure 5 Thermogravimetric analysis of the alloy samples prepared in this comparative example was performed, and the results are shown in Figure 6 shown.

[0044] Comparative Example 2

[0045] In this comparative example, an alloy sample is prepared by the same method as in Example 1, except that the molar ratio of the alloy components in this comparative example is Al:Co:Cr:Fe:Ni:Zr=4:4:4:4:4:0.1.

[0046] Comparative Example 3

[0047] The alloy sample of this comparative example is prepared by the same method as that of Example 1, except that the molar ratio of the alloy components in this comparative example is Al:Co:Cr:Fe:Ni:Zr=3.3:3.3:3.3:5:5:0.2.

[0048] The alloy samples prepared in this comparative example were subjected to XRD experiments, and the results are as follows: Figure 2 The alloy samples prepared in this comparative example were subjected to SEM experiments, and the results were as follows Figure 3 The alloy samples prepared in this comparative example were subjected to Vickers hardness test, and the results were as follows Figure 4 As shown; the compressive strength test of the alloy sample prepared in this comparative example was carried out, and the results are as follows Figure 5 Thermogravimetric analysis of the alloy samples prepared in this comparative example was performed, and the results are shown in Figure 6 shown.

[0049] Comparative Example 4

[0050] The alloy sample of this comparative example is prepared by the same method as that of Example 1, except that the molar ratio of the alloy components in this comparative example is Al:Co:Cr:Fe:Ni:Zr=3.3:3.3:3.3:5:5:0.4.

[0051] The alloy samples prepared in this comparative example were subjected to XRD experiments, and the results are as follows: Figure 2 The alloy samples prepared in this comparative example were subjected to SEM experiments, and the results were as follows Figure 3 The alloy samples prepared in this comparative example were subjected to Vickers hardness test, and the results were as follows Figure 4 As shown; the compressive strength test of the alloy sample prepared in this comparative example was carried out, and the results are as follows Figure 5Thermogravimetric analysis of the alloy samples prepared in this comparative example was performed, and the results are shown in Figure 6 shown.

[0052] pass Figure 2 , 3 It can be seen that the Laves phase exists in the alloy sample prepared in Comparative Example 1, while the Laves phase does not exist in the alloy sample prepared in Example 1, indicating that the addition of Zr can inhibit the formation of the Laves phase in the alloy. The Laves phase is a brittle phase. Its formation and increase in quantity will lead to increased brittleness of the alloy, which is not conducive to improving the comprehensive performance of the alloy. Therefore, by inhibiting the formation of the Laves phase, the amount of brittle phase in the alloy can be effectively reduced, and at the same time, the BCC phase and FCC phase structure can be stably formed in the alloy, thereby ensuring that the alloy has good thermal stability and creep resistance in a high temperature environment. Figure 4 It can be seen that the Vickers hardness of the alloy in Example 1 is 413 HV, and the Vickers hardness of the alloy in Comparative Example 1 is 342 HV. Therefore, after adding Zr, not only can the formation of Laves phase be suppressed to avoid the increase of alloy brittleness, but also the hardness of the alloy can be effectively improved.

[0053] pass Figure 2 , 3 It can also be seen that the Laves phase in the alloy of Comparative Example 3 increases significantly, indicating that when the Zr content in the alloy increases, its inhibitory effect on the formation of the Laves phase will decrease, and it may also promote the formation of the Laves phase. Figure 4 It can be seen that the formation of Laves phase has a certain effect on improving the hardness of the alloy, but Figure 5 It can be seen that the compressive strength of Comparative Example 3 is significantly reduced, and even cannot reach the compressive strength level of Comparative Example 1. Therefore, it can be seen that the increase in Zr content has a greater impact on the comprehensive properties of the alloy. At the same time, with the further increase of Zr content (Comparative Example 4), Figure 2 , 3 It can be seen that the Laves phase in Comparative Example 4 is reduced again, indicating that when the Zr content is further increased, the formation of the Laves phase in the alloy can be inhibited. Figure 4 , Figure 5 , Figure 6 It can be seen that the alloy hardness, compressive strength and thermogravimetric stability (thermogravimetric stability can characterize the high-temperature oxidation resistance of the alloy, the better the thermogravimetric stability, the better the high-temperature oxidation resistance of the alloy) of Comparative Example 4 are all reduced. Therefore, the comprehensive performance of the alloy cannot be improved at this time. Therefore, the control of the Zr content in the present invention can optimize the comprehensive performance of the alloy.

[0054] Compared with Comparative Example 2, Example 1 optimizes the proportional relationship in the high entropy alloy, and stabilizes the austenite phase by increasing the ratio of Fe and Ni, thereby improving the strength and plasticity of the alloy. At the same time, the proportions of Al, Co and Cr are moderately reduced, reducing the formation of brittle phases such as σ phase and Laves phase, and further improving the toughness of the material. In the alloy, the interaction of each component not only effectively inhibits the formation of brittle phases, but also promotes the generation of stable phases and refines the grain structure, thereby improving the comprehensive performance of the material. For example, Zr reacts with other elements to generate fine strengthening phases such as Al3Zr and Cr-Zr, which are dispersed in the alloy, further refine the grains, inhibit grain boundary sliding, and thus improve the comprehensive performance of the material.

[0055] Finally, it should be noted that the above preferred embodiments are only used to illustrate the technical solutions of the present invention rather than to limit it. Although the present invention has been described in detail through the above preferred embodiments, those skilled in the art should understand that various changes can be made in form and details without departing from the scope defined by the claims of the present invention.

Claims

1. A new type of high entropy alloy material, characterized in that: The chemical expression of the high entropy alloy material is AlCoCrFeNiZr, wherein the molar ratio of Al, Co, Cr, Fe, Ni and Zr is Al:Co:Cr:Fe:Ni:Zr=3.3:3.3:3.3:5:5:0.

1.

2. A new type of high entropy alloy material according to claim 1, characterized in that: The high entropy alloy material consists of FCC and BCC phases.

3. A method for preparing the novel high entropy alloy material according to claim 1 or 2, characterized in that: The preparation method comprises the following steps: (1) Raw material pretreatment: grinding the raw metals Al, Co, Cr, Fe, Ni, and Zr with a grinding wheel and polishing with sandpaper in turn, then ultrasonically cleaning the raw metals with ethanol, and then drying the raw metals for later use; (2) Vacuum arc melting: weighing the raw material metals pretreated in step (1) according to the molar ratio of the alloy components, placing the raw material metals in the order of Al, Ni, Co, Fe, Zr, and Cr from bottom to top into the crucible sub-tank of the vacuum arc furnace, then evacuating the vacuum arc furnace, and then filling the vacuum arc furnace with protective gas to normal pressure to melt the raw material metals; (3) Alloy suction casting: The molten alloy liquid after smelting in the step (2) is sucked into a copper mold and cooled to form a high entropy alloy material.

4. The preparation method according to claim 3, characterized in that: The purity of the raw metal is not less than 99.99%.

5. The preparation method according to claim 3, characterized in that: In the step (2), the smelting current intensity is 180-220A. During the smelting process, the smelting is turned over once every 2-5 minutes, and the turning is repeated 6-7 times.

6. The preparation method according to claim 3, characterized in that: In the step (2), the protective gas is argon.

7. The preparation method according to claim 3, characterized in that: In the step (2), the vacuum is evacuated to 5×10 -3 Pa.