Production method of seamless steel tube for Q345 steel grade fire-resistant structure

By using carbon-manganese steel type plus titanium microalloy treatment and molybdenum element addition in Q345 steel grade seamless steel pipes, combined with smelting and heat treatment processes, the problem of steel structures falling under high temperature conditions is solved, and high temperature yield is achieved The improvement of strength and seismic resistance meets the performance requirements of refractory steel for construction.

CN119020664AActive Publication Date: 2024-11-26BAOTOU IRON & STEEL (GROUP) CO LTD
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
CN202411083896.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-08
Publication Date
2024-11-26
Estimated Expiration
2044-08-08

AI Technical Summary

Technical Problem

The existing steel structures lose their load-bearing capacity under high temperature conditions, making it difficult to maintain sufficient yield strength and seismic resistance during fire periods, and the welding performance is insufficient, which cannot meet the fire resistance and seismic resistance requirements of buildings.

Method used

Using carbon-manganese steel type and titanium microalloy treatment, and by adding molybdenum elements, combined with optimized smelting and heat treatment processes, the Q345 steel-grade seamless steel pipes are prepared to control chemical composition and grain size, and improve high-temperature mechanical properties. .

Benefits of technology

At a temperature above 600℃, 2/3 of the room temperature yield strength was maintained, and the yield strength ratio was less than 0.8, which improved seismic performance and welding performance, and met the performance indicators of refractory steel for construction.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004984610980000031
    Figure BDA0004984610980000031
  • Figure BDA0004984610980000041
    Figure BDA0004984610980000041
  • Figure BDA0004984610980000042
    Figure BDA0004984610980000042
Patent Text Reader

Abstract

The invention discloses a production method of a seamless steel tube for a Q345 steel grade fire-resistant structure. The production process flow is briefly described as follows: molten iron pretreatment, top-bottom combined blown converter smelting, LF furnace refining, VD vacuum treatment, round billet continuous casting, tube billet heating, perforation, continuous rolling of a continuous rolling tube, fixed tension reducing, heat treatment, cooling bed treatment, saw cutting and straightening. The steel pipe comprises the following chemical components in percentage by weight: 0.14-0.17% of C; 0.20% to 0.30% of Si; mn: 1.30 to 1.40%; less than or equal to 0.020% of P; s: less than or equal to 0.010%; 0.015 to 0.040 percent of Al; ti: 0.008% to 0.020%; 0.20-0.30% of Mo, and the balance being iron and impurities. Titanium-added microalloying treatment is carried out on carbon-manganese steel, and the mechanical property at high temperature is improved by adding the molybdenum element, so that the use requirement of fire resistance is met.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of ferrous metallurgy, and in particular relates to a production method of a seamless steel pipe for a Q345 steel grade refractory structure. Background Art

[0002] Steel structure is the structural manifestation of advanced steel materials to achieve the target structure. It is a comprehensive embodiment of structural design, material application, and structural function. Seamless steel pipes for steel structures are mainly made by seamless pipe making technology and are often used in the connection and support parts of steel structures.

[0003] When a fire occurs, the strength of steel decreases rapidly due to the high temperature and cannot maintain the original strength of the building structure. When the temperature of the steel structure itself exceeds 550℃, the yield strength of the steel will drop by more than 50%; when the temperature is above 600℃ for a certain period of time, the steel will completely lose its original structural bearing capacity.

[0004] Because it is mainly used as a load-bearing material at room temperature, it is only required to maintain a high yield strength under high temperature conditions for a short period of time (usually 1 to 3 hours) when encountering a fire. 2 / 3 of the yield strength of steel at room temperature is equivalent to the long-term allowable stress value of the material. When a fire occurs, if the yield point of the fire-resistant steel can still be maintained above this value, the building will not collapse. Therefore, it is required that the yield strength of fire-resistant steel at a certain high temperature is not less than 2 / 3 of the yield strength at room temperature.

[0005] At the same time, as a structural material for construction, it is always hoped to maximize the ability of steel to absorb seismic energy. If the steel's yield strength ratio (Rel / Rm) is low, it will be beneficial for absorbing energy during an earthquake. Generally, the yield strength ratio of seismic-resistant and fire-resistant steel is required to be no more than 80%.

[0006] In addition, it is also very important to control the fluctuation range of the yield strength of construction steel. When the yield strength fluctuation is small, the steel structure is an overall failure mechanism, and its overall plastic deformation capacity is very high, and its seismic performance is excellent. Therefore, for seismic design, it is also necessary to require the use of steel with a narrow yield range. At the same time, building refractory materials also need to have good welding performance. In summary and based on the general requirements of construction steel, the performance indicators of building refractory steel pipes are determined as follows:

[0007] (1) Fire resistance: Rel 600℃ ≥(2 / 3)Rel 20℃ ;

[0008] (2) The room temperature mechanical properties and other quality indicators meet the requirements of ordinary construction steel standards;

[0009] (3) The yield strength ratio of earthquake resistance at room temperature is less than 80%. Summary of the invention

[0010] The purpose of the present invention is to provide a method for producing a Q345 steel grade seamless steel pipe for fire-resistant structure, which adopts carbon-manganese steel and titanium micro-alloying treatment, and improves the mechanical properties at high temperature by adding molybdenum element to meet the fire-resistant use requirements, and has excellent performance.

[0011] In order to solve the above technical problems, the present invention adopts the following technical solutions:

[0012] The present invention discloses a method for producing a Q345 steel grade seamless steel pipe for refractory structure. The production process is briefly described as follows: molten iron pretreatment → top and bottom combined blowing converter smelting → LF furnace refining → VD vacuum treatment → round billet continuous casting

[0013] → tube heating → piercing → continuous tube rolling → fixed tension and diameter reduction → heat treatment → cooling bed → sawing → straightening; Among them:

[0014] 1) Pre-treating the blast furnace molten iron to reduce the weight percentage of S in the molten iron to less than 0.050%;

[0015] 2). Add the pre-treated molten iron into the top and bottom double-blown converter, add 10% scrap steel by weight, adopt the single slag process to smelt, control the final slag basicity and the end point target: [C] steel tapping ≥ 0.10%; deoxidation and alloying are carried out during the steel tapping process, and the final deoxidation adopts the aluminum deoxidation process. The steel tapping process must be blocked or slag removed. After the alloy is added during the steel tapping process, lime blocks are added;

[0016] 3). Refining in LF furnace: During the whole refining process, argon is blown normally as required, and the heating is carried out by gradually increasing the heating rate from low to high levels; slag making, desulfurization, composition adjustment and heating operations are carried out according to the composition and temperature of the molten steel in the converter; white slag making operation is adopted;

[0017] 4). After the LF furnace refining is completed, keep the bottom soft argon blowing for more than 10 minutes;

[0018] 5). Perform VD vacuum treatment: vacuum degree ≤ 0.10KPa, deep vacuum time ≥ 10 minutes;

[0019] 6). Feed fixed-length calcium silicon wire, blow argon for more than 15 minutes after feeding; cast the molten steel after VD vacuum treatment into round billets, adopt low pulling speed, constant pulling speed control and electromagnetic stirring process; control the superheat of molten steel; cut the billet into round tube billets after straightening;

[0020] The round tube billets that have passed the inspection and whose sulfur print is not greater than level 2.0 are made into tubes. The tube making process is as follows;

[0021] Continuously check the temperature of the preheating section, heating section, and soaking section. The temperature control of each section of the ring furnace is shown in the table below;

[0022]

[0023] Heat treatment is performed on the rolled seamless steel pipe to obtain a qualified steel pipe whose performance meets the standard requirements;

[0024] The chemical composition of the steel pipe is as follows by weight: C: 0.14-0.17%; Si: 0.20-0.30%; Mn: 1.30-1.40%; P: ≤0.020%; S: ≤0.010%; Al: 0.015-0.040%; Ti: 0.008-0.020%; Mo: 0.20-0.30%, and the rest is iron and unavoidable impurities.

[0025] Furthermore, the heat treatment is normalizing treatment: the normalizing temperature is 910±10°C, the normalizing holding time is 70min, and the cooling method is air cooling.

[0026] Furthermore, the computer control system records the heating temperature of each section online, and requires the temperature of the preheating section and the soaking section to be well controlled to ensure thorough and uniform heating without overburning.

[0027] Furthermore, hot tools must be measured before use, and rollers must be inspected and treated before rolling to avoid scratches.

[0028] Further, the heated tube billets are rolled into seamless steel tubes, and each batch is subjected to at least one hot sampling to check the geometric dimensions.

[0029] Furthermore, the yield strength ratio of the seamless steel pipe after heat treatment is less than the required 0.8.

[0030] Furthermore, after heat treatment, the grain size of the seamless steel pipe reaches level 8, and the structure is ferrite plus pearlite plus a small amount of bainite.

[0031] Compared with the prior art, the beneficial technical effects of the present invention are:

[0032] The present invention adopts 16MnMoTi steel, the material composition is reasonably designed, and the cost is low. The performance of the steel pipe prepared by the optimized process meets the fire-resistant use requirements. DETAILED DESCRIPTION

[0033] The present invention is further described in detail below with reference to examples.

[0034] A method for producing a Q345 steel grade seamless steel pipe for refractory structure, specifically comprising:

[0035] 1. Steel smelting

[0036] 1.1 Actual smelting product composition

[0037] The composition of the trial tube billet is strictly controlled within the required range, and the specific data is shown in Table 2.

[0038] Table 2 Finished product ingredients (%)

[0039]

[0040] 1.2 Sulfur print test results

[0041] The results of the sulfur print test of the ingot are listed in Table 3, among which the center crack and inclusions are level one, the middle crack and subcutaneous crack are level zero, and the quality of the ingot is in good condition.

[0042] Table 3 Sulphur print test results of ingot

[0043]

[0044] 1.3 Inclusion Control

[0045] From the data in Table 4, it can be seen that inclusions are well controlled.

[0046] Table 4 Metallographic inspection results

[0047]

[0048] 2. Seamless steel pipe specifications

[0049] The specification of seamless steel pipe is φ426×20mm.

[0050] 3. Heat treatment of steel

[0051] 3.1 Heat treatment system

[0052] The rolled steel pipe is normalized in the heat treatment furnace operation line. The heat treatment system is shown in Table 5:

[0053] Table 5 Heat treatment system

[0054]

[0055] 3.2 Mechanical properties

[0056] After heat treatment, samples were taken for inspection. The tensile test results are shown in Table 6. The mechanical properties met the standard requirements after treatment, and the yield strength ratio was 0.67, which is less than the required 0.8.

[0057] Table 6 Tensile test results

[0058]

[0059] 3.3 Impact energy

[0060] The impact test results are shown in Table 7. From the data in the table, it can be seen that the impact energy fully meets the standard requirements:

[0061] Table 7 Normalized impact test results

[0062]

[0063] 3.4 Grain size structure after heat treatment

[0064] After heat treatment, the grain size reaches level 8, and the structure is ferrite plus pearlite plus a small amount of bainite.

[0065] 4. High temperature tension

[0066] The high temperature tensile force at 600℃ is greater than two-thirds of that at room temperature, meeting the requirements.

[0067] Table 8 High temperature mechanical properties

[0068]

[0069] The embodiments described above are only descriptions of the preferred modes of the present invention, and are not intended to limit the scope of the present invention. Without departing from the design spirit of the present invention, various modifications and improvements made to the technical solutions of the present invention by ordinary technicians in this field should all fall within the protection scope determined by the claims of the present invention.

Claims

1. A method for producing a Q345 steel grade seamless steel pipe for refractory structure, characterized in that: The production process can be briefly described as follows: hot metal pretreatment → top and bottom combined blowing converter smelting → LF furnace refining → VD vacuum treatment → round billet continuous casting → tube billet heating → perforation → continuous rolling → fixed tension and diameter reduction → heat treatment → cooling bed → sawing → straightening; among which: 1) Pre-treating the blast furnace molten iron to reduce the weight percentage of S in the molten iron to less than 0.050%; 2). Add the pre-treated molten iron into the top and bottom double-blown converter, add 10% scrap steel by weight, adopt the single slag process to smelt, control the final slag basicity and the end point target: [C] steel tapping ≥ 0.10%; deoxidation and alloying are carried out during the steel tapping process, and the final deoxidation adopts the aluminum deoxidation process. The steel tapping process must be blocked or slag removed. After the alloy is added during the steel tapping process, lime blocks are added; 3). Refining in LF furnace: During the whole refining process, argon is blown normally as required, and the heating is carried out by gradually increasing the heating rate from low to high levels; slag making, desulfurization, composition adjustment and heating operations are carried out according to the composition and temperature of the molten steel in the converter; white slag making operation is adopted; 4). After the LF furnace refining is completed, keep the bottom soft argon blowing for more than 10 minutes; 5). Perform VD vacuum treatment: vacuum degree ≤ 0.10KPa, deep vacuum time ≥ 10 minutes; 6). Feed fixed-length calcium silicon wire, blow argon for more than 15 minutes after feeding; cast the molten steel after VD vacuum treatment into round billets, adopt low pulling speed, constant pulling speed control and electromagnetic stirring process; control the superheat of molten steel; cut the billet into round tube billets after straightening; The round tube billets that have passed the inspection and whose sulfur print is not greater than level 2.0 are made into tubes. The tube making process is as follows; Continuously check the temperature of the preheating section, heating section, and soaking section. The temperature control of each section of the ring furnace is shown in the table below; Heat treatment is performed on the rolled seamless steel pipe to obtain a qualified steel pipe whose performance meets the standard requirements; The chemical composition of the steel pipe is as follows by weight: C: 0.14-0.17%; Si: 0.20-0.30%; Mn: 1.30-1.40%; P: ≤0.020%; S: ≤0.010%; Al: 0.015-0.040%; Ti: 0.008-0.020%; Mo: 0.20-0.30%, and the rest is iron and unavoidable impurities.

2. The method for producing a Q345 steel grade seamless steel pipe for refractory structure according to claim 1, characterized in that: The heat treatment is normalizing treatment: the normalizing temperature is 910±10° C., the normalizing holding time is 70 minutes, and the cooling method is air cooling.

3. The method for producing a Q345 steel grade seamless steel pipe for refractory structure according to claim 1, characterized in that: The computer control system records the heating temperature of each section online, and requires the temperature of the preheating section and the soaking section to be well controlled to ensure thorough and uniform heating without overburning.

4. The method for producing a Q345 steel grade seamless steel pipe for refractory structure according to claim 1, characterized in that: Hot tools must be measured before use, and rollers must be inspected and treated before rolling to avoid scratches.

5. The method for producing a Q345 steel grade seamless steel pipe for refractory structure according to claim 1, characterized in that: The heated tube billets are rolled into seamless steel tubes, and hot sampling is carried out at least once for each batch to check the geometric dimensions.

6. The method for producing a Q345 steel grade seamless steel pipe for refractory structure according to claim 1, characterized in that: The yield strength ratio of the seamless steel pipe after heat treatment is less than the required 0.

8.

7. The method for producing a Q345 steel grade seamless steel pipe for refractory structure according to claim 1, characterized in that: After heat treatment, the grain size of the seamless steel pipe reaches level 8, and the structure is ferrite plus pearlite plus a small amount of bainite.

Citation Information

Patent Citations

  • High strength low alloy structural normalizing A633GRD steel plate and production method thereof

    CN102345059A

  • Atmosphere corrosion resistance seamless steel tube containing rare earth and production method thereof

    CN103290334A

  • Low-cost and H2S-corrosion-resistant L390NS pipeline tube containing rare earth and production method of pipeline tube

    CN103667929A

  • 345MPa-level steel plate for high-rise building structure and production method thereof

    CN103695775A

  • Low-alloy high-strength large-diameter thick-walled seamless steel pipe and manufacturing method thereof

    CN105586532A