Titanium-containing, boron-containing and aluminum-containing killed cold forging steel and refining method thereof

By refining titanium- and boron- and aluminum-killed cold heading steel, controlling the addition of alloying elements and bottom blowing stirring, the oxidation of Ti and B elements was solved, the alloy hit rate and steel cleanliness were improved, and the casting performance and product quality were stabilized.

CN119020692APending Publication Date: 2024-11-26CHANGSHU LONGTENG SPECIAL STEEL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411210519.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-30
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

In the existing technology, titanium-, boron-, and aluminum-killed cold heading steel has a low alloy hit rate, poor steel casting properties, and the Ti and B elements are easily oxidized, affecting the cleanliness of the molten steel and the quality of the product.

Method used

A refining method for titanium-, boron-, and aluminum-killed cold heading steel is adopted, which includes KR desulfurization, converter smelting, LF refining, and continuous casting. By controlling the addition of alloying elements and bottom blowing agitation, the yield of Ti and B elements is ensured. Ultra-high basicity slag and argon protection are used to reduce oxide inclusions and improve the cleanliness of molten steel.

Benefits of technology

It improved the alloy hit rate, stabilized casting performance, ensured product quality, reduced oxide inclusions, and improved the cleanliness of molten steel and production stability.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention relates to killed cold forging steel containing titanium, boron and aluminum and a refining method of the killed cold forging steel. The refining method comprises the steps of KR desulfurization, converter smelting, converter tapping, LF refining and continuous casting protective pouring. The converter recarburization replaces a high carbon catch technology, so that high-carbon and low-oxygen molten steel is obtained at the end point of the converter, the stable yield of Ti and B elements is ensured, the problem of oxidation of Ti and B alloys of the killed cold forging steel containing titanium, boron and aluminum is effectively solved, the cleanliness of the molten steel is improved, and the pouring performance and the product quality are stabilized.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a titanium-containing, boron-containing, aluminum-killed cold heading steel and a refining method thereof, belonging to the technical field of metallurgy, in particular to a refining method for aluminum-killed steel. Background Art

[0002] Cold heading steel is generally aluminum-killed steel, but due to the large number of alloy additions, the long refining cycle, improper deoxidation alloying and slag making process control, it is easy to cause oxidation of alloy elements, which is not conducive to cleanliness control. In the prior art, more attention is paid to the influence of aluminum elements on cold heading steel. For example, the application with the publication (announcement) number CN112609131A provides a low-carbon aluminum-killed cold heading steel and a production method thereof. The composition of the cold heading steel is: C 0.06-0.09%, Mn 0.30-0.50%, Si0.03-0.06%, P≤0.015%, S≤0.010%, Al 0.020-0.040%, and the balance is Fe and unavoidable impurities. The low-carbon aluminum-killed cold heading steel is prepared through steelmaking, continuous casting, hot rolling and wire-laying processes. Through composition adjustment and process optimization, the mechanical properties of the prepared cold heading steel meet the use requirements.

[0003] However, in reality, other elements contained in the steel also have a great influence on the performance. For example, if Ti is oxidized in large quantities, it will cause nozzle nodules, which also brings considerable difficulty to the calcium treatment process. It is also very difficult to control trace B elements, because B elements are easy to oxidize and combine with N to form BN precipitates during the continuous casting process, affecting the quality of the ingot.

[0004] Therefore, it is necessary to provide a composition and refining method for titanium-containing boron-containing aluminum killed cold heading steel to effectively solve the problems of low alloy hit rate and poor castability of molten steel of titanium-containing boron-containing cold heading steel. Summary of the invention

[0005] The invention provides a titanium-containing boron-containing aluminum killed cold heading steel and a refining method thereof, which effectively solves the oxidation problem of Ti and B alloys in titanium-containing and boron-containing aluminum killed cold heading steel, improves the cleanliness of molten steel, and stabilizes casting performance and product quality.

[0006] The technical solution adopted by the present invention to solve its technical problem is: A titanium-boron-aluminum killed cold heading steel comprising the following chemical components in percentage by mass: C: 0.30-0.40%, Si: 0.10-0.20%, Mn: 0.45-0.60%, Alt: 0.010-0.045%, P≤0.018%, S≤0.012%, Cr: 0.10-0.20%, Ti: 0.015-0.055%, B: 0.0010-0.0030%, Ni≤0.03%, As≤0.02%, Cu≤0.03%, Fe and other inevitable components; The refining method of the titanium-containing, boron-containing, aluminum-killed cold heading steel specifically comprises the following steps: Step S1: KR desulfurization. The mass percentages of the elements in the molten iron after KR desulfurization are as follows: C: 4.0-4.3%, Si: 0.30-0.65%, Mn: 0.10-0.25%, P≤0.13%, S≤0.005%. The temperature after desulfurization is 1320-1380°C. Step S2: converter smelting, adding the desulfurized molten iron and clean scrap steel into the converter for smelting, with the scrap steel ratio being 10-20%. The C content in the molten steel is controlled to be ≤0.08% at the end of converter smelting, and oxygen blowing is stopped; Add carbon powder to the converter, start bottom blowing and stirring until C in the molten steel is 0.15-0.25%, O≤0.035%, while controlling P≤0.016%, S≤0.008%, and temperature≥1600℃; Step S3: tapping the converter. When 1 / 3 of the converter is tapped, alloys are added in the order of carbon alloy, metallic aluminum, high carbon ferrochrome, and silicon manganese. When 90% of the tapping is completed, lime and calcium aluminosilicate synthetic slag are added. Before the tapping is completed, all the alloys, lime, and calcium aluminosilicate synthetic slag are added. The ladle is bottom blown and stirred throughout the tapping process. After the tapping is completed, stirring is continued for a preset time, and then the steel is transported to LF for refining. Step S4: LF refining, LF refining station, start ladle bottom blowing and stirring, power on to increase temperature, and take samples to measure the chemical composition of molten steel and slag. After the molten steel and slag components are tested, add alloy and carbon powder to fine-tune the molten steel composition according to the target composition of titanium-containing, boron-containing, and aluminum-killed cold heading steel grades, so that the molten steel composition reaches the target composition. At the same time, add lime, calcium carbide, and calcium aluminate slag deoxidizer to adjust the slag composition. After the molten steel temperature, composition, and slag composition reach the target, add ferrotitanium to make the Ti element content reach the target composition. After weak stirring for 3-5 minutes, add ferroboron. After weak stirring for 3-5 minutes, perform calcium treatment. During the calcium treatment, feed silicon calcium wire. After the calcium treatment is completed, adjust the ladle bottom blowing to the soft stirring mode. After the soft stirring is completed, transport the molten steel to the continuous casting pouring; Step S5: continuous casting to form the titanium-containing, boron-containing, and aluminum-killed cold heading steel according to claim 1; Furthermore, in step S2, the added clean scrap steel includes the following chemical components in mass percentage: S content ≤ 0.008%, P content ≤ 0.015%, Ni ≤ 0.15%, Cu ≤ 0.08%, As ≤ 0.015%, and the rest is Fe and other unavoidable components; Furthermore, in step S2, the specific process of adding carbon powder into the converter is to open four bottom blows at the bottom of the converter, wherein three bottom blows of argon are set at a flow rate of 500-1000NL / min; one bottom blow of oxygen is set at a flow rate of 2000-5000NL / min; Further, in step S3, when 1 / 3 of the steel is tapped from the converter, the amount of carbon-containing alloy added is 1.5-2.5 kg / t, the amount of metallic aluminum added is 1.5-2.0 kg / t, the amount of high-carbon ferrochrome added is 1.7-2.3 kg / t, and the amount of silicon manganese added is 4.5-6.5 kg / t; When the steel is 90% tapped, the amount of lime added is 2.5-3.5kg / t, and the amount of calcium silicate synthetic slag added is 6-8kg / t; The ladle is bottom blown and stirred throughout the steel tapping process. The bottom blowing flow rate is set to 200-400NL / min. After the steel tapping is completed, it is stirred for another 3-5 minutes before being transported to the refining process. Further, in step S3, the mass percentages of the elements in the carbon-containing alloy are: C: 35-45%, P≤0.015%, S≤0.007%, and the rest are Fe and other inevitable components; The mass percentage of each element in metallic aluminum is: Al ≥ 99.7%, the rest is Fe and other inevitable components; The mass percentages of the elements in high carbon ferrochrome are: Cr: 53-57%, C: 8-12%, and the rest are Fe and other inevitable components; The mass percentage of each element in silicon manganese is: Si: 18-23%, Mn: 67-70%, P≤0.018%, S≤0.012%, and the rest is Fe and other inevitable components; The components of lime are calculated by mass percentage as follows: CaO ≥ 95%, and other inevitable components; The components of calcium aluminosilicate synthetic slag are calculated by mass percentage as follows: CaO: 45-55%, Al2O3: 35-45%, SiO2≤5%, MgO: 3-6%, and the rest are inevitable components; Further, in step S4, after the LF refining enters the station, the ladle bottom blowing and stirring are turned on, and the bottom blowing flow rate is set to 200-300NL / min; When adding alloy and carbon powder to fine-tune the composition of molten steel, set the bottom blowing flow rate to 250-350NL / min; When adding lime, calcium carbide, and calcium aluminate slag deoxidizer to adjust the slag composition, set the bottom blowing flow rate to 150-200NL / min; When adding ferrotitanium and ferroboron, set the bottom blowing flow rate to 100-150NL / min; When weak stirring is used, the bottom blowing flow rate is set to 80-100NL / min; During calcium treatment, the bottom blowing flow rate is set to 150-200NL / min; During soft stirring, set the bottom blowing flow rate to 20-60NL / min; Furthermore, in step S4, the amount of lime added is 1.0-2.5 kg / t, the amount of calcium carbide added is 0.8-1.5 kg / t, and the amount of calcium aluminate slag deoxidizer added is 1.5-2.5 kg / t; The components of lime are calculated by mass percentage as follows: CaO ≥ 95%, and other inevitable components; The components in calcium carbide are calculated by mass percentage as follows: CaC2 ≥ 95, and other inevitable components; The components of calcium aluminate slag deoxidizer are calculated by mass percentage as follows: CaO: 45-55%, Al2O3: 20-30%, metal aluminum 10-20%, metal calcium 5-10%, SiO2≤3%, and other inevitable components; During calcium treatment, 1-1.5 m / t of silicon-calcium wire is fed, with a Ca content of 25-35%, and the rest being Si and unavoidable impurities; the wire feeding rate during calcium treatment is set to 5-8 m / s, the outlet of the silicon-calcium wire feeding machine is ≤20 cm away from the ladle slag surface, and the soft stirring is ≥15 min after the calcium treatment is completed; Further, in step S4, the slag basicity obtained after refining is ≥30, the (CaO / Al2O3) C / A ratio is 1.8-2.2, and the T.Fe+MnO content is ≤0.8%; Further, in step S5, the continuous casting process uses a three-layer middle-layer covering agent, and the thickness of each layer of the covering agent is ≥15 mm; The first layer is a calcium aluminate covering agent, and the components by mass percentage are: CaO: 50-55%, Al2O3: 25-35%, MgO: 3-6%, Na2O: 2-5%, and other inevitable components; The second layer is fine lime powder, with a particle size of 1-3mm accounting for ≥90% and a maximum particle size of 6mm; The third layer is carbonized rice husk, and the mass percentage of each component is: SiO2 ≥ 85%, and the rest is C and other inevitable components.

[0007] Through the above technical solution, compared with the prior art, the present invention has the following beneficial effects: 1. The titanium-boron-aluminum-killed cold heading steel provided by the present invention has a high alloy hit rate, the product is not easy to crack during the processing, and the finished product quality is high; 2. The refining method of titanium-containing boron-containing aluminum-killed cold heading steel provided by the present invention innovatively proposes a converter carbon increase technology to replace high carbon drawing technology, so that high-carbon, low-oxygen molten steel is obtained at the end of the converter, which is very beneficial to improving cleanliness; 3. The refining method of titanium-containing boron-containing aluminum killed cold heading steel provided by the present invention ensures the stable yield of Ti and B elements, guarantees the quality of molten steel, and ensures the stability of production. DETAILED DESCRIPTION

[0008] The specific range used in this embodiment is only to illustrate the technical solution and does not limit the protection scope of the present invention.

[0009] As pointed out in the background technology, the Ti and B elements contained in aluminum-killed cold heading steel will affect the pouring performance of molten steel. Therefore, the present application provides a titanium-containing, boron-containing, aluminum-killed cold heading steel and a refining method thereof, which effectively solves the oxidation problem of Ti and B alloys in titanium-containing and boron-containing aluminum-killed cold heading steels, improves the cleanliness of molten steel, and stabilizes the pouring performance and product quality.

[0010] The refining method for titanium-containing, boron-containing, and aluminum-killed cold heading steel specifically comprises the following steps: Step S1: KR desulfurization. The mass percentages of the elements in the molten iron after KR desulfurization are as follows: C: 4.0-4.3%, Si: 0.30-0.65%, Mn: 0.10-0.25%, P≤0.13%, S≤0.005%. The temperature after desulfurization is 1320-1380°C.

[0011] Step S2: converter smelting, adding the desulfurized molten iron and clean scrap steel into the converter for smelting, with the scrap steel ratio being 10-20%. The C content in the molten steel is controlled to be ≤0.08% at the end of converter smelting, and oxygen blowing is stopped; The added clean scrap steel includes the following chemical components in mass percentage: S content ≤ 0.008%, P content ≤ 0.015%, Ni ≤ 0.15%, Cu ≤ 0.08%, As ≤ 0.015%, and the rest is Fe and other inevitable components.

[0012] Add carbon powder to the converter, start bottom blowing and stirring until C in the molten steel is 0.15-0.25%, O≤0.035%, while controlling P≤0.016%, S≤0.008%, and temperature≥1600℃; The specific process of adding carbon powder into the converter is to open four bottom blowing at the bottom of the converter, of which three are argon blows with a set flow rate of 500-1000NL / min; one is oxygen blows with a set flow rate of 2000-5000NL / min.

[0013] This step is one of the innovative points of this application. Through the carbon increase technology in the converter, the carbon content of the steel out of the converter is increased, the oxygen content of the molten steel is reduced, the oxidation of the alloy in the deoxidation and alloying process is reduced, and the amount of oxide inclusions generated is also reduced.

[0014] Step S3: tapping the converter. When 1 / 3 of the converter is tapped, add the alloy in the order of carbon-containing alloy, metallic aluminum, high carbon ferrochrome, and silicon manganese. Preferably, the amount of carbon-containing alloy added is 1.5-2.5 kg / t, and the mass percentage of each element in the carbon-containing alloy is: C: 35-45%, P≤0.015%, S≤0.007%, and the rest is Fe and other inevitable components; the amount of metallic aluminum added is 1.5-2.0 kg / t, and the mass percentage of each element in the metallic aluminum is: Al≥99.7%, and the rest is: The rest are Fe and other inevitable components; the addition amount of high carbon ferrochrome is 1.7-2.3kg / t, and the mass percentage of each element in high carbon ferrochrome is: Cr: 53-57%, C: 8-12%, and the rest are Fe and other inevitable components; the addition amount of silicon manganese is 4.5-6.5kg / t, and the mass percentage of each element in silicon manganese is: Si: 18-23%, Mn: 67-70%, P≤0.018%, S≤0.012%, and the rest are Fe and other inevitable components.

[0015] When 90% of the steel is tapped, lime and calcium aluminosilicate synthetic slag are added. Preferably, the amount of lime added is 2.5-3.5 kg / t, and the components in the lime are calculated by mass percentage as follows: CaO ≥ 95%, and other inevitable components; the amount of calcium aluminosilicate synthetic slag added is 6-8 kg / t, and the components of the calcium aluminosilicate synthetic slag are calculated by mass percentage as follows: CaO: 45-55%, Al2O3: 35-45%, SiO2 ≤ 5%, MgO: 3-6%, and the rest are inevitable components; All alloy, lime and calcium aluminosilicate synthetic slag are added before steel tapping is completed. The ladle bottom blowing and stirring are turned on during the whole steel tapping process. The bottom blowing flow rate is set to 200-400NL / min. The ladle bottom blowing is turned off after steel tapping is completed. Stir for another 3-5 minutes and then transport to LF for refining treatment. In the converter steelmaking process, carbon-containing alloys are first deoxidized and alloyed to further reduce the oxygen content of the molten steel. At the same time, it avoids boiling the molten steel directly with carbon powder. However, it can also produce a large amount of CO2 gas, strengthen the stirring of the molten steel, close the bottom blowing of the ladle, and save argon.

[0016] Step S4: LF refining, LF refining station, set the bottom blowing flow rate to 200-300NL / min; start the ladle bottom blowing and stirring, power on to increase the temperature, and take samples to measure the chemical composition of the molten steel and slag. After the molten steel and slag components are tested, add alloy and carbon powder to fine-tune the molten steel composition according to the target composition of the titanium-containing, boron-containing, and aluminum-killed cold heading steel grade, so that the molten steel composition reaches the target composition. At this time, set the bottom blowing flow rate to 250-350NL / min; at the same time, add lime, calcium carbide, and calcium aluminate slag deoxidizer to adjust the slag composition, set the bottom blowing flow rate to 150-200NL / min, and after the molten steel temperature, composition, and slag composition reach the target, add ferrotitanium to make the Ti element content reach the target composition, and weakly stir for 3-5m in, then add ferroboron, and set the bottom blowing flow rate to 100-150NL / min when adding ferrotitanium and ferroboron; after weak stirring for 3-5 minutes, carry out calcium treatment, feed silicon-calcium wire during calcium treatment, and the wire feeding rate is 5-8m / s. The outlet of the silicon-calcium wire of the wire feeding machine is ≤20cm away from the slag surface of the ladle. After the calcium treatment, adjust the bottom blowing of the ladle to the soft stirring mode, and the soft stirring is ≥15min. After the soft stirring is completed, the molten steel is transported to the continuous casting pouring; here, the bottom blowing flow rate is set to 80-100NL / min during weak stirring, the bottom blowing flow rate is set to 80-100NL / min during weak stirring, the bottom blowing flow rate is set to 150-200NL / min during calcium treatment, and the bottom blowing flow rate is set to 20-60NL / min during soft stirring.

[0017] Similarly, the present application defines the various components and addition amounts in the LF refining process. Specifically, the amount of lime added is 1.0-2.5kg / t, the amount of calcium carbide added is 0.8-1.5kg / t, and the amount of calcium aluminate slag deoxidizer added is 1.5-2.5kg / t; the components in the lime are calculated by mass percentage as follows: CaO ≥ 95%, and other inevitable components; the components in the calcium carbide are calculated by mass percentage as follows: CaC2 ≥ 95, and other inevitable components; the components in the calcium aluminate slag deoxidizer are calculated by mass percentage as follows: CaO: 45-55%, Al2O3: 20-30%, metallic aluminum 10-20%, metallic calcium 5-10%, SiO2 ≤ 3%, and other inevitable components; 1-1.5m / t of silicon calcium wire is fed, the Ca content is 25-35%, and the rest are Si and inevitable impurity components.

[0018] In the converter steel-making and refining process of step S3 and step S4, calcium carbide, slag deoxidizer and the like are used to strongly deoxidize the slag to produce ultra-high basicity and extremely low oxidation slag, and then titanium iron and boron iron are added for alloying to greatly reduce the oxidation amount of the two alloy elements, and then calcium treatment is performed to modify the inclusions and protect the easily oxidized elements in the molten steel.

[0019] After LF refining in step S4, the slag basicity obtained at the end is ≥30, the (CaO / Al2O3) C / A ratio is 1.8-2.2, and the T.Fe+MnO content is ≤0.8%.

[0020] Step S5: continuous casting to form titanium-containing, boron-containing, and aluminum-killed cold heading steel.

[0021] During continuous casting protective pouring, a three-layer middle-layer covering agent is used in the continuous casting process, and the thickness of each layer of the covering agent is ≥15mm; the first layer is a calcium aluminate covering agent, and the components are calculated by mass percentage as follows: CaO: 50-55%, Al2O3: 25-35%, MgO: 3-6%, Na2O: 2-5%, and other inevitable components; the second layer is fine lime powder, with a particle size of 1-3mm accounting for ≥90%, and a maximum particle size of 6mm; the third layer is carbonized rice husk, and the components are calculated by mass percentage as follows: SiO2≥85%, and the rest are C and other inevitable components.

[0022] During the continuous casting process, it should also be noted that the sliding nozzle at the bottom of the ladle usually refers to the long water buckle of the large ladle and the connection part of the submerged nozzle. One end of the long water nozzle of the large ladle is connected to the lower nozzle of the sliding nozzle at the bottom of the ladle, and the other end is inserted into the molten steel in the tundish, which plays a role in guiding the molten steel and preventing the secondary oxidation and splashing of the molten steel. The submerged nozzle is connected between the tundish and the crystallizer to guide the molten steel in the tundish into the crystallizer. In the process of pouring molten steel from the ladle to the tundish, the opening and closing of the sliding nozzle at the bottom of the ladle controls the outflow of molten steel, and the long water nozzle of the large ladle is closely connected with the lower nozzle of the sliding nozzle to ensure that the molten steel can smoothly flow from the ladle through the long water nozzle into the tundish. Therefore, the long water nozzle buckle of the large ladle and the connection part of the submerged nozzle are closely connected with the relevant parts of the lower nozzle of the sliding nozzle at the bottom of the ladle, which is an important connection and transition area in the process of molten steel pouring. Preferably, the large-package long water buckle and the immersed water inlet connection parts are all sealed with argon gas, and the argon gas flow rate is ≥15NL / min.

[0023] By combining fine control of bottom blowing in each refining operation, multi-layer protective slag in the continuous casting process and argon seal protective pouring and other measures, high-purity and high-casting molten steel was finally obtained. The further formed titanium-boron-aluminum killed cold heading steel fully met the expected results, including the following chemical compositions in mass percentage: C: 0.30-0.40%, Si: 0.10-0.20%, Mn: 0.45-0.60%, Alt: 0.010-0.045%, P≤0.018%, S≤0.012%, Cr: 0.10-0.20%, Ti: 0.015-0.055%, B: 0.0010-0.0030%, Ni≤0.03%, As≤0.02%, Cu≤0.03%, as well as Fe and other inevitable components.

[0024] It will be understood by those skilled in the art that, unless otherwise defined, all terms (including technical and scientific terms) used herein have the same meaning as generally understood by those skilled in the art to which this application belongs. It should also be understood that terms such as those defined in common dictionaries should be understood to have meanings consistent with the meanings in the context of the prior art, and will not be interpreted with idealized or overly formal meanings unless defined as herein.

[0025] The meaning of "and / or" described in this application means that the situations where each exists alone or both exist at the same time are included.

[0026] The term “connection” as used in this application may mean a direct connection between components or an indirect connection between components via other components.

[0027] Based on the above ideal embodiments of the present invention, the relevant staff can make various changes and modifications without departing from the technical concept of the present invention through the above description. The technical scope of the present invention is not limited to the contents of the specification, and its technical scope must be determined according to the scope of the claims.

Claims

1. A titanium-boron-aluminum killed cold heading steel, characterized in that: It includes the following chemical components in mass percentage: C: 0.30-0.40%, Si: 0.10-0.20%, Mn: 0.45-0.60%, Alt: 0.010-0.045%, P≤0.018%, S≤0.012%, Cr: 0.10-0.20%, Ti: 0.015-0.055%, B: 0.0010-0.0030%, Ni≤0.03%, As≤0.02%, Cu≤0.03%, as well as Fe and other inevitable components.

2. The refining method of titanium-containing boron-containing aluminum killed cold heading steel according to claim 1, characterized in that: The specific steps include: Step S1: KR desulfurization. The mass percentages of the elements in the molten iron after KR desulfurization are as follows: C: 4.0-4.3%, Si: 0.30-0.65%, Mn: 0.10-0.25%, P≤0.13%, S≤0.005%. The temperature after desulfurization is 1320-1380°C. Step S2: converter smelting, adding the desulfurized molten iron and clean scrap steel into the converter for smelting, with the scrap steel ratio being 10-20%. The C content in the molten steel is controlled to be ≤0.08% at the end of converter smelting, and oxygen blowing is stopped; Add carbon powder to the converter, start bottom blowing and stirring until C in the molten steel is 0.15-0.25%, O≤0.035%, while controlling P≤0.016%, S≤0.008%, and temperature≥1600℃; Step S3: tapping the converter. When 1 / 3 of the converter is tapped, alloys are added in the order of carbon alloy, metallic aluminum, high carbon ferrochrome, and silicon manganese. When 90% of the tapping is completed, lime and calcium aluminosilicate synthetic slag are added. Before the tapping is completed, all the alloys, lime, and calcium aluminosilicate synthetic slag are added. The ladle is bottom blown and stirred throughout the tapping process. After the tapping is completed, stirring is continued for a preset time, and then the steel is transported to LF for refining. Step S4: LF refining, LF refining station, start ladle bottom blowing and stirring, power on to increase temperature, and take samples to measure the chemical composition of molten steel and slag. After the molten steel and slag components are tested, add alloy and carbon powder to fine-tune the molten steel composition according to the target composition of titanium-containing, boron-containing, and aluminum-killed cold heading steel grades, so that the molten steel composition reaches the target composition. At the same time, add lime, calcium carbide, and calcium aluminate slag deoxidizer to adjust the slag composition. After the molten steel temperature, composition, and slag composition reach the target, add ferrotitanium to make the Ti element content reach the target composition. After weak stirring for 3-5 minutes, add ferroboron. After weak stirring for 3-5 minutes, perform calcium treatment. During the calcium treatment, feed silicon calcium wire. After the calcium treatment is completed, adjust the ladle bottom blowing to the soft stirring mode. After the soft stirring is completed, transport the molten steel to the continuous casting pouring; Step S5: Continuously casting and pouring to form the titanium-containing, boron-containing, and aluminum-killed cold heading steel as described in claim 1.

3. The refining method of titanium-containing boron-containing aluminum killed cold heading steel according to claim 2, characterized in that: In step S2, the added clean scrap steel includes the following chemical components in mass percentage: S content ≤ 0.008%, P content ≤ 0.015%, Ni ≤ 0.15%, Cu ≤ 0.08%, As ≤ 0.015%, and the rest is Fe and other inevitable components.

4. The refining method of titanium-containing boron-containing aluminum killed cold heading steel according to claim 2, characterized in that: In step S2, the specific process of adding carbon powder into the converter is to open four bottom blows at the bottom of the converter, of which three are argon blows with a flow rate set to 500-1000NL / min; and one is oxygen blows with a flow rate set to 2000-5000NL / min.

5. The refining method of titanium-containing boron-containing aluminum killed cold heading steel according to claim 2, characterized in that: In step S3, when 1 / 3 of the steel is tapped from the converter, the amount of carbon-containing alloy added is 1.5-2.5 kg / t, the amount of metallic aluminum added is 1.5-2.0 kg / t, the amount of high-carbon ferrochrome added is 1.7-2.3 kg / t, and the amount of silicon-manganese added is 4.5-6.5 kg / t; When the steel is 90% tapped, the amount of lime added is 2.5-3.5kg / t, and the amount of calcium silicate synthetic slag added is 6-8kg / t; The ladle bottom blowing and stirring are turned on throughout the steel tapping process, and the bottom blowing flow rate is set to 200-400NL / min. After the steel tapping is completed, stirring is continued for 3-5 minutes before transportation to refining treatment.

6. The refining method of titanium-containing boron-containing aluminum killed cold heading steel according to claim 5, characterized in that: In step S3, the mass percentages of the elements in the carbon-containing alloy are: C: 35-45%, P≤0.015%, S≤0.007%, and the rest are Fe and other inevitable components; The mass percentage of each element in metallic aluminum is: Al ≥ 99.7%, the rest is Fe and other inevitable components; The mass percentages of the elements in high carbon ferrochrome are: Cr: 53-57%, C: 8-12%, and the rest are Fe and other inevitable components; The mass percentage of each element in silicon manganese is: Si: 18-23%, Mn: 67-70%, P≤0.018%, S≤0.012%, and the rest is Fe and other inevitable components; The components of lime are calculated by mass percentage as follows: CaO ≥ 95%, and other inevitable components; The components of calcium aluminosilicate synthetic slag are calculated by mass percentage as follows: CaO: 45-55%, Al2O3: 35-45%, SiO2≤5%, MgO: 3-6%, and the rest are inevitable components.

7. The refining method of titanium-containing boron-containing aluminum killed cold heading steel according to claim 2, characterized in that: In step S4, after the LF refining enters the station, the ladle bottom blowing and stirring are turned on, and the bottom blowing flow rate is set to 200-300NL / min; When adding alloy and carbon powder to fine-tune the composition of molten steel, set the bottom blowing flow rate to 250-350NL / min; When adding lime, calcium carbide, and calcium aluminate slag deoxidizer to adjust the slag composition, set the bottom blowing flow rate to 150-200NL / min; When adding ferrotitanium and ferroboron, set the bottom blowing flow rate to 100-150NL / min; When weak stirring is used, the bottom blowing flow rate is set to 80-100NL / min; During calcium treatment, the bottom blowing flow rate is set to 150-200NL / min; During soft stirring, the bottom blowing flow rate is set to 20-60NL / min.

8. The refining method of titanium-containing boron-containing aluminum killed cold heading steel according to claim 2, characterized in that: In step S4, the amount of lime added is 1.0-2.5 kg / t, the amount of calcium carbide added is 0.8-1.5 kg / t, and the amount of calcium aluminate slag deoxidizer added is 1.5-2.5 kg / t; The components of lime are calculated by mass percentage as follows: CaO ≥ 95%, and other inevitable components; The components in calcium carbide are calculated by mass percentage as follows: CaC2 ≥ 95, and other inevitable components; The components of calcium aluminate slag deoxidizer are calculated by mass percentage as follows: CaO: 45-55%, Al2O3: 20-30%, metal aluminum 10-20%, metal calcium 5-10%, SiO2≤3%, and other inevitable components; During calcium treatment, 1-1.5 m / t of silicon-calcium wire is fed, the Ca content is 25-35%, and the rest is Si and unavoidable impurities; the wire feeding rate during calcium treatment is set to 5-8 m / s, the outlet of the silicon-calcium wire of the wire feeding machine is ≤20 cm away from the slag surface of the ladle, and the soft stirring is ≥15 min after the calcium treatment.

9. The refining method of titanium-containing boron-containing aluminum killed cold heading steel according to claim 8, characterized in that: In step S4, the slag basicity obtained after refining is ≥30, the (CaO / Al2O3) C / A ratio is 1.8-2.2, and the T.Fe+MnO content is ≤0.8%.

10. The refining method of titanium-containing boron-containing aluminum killed cold heading steel according to claim 2, characterized in that: In step S5, a three-layer middle-layer covering agent is used in the continuous casting process, and the thickness of each layer of the covering agent is ≥15 mm; The first layer is a calcium aluminate covering agent, and the components by mass percentage are: CaO: 50-55%, Al2O3: 25-35%, MgO: 3-6%, Na2O: 2-5%, and other inevitable components; The second layer is fine lime powder, with a particle size of 1-3mm accounting for ≥90% and a maximum particle size of 6mm; The third layer is carbonized rice husk, and the mass percentage of each component is: SiO2 ≥ 85%, and the rest is C and other inevitable components.