Monomolecular array chip based on high-entropy alloy plasmon and preparation method thereof
By depositing high-entropy alloy coating materials on single-molecular array chips, the signal-to-noise ratio is improved, the problem of low signal-to-noise ratio in the prior art is solved, and higher detection accuracy and reliability are achieved, especially in single-molecule Immune analysis.
Patent Information
- Application Number
- CN202411141726.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-20
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2044-08-20
AI Technical Summary
The signal-to-noise of a single-molecule array chip is relatively low, which affects the accuracy and reliability of detection. It is especially difficult to accurately extract the target signal in single-molecule immune analysis, which limits its application breadth and accuracy.
Single-molecular array chip preparation method using high-entropy alloy plasmons, by depositing high-entropy alloy coating materials, including precious metal composite materials and synergistic composite metal materials on the substrate chip, using thermal evaporation thin film deposition and magnetron sputtering coating Technology, combined with the plasma cleaning step, a high entropy alloy film with a thickness of 80 to 120 nm is formed.
The signal-to-noise ratio of single-molecular array chips is significantly improved, the accuracy and reliability of single-molecular immunoassays are enhanced, and the detection sensitivity is improved by about 2 orders of magnitude.
Smart Images

Figure CN119020729A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of biological detection chips, in particular to the production technology of single molecule immune detection chips. Background Art
[0002] Single Molecule Array (SiMoA) technology is a method that uses single molecule counting to detect trace biomarkers. The detection limit of this technology can reach the order of femtogram (fg / mL), and it is currently the most representative single molecule immunoassay technology. The system is derived from a detection system developed by David Walt and David Duffy's team. Its detection principle is similar to digital PCR, and both are achieved through single molecule isolation combined with single molecule level signal amplification through a microreactor unit.
[0003] This technology is a single-molecule immunoassay based on a microarray chip. It is to carve (or cast) thousands of micron-scale microwells on a millimeter-scale chip, with each microwell volume of about 40 fl (i.e., a single-molecule array chip). Then, the immune complex magnetic beads are distributed in the microwells, and the fluorescent spots are counted with the help of a high-resolution fluorescence microscope. Based on the Poisson distribution theory, the ratio of the number of wells containing beads and fluorescent products at the same time to the total number of wells containing beads is calculated to determine the concentration of the detected substance in the test sample. The operation process is roughly as follows:
[0004] (1) using magnetic beads labeled with capture antibodies to capture antigens in the sample;
[0005] (2) labeling the captured antigen using a biotinylated detection antibody;
[0006] (3) adding streptavidin-galactosidase complex to bind to biotin on the detection antibody;
[0007] (4) The washed magnetic beads are mixed with the substrate and loaded into a single molecule array chip. The magnetic field is used to make the magnetic beads fall into microwells that are perfectly matched to their size, and an oil phase is added to physically isolate the microwells.
[0008] (5) The microwell containing galactosidase produces fluorescent products due to the catalysis of the substrate by the enzyme molecules;
[0009] (6) Performing fluorescence imaging on the microwell array and achieving quantitative detection by comparing the number of microwells emitting fluorescent signals with a standard curve.
[0010] One of the main problems with this technology is the low sensitivity of its single array signal, which directly affects the accuracy and reliability of detection. In practical applications, especially in single-molecule immunoassays, it is necessary to detect and analyze extremely small amounts of molecules. However, the signal-to-noise ratio of single-molecule array chips in the prior art is poor, which makes it difficult to accurately extract the target signal from the background noise, limiting its application breadth and accuracy in biomolecule detection. Summary of the invention
[0011] In order to improve the signal-to-noise ratio of a single-molecule array chip and further improve the accuracy and reliability of the technology in single-molecule immunoassay, the present invention provides a single-molecule array chip based on high-entropy alloy plasmons and a preparation method thereof.
[0012] The technical solution adopted by the present invention is: a method for preparing a single-molecule array chip based on high-entropy alloy plasmons, characterized in that: the production raw materials include a substrate chip and a high-entropy alloy coating material; the high-entropy alloy coating material is composed of a precious metal composite material and a synergistic composite metal material in a mass ratio of 1:0.12 to 3.75; the precious metal composite material is composed of gold and silver in a mass ratio of 1:0.08 to 3; the synergistic composite metal material is composed of ruthenium and palladium in a mass ratio of 1:0.2 to 1.5.
[0013] As a further improvement of the present invention, the step of forming a high entropy alloy film on the substrate chip to obtain a coated chip is also included. More preferably, the thickness of the high entropy alloy film of the coated chip is 80-120 nm.
[0014] As a further improvement of the present invention, the base chip is selected from any one of a silicon single crystal substrate base chip, a FZ single crystal silicon wafer, a CZ single crystal silicon wafer, a semi-insulating single crystal silicon wafer, and an ultra-high purity single crystal silicon wafer.
[0015] The above-mentioned coated chip can be obtained by depositing the high entropy alloy coating material on the substrate chip through thermal evaporation thin film deposition technology, or by depositing the high entropy alloy coating material on the substrate chip through magnetron sputtering coating technology.
[0016] If thermal evaporation thin film deposition technology is used for coating, the following specific steps can be followed:
[0017] S1. Surface treatment of the substrate chip is performed by ultrasonic cleaning or argon plasma cleaning to remove residual organic matter and oxides;
[0018] S2, placing the high entropy alloy coating material in the vacuum chamber of the thermal evaporation coating machine, placing the substrate chip on the rotary coating table, controlling the rotation speed to 20-50 rpm, and the vacuum degree to 10 -6 ~10 -7torr, the heating temperature is 500-600℃ to start the thermal evaporation film deposition; during the deposition process, the deposition rate is measured in real time by a quartz crystal microbalance, and the evaporation rate is adjusted by adjusting the heating power and the evaporation source temperature to control the deposition rate within
[0019] S3. The sample is released by gradually increasing the ambient pressure or opening the gas inlet valve to restore the atmospheric pressure and obtain a coated chip.
[0020] The above steps can ensure uniform and high-quality deposition of the metal film on the substrate surface, providing a reliable basis for the subsequent preparation of the single-molecule array chip.
[0021] As a further improvement of the present invention, the method further includes the step of plasma cleaning the coated chip.
[0022] The parameters of the above plasma cleaning can be set as follows: use high-purity oxygen as the cleaning gas, set the gas pressure to 0.1-1 mTorr, the gas flow rate to 5-20 sccm, the RF power to 100-500 W, and the cleaning time to 5-30 min.
[0023] The present invention also discloses a single-molecule array chip based on high-entropy alloy plasmons, which is prepared by the preparation method of the single-molecule array chip based on high-entropy alloy plasmons of the present invention.
[0024] The beneficial effect of the present invention is that the single-molecule array chip based on high-entropy alloy plasmon prepared by the method of the present invention can significantly improve the signal-to-noise ratio of the single-molecule array chip, and further improve the accuracy and reliability of the technology in single-molecule immunoassay. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 This is a morphology image of the single molecule array chip of Example 1 under an atomic force microscope (AFM). DETAILED DESCRIPTION
[0026] The present invention is further described below in conjunction with embodiments.
[0027] Embodiment 1:
[0028] Prepare the single molecule array chip as follows:
[0029] (1) A high entropy alloy coating material is prepared according to a mass ratio of a precious metal composite material to a synergistic composite metal material of 1:2, wherein the precious metal composite material is composed of gold and silver in a mass ratio of 1:1.4, and the synergistic composite metal material is composed of ruthenium and palladium in a mass ratio of 1:1.
[0030] (2) Using ultrasonic cleaning to treat the surface of the substrate chip (silicon single crystal substrate substrate chip, cut from 4 inches, thickness 525 μm) to remove residual organic matter and oxides;
[0031] (3) Place the above high entropy alloy coating material in the vacuum chamber of the thermal evaporation coating machine, place the substrate chip on the rotary coating table, control the rotation speed to 30 rpm, and the vacuum degree to 10 -6 torr, the heating temperature was 600℃ to start the thermal evaporation film deposition; during the deposition process, the deposition rate was measured in real time by a quartz crystal microbalance, and the evaporation rate was adjusted by adjusting the heating power and the evaporation source temperature to control the deposition rate within When the thickness of the high entropy alloy film of the coated chip reaches 100 nm, the gas inlet valve is opened to restore the atmospheric pressure to release the sample to obtain the coated chip.
[0032] (4) Use a plasma cleaning machine (CPC-G / Gplus) to clean the coated chip. Use high-purity oxygen (oxygen purity ≥ 99.995%) as the cleaning gas. Set the gas pressure to 0.5 mTorr, the gas flow rate to 12 sccm, the RF power to 200 W, and the cleaning time to 25 min. After the cleaning is completed, gradually restore the atmospheric pressure to complete the treatment, and obtain a single molecule array chip.
[0033] The surface morphology of the single molecule array chip was observed using an atomic force microscope (AFM). Figure 1 shown.
[0034] Embodiment 2:
[0035] Prepare the single molecule array chip as follows:
[0036] (1) A high entropy alloy coating material is prepared according to a mass ratio of a precious metal composite material to a synergistic composite metal material of 1:3.5, wherein the precious metal composite material is composed of gold and silver in a mass ratio of 1:1, and the synergistic composite metal material is composed of ruthenium, palladium and platinum in a mass ratio of 1:0.5.
[0037] (2) Argon plasma cleaning is used to treat the surface of the substrate chip (silicon single crystal substrate substrate chip, cut from 4 inches, thickness 525 μm) to remove residual organic matter and oxides;
[0038] (3) Place the above high entropy alloy coating material in the vacuum chamber of the thermal evaporation coating machine, place the substrate chip on the rotary coating table, control the speed to 35 rpm, and the vacuum degree to 10 -7 torr, the heating temperature was 520℃ to start the thermal evaporation film deposition; during the deposition process, the deposition rate was measured in real time by a quartz crystal microbalance, and the evaporation rate was adjusted by adjusting the heating power and the evaporation source temperature to control the deposition rate within When the thickness of the high entropy alloy film of the coated chip reaches 100 nm, the gas inlet valve is opened to restore the atmospheric pressure to release the sample to obtain the coated chip.
[0039] (4) Use a plasma cleaning machine (CPC-G / Gplus) to clean the coated chip. Use high-purity oxygen (oxygen purity ≥ 99.995%) as the cleaning gas. Set the gas pressure to 0.3 mTorr, the gas flow rate to 20 sccm, the RF power to 450 W, and the cleaning time to 15 min. After the cleaning is completed, gradually restore the atmospheric pressure to complete the treatment, and obtain a single molecule array chip.
[0040] Embodiment three:
[0041] Prepare the single molecule array chip as follows:
[0042] (1) A high entropy alloy coating material is prepared according to a mass ratio of a precious metal composite material to a synergistic composite metal material of 1:0.5, wherein the precious metal composite material is composed of gold and silver in a mass ratio of 1:0.2, and the synergistic composite metal material is composed of ruthenium and palladium in a mass ratio of 1:1.5.
[0043] (2) Using ultrasonic cleaning to treat the surface of the substrate chip (silicon single crystal substrate substrate chip, cut from 4 inches, thickness 525 μm) to remove residual organic matter and oxides;
[0044] (3) Place the above high entropy alloy coating material in the vacuum chamber of the thermal evaporation coating machine, place the substrate chip on the rotary coating table, control the speed to 20 rpm, and the vacuum degree to 10 -6 torr, the heating temperature was 500℃ to start the thermal evaporation film deposition; during the deposition process, the deposition rate was measured in real time by a quartz crystal microbalance, and the evaporation rate was adjusted by adjusting the heating power and the evaporation source temperature to control the deposition rate within When the thickness of the high entropy alloy film of the coated chip reaches 100 nm, the gas inlet valve is opened to restore the atmospheric pressure to release the sample to obtain the coated chip.
[0045] (4) Use a plasma cleaning machine (CPC-G / Gplus) to clean the coated chip. Use high-purity oxygen (oxygen purity ≥ 99.995%) as the cleaning gas. Set the gas pressure to 0.8 mTorr, the gas flow rate to 6 sccm, the RF power to 250 W, and the cleaning time to 30 min. After the cleaning is completed, gradually restore the atmospheric pressure to complete the treatment, and obtain a single molecule array chip.
[0046] Comparative Example 1:
[0047] This comparative example is a control experiment of Example 1, and is implemented according to the same steps and conditions as Example 1, except that the step of coating the substrate chip is not included. The specific implementation steps are as follows:
[0048] (1) Using ultrasonic cleaning to treat the surface of the substrate chip (from the same batch as in Example 1, silicon single crystal substrate substrate chip, cut from 4 inches, with a thickness of 525 μm) to remove residual organic matter and oxides;
[0049] (2) The above chip was cleaned using a plasma cleaning machine (CPC-G / Gplus). High-purity oxygen (oxygen purity ≥ 99.995%) was used as the cleaning gas. The gas pressure was set to 0.5 mTorr, the gas flow rate was 12 sccm, the RF power was 200 W, and the cleaning time was 25 min. After the cleaning was completed, the atmospheric pressure was gradually restored to complete the treatment, and a single molecule array chip was obtained.
[0050] Comparative Example 2:
[0051] This comparative example is a control experiment of Example 1, and is implemented according to the same steps and conditions as Example 1, except that the step of plasma cleaning the coated chip is not included. The specific implementation steps are as follows:
[0052] (1) A high entropy alloy coating material is prepared according to a mass ratio of a precious metal composite material to a synergistic composite metal material of 1:2, wherein the precious metal composite material is composed of gold and silver in a mass ratio of 1:1.4, and the synergistic composite metal material is composed of ruthenium and palladium in a mass ratio of 1:1.
[0053] (2) Using ultrasonic cleaning to treat the surface of the substrate chip (from the same batch as in Example 1, silicon single crystal substrate substrate chip, cut from 4 inches, with a thickness of 525 μm) to remove residual organic matter and oxides;
[0054] (3) Place the above high entropy alloy coating material in the vacuum chamber of the thermal evaporation coating machine, place the substrate chip on the rotary coating table, control the rotation speed to 30 rpm, and the vacuum degree to 10 -6 torr, the heating temperature was 600℃ to start the thermal evaporation film deposition; during the deposition process, the deposition rate was measured in real time by a quartz crystal microbalance, and the evaporation rate was adjusted by adjusting the heating power and the evaporation source temperature to control the deposition rate within When the thickness of the high entropy alloy film on the coated chip reaches 100 nm, the gas inlet valve is opened to restore the atmospheric pressure to release the sample to obtain a single molecule array chip.
[0055] Comparative Example 3:
[0056] This comparative example is a control experiment of Example 1, and is implemented according to the same steps and conditions as Example 1, with the only difference being that: under the premise that the total thickness of the coating remains unchanged, the coating material only uses the precious metal composite material. The specific implementation steps are as follows:
[0057] (1) The coating material is a precious metal composite material, wherein the precious metal composite material is composed of gold and silver in a mass ratio of 1:1.4.
[0058] (2) Using ultrasonic cleaning to treat the surface of the substrate chip (from the same batch as in Example 1, silicon single crystal substrate substrate chip, cut from 4 inches, with a thickness of 525 μm) to remove residual organic matter and oxides;
[0059] (3) Place the above-mentioned precious metal composite material in the vacuum chamber of a thermal evaporation coating machine, place the substrate chip on a rotary coating table, control the rotation speed to 30 rpm, and the vacuum degree to 10 -6 torr, the heating temperature was 600℃ to start the thermal evaporation film deposition; during the deposition process, the deposition rate was measured in real time by a quartz crystal microbalance, and the evaporation rate was adjusted by adjusting the heating power and the evaporation source temperature to control the deposition rate within When the thickness of the precious metal film of the coated chip reaches 100 nm, the gas inlet valve is opened to restore the atmospheric pressure to release the sample to obtain the coated chip.
[0060] (4) Use a plasma cleaning machine (CPC-G / Gplus) to clean the coated chip. Use high-purity oxygen (oxygen purity ≥ 99.995%) as the cleaning gas. Set the gas pressure to 0.5 mTorr, the gas flow rate to 12 sccm, the RF power to 200 W, and the cleaning time to 25 min. After the cleaning is completed, gradually restore the atmospheric pressure to complete the treatment, and obtain a single molecule array chip.
[0061] Comparative Example 4:
[0062] This comparative example is a control experiment of Example 1, and is implemented according to the same steps and conditions as Example 1, with the only difference being that, under the premise that the total thickness of the coating remains unchanged, the coating material only uses the synergistic composite metal material. The specific implementation steps are as follows:
[0063] (1) The coating material is a synergistic composite metal material, and the synergistic composite metal material is composed of ruthenium and palladium in a mass ratio of 1:1.
[0064] (2) Using ultrasonic cleaning to treat the surface of the substrate chip (from the same batch as in Example 1, silicon single crystal substrate substrate chip, cut from 4 inches, with a thickness of 525 μm) to remove residual organic matter and oxides;
[0065] (3) Place the above high entropy alloy coating material in the vacuum chamber of the thermal evaporation coating machine, place the substrate chip on the rotary coating table, control the rotation speed to 30 rpm, and the vacuum degree to 10 -6 torr, the heating temperature was 600℃ to start the thermal evaporation film deposition; during the deposition process, the deposition rate was measured in real time by a quartz crystal microbalance, and the evaporation rate was adjusted by adjusting the heating power and the evaporation source temperature to control the deposition rate within When the thickness of the high entropy alloy film of the coated chip reaches 100 nm, the gas inlet valve is opened to restore the atmospheric pressure to release the sample to obtain the coated chip.
[0066] (4) Use a plasma cleaning machine (CPC-G / Gplus) to clean the coated chip. Use high-purity oxygen (oxygen purity ≥ 99.995%) as the cleaning gas. Set the gas pressure to 0.5 mTorr, the gas flow rate to 12 sccm, the RF power to 200 W, and the cleaning time to 25 min. After the cleaning is completed, gradually restore the atmospheric pressure to complete the treatment, and obtain a single molecule array chip.
[0067] Comparative Example 5:
[0068] This comparative example is a control experiment of Example 1, and is implemented according to the same steps and conditions as Example 1, with the only difference being that the synergistic composite metal material is all made of ruthenium (the mass ratio of the precious metal composite material to the synergistic composite metal material remains unchanged). The specific implementation steps are as follows:
[0069] (1) A high entropy alloy coating material is prepared according to a mass ratio of a precious metal composite material to a synergistic composite metal material of 1:2, wherein the precious metal composite material is composed of gold and silver in a mass ratio of 1:1.4, and the synergistic composite metal material is ruthenium.
[0070] (2) Using ultrasonic cleaning to treat the surface of the substrate chip (from the same batch as in Example 1, silicon single crystal substrate substrate chip, cut from 4 inches, with a thickness of 525 μm) to remove residual organic matter and oxides;
[0071] (3) Place the above high entropy alloy coating material in the vacuum chamber of the thermal evaporation coating machine, place the substrate chip on the rotary coating table, control the rotation speed to 30 rpm, and the vacuum degree to 10 -6 torr, the heating temperature was 600℃ to start the thermal evaporation film deposition; during the deposition process, the deposition rate was measured in real time by a quartz crystal microbalance, and the evaporation rate was adjusted by adjusting the heating power and the evaporation source temperature to control the deposition rate within When the thickness of the high entropy alloy film of the coated chip reaches 100 nm, the gas inlet valve is opened to restore the atmospheric pressure to release the sample to obtain the coated chip.
[0072] (4) Use a plasma cleaning machine (CPC-G / Gplus) to clean the coated chip. Use high-purity oxygen (oxygen purity ≥ 99.995%) as the cleaning gas. Set the gas pressure to 0.5 mTorr, the gas flow rate to 12 sccm, the RF power to 200 W, and the cleaning time to 25 min. After the cleaning is completed, gradually restore the atmospheric pressure to complete the treatment, and obtain a single molecule array chip.
[0073] Comparative Example 6:
[0074] This comparative example is a control experiment of Example 1, and is implemented according to the same steps and conditions as Example 1, with the only difference being that the synergistic composite metal material is all palladium (the mass ratio of the precious metal composite material and the synergistic composite metal material remains unchanged). The specific implementation steps are as follows:
[0075] (1) A high entropy alloy coating material is prepared according to a mass ratio of a precious metal composite material to a synergistic composite metal material of 1:2, wherein the precious metal composite material is composed of gold and silver in a mass ratio of 1:1.4, and the synergistic composite metal material is palladium.
[0076] (2) Using ultrasonic cleaning to treat the surface of the substrate chip (from the same batch as in Example 1, silicon single crystal substrate substrate chip, cut from 4 inches, with a thickness of 525 μm) to remove residual organic matter and oxides;
[0077] (3) Place the above high entropy alloy coating material in the vacuum chamber of the thermal evaporation coating machine, place the substrate chip on the rotary coating table, control the rotation speed to 30 rpm, and the vacuum degree to 10 -6 torr, the heating temperature was 600℃ to start the thermal evaporation film deposition; during the deposition process, the deposition rate was measured in real time by a quartz crystal microbalance, and the evaporation rate was adjusted by adjusting the heating power and the evaporation source temperature to control the deposition rate within When the thickness of the high entropy alloy film of the coated chip reaches 100 nm, the gas inlet valve is opened to restore the atmospheric pressure to release the sample to obtain the coated chip.
[0078] (4) Use a plasma cleaning machine (CPC-G / Gplus) to clean the coated chip. Use high-purity oxygen (oxygen purity ≥ 99.995%) as the cleaning gas. Set the gas pressure to 0.5 mTorr, the gas flow rate to 12 sccm, the RF power to 200 W, and the cleaning time to 25 min. After the cleaning is completed, gradually restore the atmospheric pressure to complete the treatment, and obtain a single molecule array chip.
[0079] Bioanalysis experiments of low-abundance substances:
[0080] The magnetic beads were modified with Tau217 primary antibody, and the Tau-217 secondary antibody was modified with NHS-Fitc. The Tau-217 antigen of different concentrations was captured by one-step method and sandwich method. After capture, the complex was dropped on the single molecule array chip for single molecule signal number statistical analysis. The specific experimental method is as follows:
[0081] 1. Experimental materials:
[0082] The single molecule array chips prepared in Examples 1 to 3 and Comparative Examples 1 to 6;
[0083] Tau217 primary antibody: antibody used to modify magnetic beads;
[0084] NHS-FITC: fluorescent dye used to modify Tau217 secondary antibody;
[0085] Tau217 antigen: target molecule for capture;
[0086] Magnetic beads: used to modify Tau217 primary antibody;
[0087] PBS buffer: used for dilution and washing.
[0088] 2. Experimental steps:
[0089] 1. Modification of magnetic beads:
[0090] (1) Dilute the Tau217 primary antibody to a final concentration of 10 μg / mL;
[0091] (2) Add Tau217 primary antibody to the magnetic beads, the reaction temperature is 25°C, and the reaction time is 1 hour;
[0092] 2. Modification of Tau217 secondary antibody:
[0093] (1) Dissolve NHS-FITC in PBS buffer at a concentration of 1 mg / mL;
[0094] (2) adding NHS-FITC to the Tau217 secondary antibody to form a Tau217 secondary antibody-NHS-FITC complex, the reaction temperature was 25°C, and the reaction time was 2 hours;
[0095] 3. Capture target molecules:
[0096] Using a one-step method, different concentrations of Tau217 antigen solutions (0.1 pg / mL, 0.5 pg / mL, 1 pg / mL, 10 pg / mL, 100 pg / mL, 1 ng / mL) were added to the modified magnetic beads. The reaction temperature was 4 °C and the reaction time was 12 h.
[0097] 4. Application of composites:
[0098] The captured Tau217 antigen complex was dropped onto the single-molecule array chip, using 10 μL of complex solution for each chip;
[0099] 5. Imaging analysis:
[0100] Fluorescence imaging of single-molecule array chips was performed using a fluorescence microscope (Zeiss Axio Observer);
[0101] The FITC channel (excitation wavelength: 488 nm, emission wavelength: 515 nm) was used to detect and record the fluorescence signal; the number of single-molecule signals under the capture conditions of different concentrations of Tau217 antigen solutions was counted, and the results are shown in Table 1.
[0102] Table 1 Statistics of single molecule signal numbers under capture conditions of different concentrations of Tau217 antigen solutions
[0103]
[0104] It can be seen from the detection results of Examples 1 to 3 in Table 1 that the single-molecule array chip prepared by the method of the present invention can generate stable single-molecule signals under the capture conditions of Tau217 antigen solution with a concentration of 0.1 pg / mL to 1 ng / mL, and has the advantages of high detection sensitivity and stable signal intensity.
[0105] From the comparison of the detection results of Example 1 and Comparative Example 1 in Table 1, it can be seen that, compared with the common single-molecule array chip without metal coating, the single-molecule array chip of the present invention has significantly higher signal intensity and the sensitivity is improved by about 2 orders of magnitude.
[0106] From the comparison between Example 1 and Comparative Example 2 in Table 1, it can be seen that the single molecule signal intensity can be significantly improved by the plasma cleaning step of the present invention.
[0107] From the comparison of Example 1, Comparative Example 3 and Comparative Example 4 in Table 1, it can be seen that, under the premise that the coating thickness is exactly the same, the single-molecule signal intensity captured by the Tau217 antigen solution of different concentrations in Example 1 is significantly higher than that of Comparative Example 3 using only the precious metal coating and Comparative Example 4 using only the synergistic composite metal coating. It can be seen that the precious metal composite material and the synergistic composite metal material of the present invention have a significant synergistic effect in improving the single-molecule signal intensity.
[0108] From the comparison of Example 1, Comparative Example 5 and Comparative Example 6 in Table 1, it can be seen that under the conditions that the coating thickness is exactly the same and the mass ratio of the precious metal composite material and the synergistic metal material is also the same, the single-molecule signal intensity captured by the Tau217 antigen solution of different concentrations in Example 1 is significantly higher than that of Comparative Example 5 using ruthenium alone as the synergistic metal material and Comparative Example 6 using palladium alone as the synergistic metal material. It can be seen that the components of the synergistic composite metal material of the present invention have a significant synergistic effect in improving the single-molecule signal intensity.
Claims
1. A method for preparing a single-molecule array chip based on high entropy alloy plasmons, characterized in that: The production raw materials include a substrate chip and a high-entropy alloy coating material; the high-entropy alloy coating material is composed of a precious metal composite material and a synergistic composite metal material in a mass ratio of 1:0.12 to 3.75; the precious metal composite material is composed of gold and silver in a mass ratio of 1:0.08 to 3; the synergistic composite metal material is composed of ruthenium and palladium in a mass ratio of 1:0.2 to 1.
5.
2. The method for preparing a single-molecule array chip based on high-entropy alloy plasmon according to claim 1, characterized in that: The method also includes the step of forming a high entropy alloy film on a substrate chip to obtain a coated chip.
3. The method for preparing a single-molecule array chip based on high-entropy alloy plasmon according to claim 2, characterized in that: The thickness of the high entropy alloy film of the coated chip is 80-120 nm.
4. The method for preparing a single-molecule array chip based on high-entropy alloy plasmon according to claim 3, characterized in that: The base chip is selected from any one of a silicon single crystal substrate base chip, a FZ single crystal silicon wafer, a CZ single crystal silicon wafer, a semi-insulating single crystal silicon wafer, and an ultra-high purity single crystal silicon wafer.
5. The method for preparing a single-molecule array chip based on high-entropy alloy plasmon according to claim 3, characterized in that: The specific preparation steps of the coated chip are: depositing the high entropy alloy coating material on the substrate chip by thermal evaporation thin film deposition technology, thereby obtaining the coated chip.
6. The method for preparing a single-molecule array chip based on high-entropy alloy plasmon according to claim 3, characterized in that: The specific preparation steps of the coated chip are: depositing the high entropy alloy coating material on the substrate chip by magnetron sputtering coating technology, thereby obtaining the coated chip.
7. The method for preparing a single-molecule array chip based on high-entropy alloy plasmon according to claim 5, characterized in that: The steps for preparing the coated chip are specifically as follows: S1. Surface treatment of the substrate chip is performed by ultrasonic cleaning or argon plasma cleaning to remove residual organic matter and oxides; S2, placing the high entropy alloy coating material in the vacuum chamber of the thermal evaporation coating machine, placing the substrate chip on the rotary coating table, controlling the rotation speed to 20-50 rpm, and the vacuum degree to 10 -6 ~10 -7 torr, the heating temperature is 500-600℃ to start thermal evaporation film deposition; During the deposition process, the deposition rate was measured in real time by a quartz crystal microbalance, and the evaporation rate was adjusted by adjusting the heating power and the evaporation source temperature to control the deposition rate within S3. The sample is released by gradually increasing the ambient pressure or opening the gas inlet valve to restore the atmospheric pressure and obtain a coated chip.
8. The method for preparing a single-molecule array chip based on high entropy alloy plasmon according to any one of claims 2 to 7, characterized in that: The method also includes the step of plasma cleaning the coated chip.
9. The method for preparing a single-molecule array chip based on high-entropy alloy plasmon according to claim 8, characterized in that: The plasma cleaning parameters are: using high-purity oxygen as the cleaning gas, setting the gas pressure to 0.1-1 mTorr, the gas flow rate to 5-20 sccm, the RF power to 100-500 W, and the cleaning time to 5-30 min.
10. A single-molecule array chip based on high-entropy alloy plasmons prepared by the method for preparing a single-molecule array chip based on high-entropy alloy plasmons according to any one of claims 1 to 9.
Citation Information
Patent Citations
Plasmon enhancement type Raman spectrum detection chip as well as detection device applying same
CN103558206A
Gene sequencing chip
CN112812954A
Mutiplexing plasmonic chip and method of manufacturing the same
KR102255110B1
Nanomagnetic detector array for biomolecular recognition
US20100188075A1
Substrate for surface-enhanced raman spectroscopy and method for producing same
US20160223467A1