Smelting method of refractory chromite

By controlling the particle size of chromite ore into the furnace and optimizing the material distribution and process parameters in the furnace, the problems of crater resistance, material collapse and power consumption increase in the process of smelting in large ore furnaces are solved, and the problem of refractory chromite ore is improved. Smelting efficiency achieves efficient and economical production of ferrochromium alloys.

CN119020669APending Publication Date: 2024-11-26SHANXI TAIGANG WANBANG CHARGE CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411146572.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-21
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

During the use of refractory chromium iron ore in large ore furnaces, problems such as chromium ore recovery, iron outlet jamming, material collapse in the furnace, increased power consumption, reduced output, and chromium run in the slag, affecting production capacity and efficiency.

Method used

By controlling the particle size of chromite into the furnace, optimizing the distribution of materials in the furnace, designing reasonable slag type, controlling the working position of the electrode and the electricity consumption of a single furnace, increasing the capacity of the molten iron and reaction time, the fixed-point fabric and circumference uniform fabric mode are used to improve the Masonry method of refractory castable.

Benefits of technology

Eliminates problems such as iron outlet jamming, collapse of furnace, increased power consumption, reduced output, and chromium running in slag, improves the reduction efficiency of refractory chromite, and achieves efficient and economical smelting effect. 2023 The Cr2O3 content in the monthly slag decreased by 0.8%, creating an effect of 1.6493 million yuan.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119020669A_ABST
    Figure CN119020669A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of iron alloy smelting, in particular to a smelting method of refractory chromite, which is characterized in that aiming at the metallurgical characteristics of the refractory chromite on a large submerged arc furnace, the contact area, the reaction temperature and the reaction time of chemical reaction of materials in the furnace are ensured by controlling the size fraction in the furnace, optimizing material distribution and exploring reasonable operation parameters, and the reduction efficiency is improved. The restricting factors such as taphole jamming, material collapse in the furnace, power consumption increase, yield reduction and chromium running in slag are solved, and efficient and economical use of the refractory chromite in the large submerged arc furnace is achieved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of ferroalloy smelting, and in particular to a smelting method of refractory chromite. Background Art

[0002] Shanxi Taigang Wanbang Furnace Material Co., Ltd. has two 75MVA fully enclosed submerged arc furnaces, which are the largest capacity furnaces for producing ferrochrome in China, with an annual output of 300,000 tons of qualified ferrochrome. This set of process uses pellets roasted from ferrochrome concentrate powder, with a certain proportion of silica, dolomite, coke particles and other auxiliary materials, which are transported into the furnace by a belt conveyor. Under the action of the electric energy provided by three single-phase 35KV transformers through three electrodes, complex physical and chemical reactions are carried out to reduce chromium, iron, silicon and other elements from their oxides to form ferrochrome and slag, which are discharged from the iron outlet.

[0003] Due to its refractory nature, refractory chromite ore has the potential to cause problems such as difficulty in reducing chromite ore, taphole obstruction, furnace collapse, increased power consumption, reduced output, and chromium leakage in the slag during use in large-scale ore-fired furnaces, which directly affect production capacity and benefits.

[0004] The present invention solves the restrictive factors such as tap hole obstruction, material collapse in the furnace, increased power consumption, reduced output, and chromium leakage in the slag during the smelting process by optimizing the smelting process route, reasonably distributing materials in the furnace, adjusting operating parameters, and implementing process control, and explores a method for efficient smelting of Tibetan chromite. Summary of the invention

[0005] The purpose of the present invention is to provide a smelting method for refractory chromite in view of the above problems.

[0006] The object of the present invention is achieved as follows: A smelting method for refractory chromite, comprising the following steps: Step 1: Controlling the particle size of the chromite entering the furnace: Controlling the particle size of the ore entering the furnace to 4-20 mm; Step 2: Optimizing the distribution state of the material in the furnace: Increasing the distribution ratio of the refractory chromite in the central high-temperature area to 20-40%; Step 3: Designing the slag type: Al2O3: 26-28.5, CaO: 5-6, Cr2O3: 4.5-6.5, MgO: 24.0-26, SiO2: 27.5-29.0, R3: 1.0- 1.1, M / A: 0.80-0.95, T slag: 1740-1760℃; Step 4: Control the electrode working position and single furnace power consumption: When smelting refractory chromite, the electrode working end position is controlled at 1550-1650mm from the horizontal position of the iron mouth, and the single furnace power consumption is controlled at 170-180KWh; Step 5: Increase the iron output of a single furnace and extend the reaction time of the refractory chromite in the furnace: The thickness of the refractory material of the iron ladle wall is 190-230mm, the capacity of a single ladle is 28-35t, and the refractory material is laid by integral pouring of refractory castables.

[0007] In step 2, there are two modes of fabric: fixed-point fabric and circular uniform fabric.

[0008] The beneficial effects of the present invention are as follows: the method optimizes and upgrades the production process route according to the metallurgical characteristics of refractory chromite, controls the particle size of the material entering the furnace, reasonably distributes the materials in operation, optimizes and matches the operating parameters, ensures that the refractory chromite, auxiliary materials and reducing agent in the furnace have sufficient contact area, reaction temperature and reaction time for chemical reaction, improves the reduction efficiency, eliminates the restrictive factors such as iron outlet obstruction, material collapse in the furnace, increased power consumption, reduced output and chromium leakage in the slag, and realizes the efficient and economical use of refractory chromite in large-scale submerged arc furnaces.

[0009] Through the application of this method, the Cr2O3 content in the slag in June 2023 decreased by 0.8% compared with the benchmark of 8.0%. The benefit calculation is: the slag volume is 18,837.4t, and the chromium content in the slag is equivalent to 50-base ferrochrome, which is 18,837.4×0.8%×0.684 / 0.5=206.16t. The price per ton is calculated at 8,000 yuan, and the benefit is: 1.6493 million yuan. BRIEF DESCRIPTION OF THE DRAWINGS

[0010] The present invention will be further described below in conjunction with the accompanying drawings.

[0011] Figure 1 This is a diagram of the ladle of the present invention before capacity expansion.

[0012] Figure 2 This is a diagram of the ladle after capacity expansion according to the present invention. DETAILED DESCRIPTION

[0013] 1. Control the appropriate particle size of chromite entering the furnace so that the material has the best reaction area after entering the furnace. The process route has been optimized for the metallurgical characteristics of refractory chromite. Before the improvement, the raw ore entering the factory was directly put into the furnace. After the powder ore enters the furnace, the permeability of the material column deteriorates, and the furnace collapses and the furnace condition deteriorates frequently. Large pieces of chromite are difficult to melt and reduce when entering the furnace. The height of the material column in the furnace is only 4.5 to 5 meters. It drops to the iron outlet area before it is fully melted and reduced. When tapping, it is blocked, which makes tapping difficult and prolongs the time. Large oxygen is used to clear the channel, and the refractory material of the iron outlet is damaged. For this reason, the size of the chromite entering the furnace is controlled and optimized. Add crushing and screening facilities, and strictly control the entry of larger particles and powder ore into the furnace.

[0014] The main measures taken: A PE400×600 jaw crusher was added to the process line for refractory chromite lump ore entering the furnace. The gap between the jaw plates of the crusher was adjusted from the normal 35mm to the minimum gap of 25mm. The particle size after crushing was tested, and the optimal value after optimization was finally 30mm in combination with the changes in furnace conditions. A screening device was added. The initial screen plate was a 5mm bar screen. Because the particles larger than 5mm accounted for 15% of the screened material, the screen plate was later replaced with a 4mm plate screen, and then optimized to a 3mm round hole steel plate screen. The particle size of the ore entering the furnace was controlled at 4 to 20mm.

[0015]

[0016] 2. Optimize the distribution of materials in the furnace. According to the temperature distribution gradient in the furnace, the temperature at the edge is slightly lower and the temperature in the center is the highest. Increase the distribution ratio of refractory chromite in the central high-temperature area to improve the reduction efficiency.

[0017] The rotary distributor's rotation mode is improved, changing the original automatic rotation distribution mode to realize the rotation distribution + fixed-point distribution mode. The rotary distributor is a rotary flow trough type, and the distribution is in two modes: fixed-point distribution + circumferential uniform distribution. The refractory chromite is distributed more to the central high-temperature area in a targeted manner, and the proportion is increased from the original 10% to 30%.

[0018] 3. Design reasonable slag shape to improve slag fluidity and melting temperature and improve reduction efficiency in the furnace.

[0019]

[0020] Through comparative tests, slag type 2 was finally determined to be the most reasonable slag type.

[0021] 4. Control the optimal electrode working position, single furnace power consumption and other process parameters.

[0022] When smelting fusible chromite in a large-scale electric arc furnace, the position of the electrode working end is controlled at 1700-1800mm from the horizontal position of the taphole, and the power consumption of a single furnace is controlled at 150-165KWh; when smelting refractory chromite, through experimental summary, the best control value is that the position of the electrode working end is controlled at 1550-1650mm from the horizontal position of the taphole, and the power consumption of a single furnace is controlled at 170-180KWh.

[0023] 5. Modify the capacity of the iron ladle to increase the iron output of a single furnace and extend the reaction time of the refractory chromite in the furnace.

[0024] Through sufficient demonstration, under the premise of ensuring safety, the existing refractory material of the ladle wall is optimized from 250mm to 210mm, thinned by 40mm, and the single ladle capacity is increased from 25t to 30t. The refractory masonry method is improved from refractory brick masonry to integral pouring of refractory castables, so as to achieve the same ladle cleaning conditions, and the number of online use of the ladle is not reduced. Embodiment 1

[0025] From June to October 2021, our company added about 10,000 tons of refractory ferrochrome ore.

[0026] In early January 2023, a batch of refractory chromite entered our company. On the 10th, we adjusted the gap of the chromite lump crusher to 20-25mm, increased the crushing of large-block ore, adjusted the sieve to a round hole sieve plate with an aperture of 3mm, and controlled the particle size of the chromite lump entering the furnace to 4-20mm. The compliance rate is above 90%.

[0027] Starting from February, in terms of fabric, we used 3 circles of uniform fabric + 2 circles of center fixed point fabric.

[0028] In terms of smelting slag type control, the slag composition is controlled as shown in the following table by adjusting the amount of dolomite added.

[0029]

[0030] The electrode position is controlled at 1580-1630mm from the horizontal position of the taphole, and the power consumption of a single furnace is controlled at 170-180KWh.

[0031] In mid-February, the thickness of the refractory material in the ladle was adjusted from 250mm to 210mm, the molten iron capacity increased by about 20%, and the smelting time of a single furnace was extended by 15 to 20 minutes.

[0032] Through the implementation of the above measures, our company added a total of 18,600 tons of refractory ferrochrome lump ore from January to June 2023. The Cr2O3 content in the slag was reduced to 7.0%, reaching the leading level among similar domestic enterprises.

[0033] The above description is only a specific embodiment of the present invention, but the structural features of the protection scope of the present invention are not limited thereto. Any changes or modifications made by any technician in the field of the present invention are all covered by the patent scope of the present invention.

Claims

1. A method for smelting refractory chromite, characterized in that: The following steps are involved: Step 1: Control the particle size of chromite entering the furnace: control the particle size of the ore entering the furnace to 4-20mm; Step 2: Optimize the distribution of materials in the furnace: Increase the distribution ratio of refractory chromite to 20-40% in the central high-temperature area; Step 3: Design slag type: Al2O3: 26-28.5, CaO: 5-6, Cr2O3: 4.5-6.5, MgO: 24.0-26, SiO2: 27.5-29.0, R3: 1.0-1.1, M / A: 0.80-0.95, T slag: 1740-1760℃; Step 4: Control the electrode working position and the power consumption of a single furnace: When smelting refractory chromite, the position of the electrode working end is controlled at 1550-1650mm from the horizontal position of the taphole, and the power consumption of a single furnace is controlled at 170-180KWh; Step 5: Increase the iron output of a single furnace and extend the reaction time of refractory chromite in the furnace: the thickness of the refractory material of the ladle wall is 190-230mm, the capacity of a single ladle is 28-35t, and the refractory material is laid by integral pouring of refractory castables.

2. The smelting method of refractory chromite according to claim 1, characterized in that: In step 2, there are two modes of fabric: fixed-point fabric and circular uniform fabric.