Etching solution and application of etching solution in etching of more than two layers of metal films
By adding hydrogen peroxide and other specific components to the etching liquid, the damage problem of the etching liquid on the metal oxide film semiconductor in the prior art is solved, and compatibility and etching of amorphous silicon, polysilicon and metal oxide active layers are achieved. Uniformity reduces damage to the active layer and improves etching stability and boundaries.
Patent Information
- Application Number
- CN202411153800.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-21
- Publication Date
- 2024-11-26
AI Technical Summary
The existing etching liquids are severely damaged due to the low fluorine-containing compounds and pH values when etching metal oxide semiconductors. Especially when copper and molybdenum alloys are used as data transmission metal traces, it is difficult to ensure etching. Uniformity and reduce damage to the active layer.
An etching liquid is provided, containing hydrogen peroxide, chelating agent, copper corrosion inhibitor, copper etchant, molybdenum alloy etchant and metal oxide damage inhibitor. Through the mutual cooperation of these components, the etching rate and stability are adjusted, and it is compatible with non- The crystalline silicon, polysilicon and metal oxide active layers reduce damage to the active layer and are suitable for etching of more than two metal films.
The compatibility and damage to the active layer are reduced when etching copper and molybdenum alloys are achieved, ensuring etching uniformity and stability, improving process boundaries, reducing corrosion to metal traces and damage to the active layer.
Smart Images

Figure CN119020787A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of etching liquid, in particular to an etching liquid and an application of the etching liquid in etching more than two layers of metal films. Background Art
[0002] The process of forming the fine circuits of a thin film transistor liquid crystal display (TFT-LCD) is to uniformly apply photoresist on a conductive metal film such as aluminum (Al), aluminum alloy, copper (Cu) and alloys containing copper, or an insulating film such as an oxide silicon film or a nitride silicon film formed on the panel, then illuminate it through a mask printed with a circuit pattern, develop it, make the photoresist into the desired circuit pattern, then transfer the circuit pattern to the metal film or insulating film under the photoresist by dry or wet etching, and finally use a stripping process to remove unnecessary photoresist through a series of flat-panel printing technologies.
[0003] The gate and data transmission metal wiring of large-size displays uses copper metal, which has lower impedance and no environmental problems than the previous aluminum and chromium. However, copper has poor adhesion to glass film and silicon, and it is necessary to prevent Cu from diffusing into the silicon layer, so a variety of barrier metals are used, among which molybdenum or molybdenum alloy is the most popular barrier metal. To make up for the above-mentioned shortcomings of copper wiring, copper is used as the main metal film, and the barrier metal is a multi-layer structure metal film using molybdenum or molybdenum alloy as the buffering metal film. The bottom of the data transmission metal wiring is the active layer, which can be amorphous silicon, polycrystalline silicon, or single crystal silicon according to the product. Recently, metal oxide semiconductor materials are also used for production.
[0004] When a metal oxide film semiconductor is used as the active layer, the existing etching solution contains fluorine compounds and has a pH value of about 2, which will cause serious damage to the metal oxide film semiconductor.
[0005] In view of this, it is particularly necessary to develop an etching solution that is suitable for using copper film and molybdenum alloy film as data transmission metal wiring, which can ensure etching uniformity when etching a large area and reduce damage to amorphous silicon, polycrystalline silicon and metal oxide semiconductors as the underlying active layer. Summary of the invention
[0006] The purpose of the present invention is to provide an etching solution and the application of the etching solution in etching more than two metal films, and to provide an etching solution applicable to amorphous silicon thin film transistors, low temperature polysilicon thin film transistors and metal oxide semiconductor thin film transistors.
[0007] The present invention is achieved in that:
[0008] In a first aspect, the present invention provides an etching solution comprising the following components:
[0009] H2O2 16.00wt%-24.00wt%;
[0010] Chelating agent 1.00wt%-5.00wt%;
[0011] Copper corrosion inhibitor 0.01wt%-2.50wt%;
[0012] Copper etchant 0.10wt%-4.00wt%;
[0013] Molybdenum alloy etchant 0.01wt%-3.00wt%;
[0014] Metal oxide damage inhibitor 0.01wt%-3.00wt%;
[0015] The remaining amount of water.
[0016] The etching solution of the present invention uses hydrogen peroxide as the main oxidant, which can provide hydrogen ions and adjust the etching rate. The etching solution of the present invention is compatible with active layers such as amorphous silicon, polycrystalline silicon, single crystal silicon and metal oxides through the mutual cooperation of hydrogen peroxide, chelating agent, copper corrosion inhibitor, copper etchant, molybdenum alloy etchant and metal oxide damage inhibitor. When copper and molybdenum alloy can be etched at the same time, the damage to various active layers is also reduced to a minimum value.
[0017] In an optional embodiment, the following components are included:
[0018] H2O2 18.00wt%-21.00wt%;
[0019] and / or, chelating agent 2.00wt%-4.00wt%;
[0020] and / or, copper corrosion inhibitor 0.20wt%-1.20wt%;
[0021] and / or, copper etchant 0.50wt%-1.50wt%;
[0022] and / or, 0.20wt%-2.00wt% of molybdenum alloy etchant;
[0023] And / or, metal oxide damage inhibitor 0.05wt%-0.50wt%.
[0024] The content of each component in the etching solution is adjusted so that the etching solution can be suitable for etching more than two layers of metal films while having good stability, maintaining a suitable etching speed, inhibiting metal wiring corrosion, reducing damage to the active layer, and improving the process margin.
[0025] In an optional embodiment, the chelating agent is selected from at least one of iminodiacetic acid, sodium iminodiacetic acid, 1,2-cyclohexanediaminetetraacetic acid, inosinic acid, sodium iminodisuccinate, nitrotriacetic acid, ethylenediaminetetraacetic acid, ethylenetrinitro, aminotrisaccharide (methylenephosphonic acid), diglyphosate, ethylenediaminetetraacetic acid (methylenephosphonic acid), diethylenetriaminepenta (trimethylphosphonic acid), glutamic acid, aminobutyric acid and glycine; the chelating agent renders the metal ions oxidized during the etching process inert, thereby minimizing the activity of free metal ions and inhibiting the decomposition of hydrogen peroxide, which is beneficial to maintaining a high etching efficiency while keeping the composition stable, and the number of pieces processed is high, so there is also economic benefit.
[0026] In an optional embodiment, the copper corrosion inhibitor is selected from heterocyclic compounds; it can inhibit the corrosion caused by the etching solution and protect the metal wiring by combining with the metal on the surface of the metal wiring.
[0027] In an optional embodiment, the copper etchant is selected from at least one of sulfuric acid, maleic acid, phosphoric acid, sulfates and phosphates; the copper etchant can improve the uniformity of the surface of the copper metal film.
[0028] In an optional embodiment, the above-mentioned molybdenum alloy etchant is selected from fluorides and nitrates; the molybdenum alloy etchant helps to maintain the good etching performance and residue removal ability of the etching solution on the molybdenum alloy, and plays a role in improving the process margin.
[0029] In an optional embodiment, the metal oxide damage inhibitor is selected from at least one of cyclohexamethylenetetramine, n-hexylamine, arginine, histidine and lysine. The presence of the metal oxide damage inhibitor can reduce damage to the metal oxide exposed during the etching process.
[0030] In an optional embodiment, the copper corrosion inhibitor is selected from azole compounds;
[0031] and / or, the copper etchant is selected from at least one of sulfuric acid, potassium sulfate, ammonium sulfate, sodium sulfate, ammonium bisulfate, maleic acid, sodium bisulfate and potassium bisulfate;
[0032] and / or, the molybdenum alloy etchant is selected from at least one of hydrofluoric acid, ammonium fluoride, sodium fluoride, potassium fluoride, ammonium bifluoride, sodium bifluoride, potassium bifluoride, ammonium nitrate, sodium nitrate, potassium nitrate and calcium nitrate;
[0033] And / or, the metal oxide damage inhibitor includes n-hexylamine.
[0034] The components in the etching solution are optimized so that the etching solution can be suitable for etching more than two metal films, has good stability, and can maintain a suitable etching speed, inhibit wiring corrosion, reduce damage to the active layer, and improve the process margin.
[0035] In an optional embodiment, the copper corrosion inhibitor is selected from at least one of 3-amino-1,2,3-triazole, 3-amino-1,2,4-triazole, 4-amino-1,2,3-triazole, 4-amino-1,2,4-triazole, 5-methyltetrazole, 5-aminotetrazole and imidazole;
[0036] And / or, the water is deionized water with a resistivity ≥ 18 MΩ·cm;
[0037] And / or, further comprising 1.40wt%-1.60wt% of polyethylene glycol.
[0038] The copper corrosion inhibitor in the etching solution is further optimized to protect the metal wiring, and polyethylene glycol is added to protect the active layer.
[0039] In an optional embodiment, the chelating agent is selected from at least one of iminodiacetic acid and sodium iminodisuccinate;
[0040] and / or, the copper corrosion inhibitor is selected from at least one of 5-aminotetrazolyl and 3-amino-1,2,4-triazole;
[0041] And / or, the copper etchant is selected from at least one of sulfuric acid and maleic acid;
[0042] And / or, the molybdenum alloy etchant is selected from at least one of hydrofluoric acid and ammonium nitrate.
[0043] The components in the etching solution are further optimized so that the etching solution has better stability, more suitable etching speed, less wiring corrosion, and less damage to the active layer.
[0044] In an optional embodiment, the following components are included:
[0045] Chelating agent 3.00wt%-3.20wt%;
[0046] and / or, copper corrosion inhibitor 0.30wt%-0.45wt%;
[0047] and / or, copper etchant 0.80wt%-1.20wt%;
[0048] and / or, 0.10wt%-0.12wt% of molybdenum alloy etchant;
[0049] And / or, 0.10 wt% to 0.15 wt% of metal oxide damage inhibitor.
[0050] The dosage of each component in the etching solution is further optimized so that the etching solution has better stability, more suitable etching speed, less wiring corrosion, and less damage to the active layer.
[0051] In an optional embodiment, the mass ratio of iminodiacetic acid to sodium iminodisuccinate in the above-mentioned chelating agent is 2.3 / 0.8-2.5 / 0.6;
[0052] and / or, the mass ratio of 5-aminotetrazolyl to 3-amino-1,2,4-triazole in the above copper corrosion inhibitor is 0.20 / 0.15-0.40 / 0.10;
[0053] And / or, the mass ratio of sulfuric acid to maleic acid in the above copper etchant is 0.5 / 0.4-0.75 / 0.2;
[0054] And / or, the mass ratio of hydrofluoric acid to ammonium nitrate in the above molybdenum alloy etchant is 0.05 / 0.06-0.07 / 0.05.
[0055] The selection and dosage of each component in the etching solution are further optimized, so that the etching solution has better stability, more suitable etching speed, less wiring corrosion, and less damage to the active layer.
[0056] In a second aspect, the present invention provides an application of the etching solution of any one of the aforementioned embodiments in etching more than two metal films, wherein the metal films include a copper-containing metal film and a molybdenum alloy film, and the molybdenum alloy film also includes at least one of titanium, nickel, and niobium.
[0057] The etching solution of the present invention can be used to etch a multilayer structure metal film containing a copper metal film and a molybdenum alloy film, is compatible with the existing active layer, does not need to perform distributed etching on each metal film layer, and is conducive to improving process redundancy.
[0058] In an optional embodiment, the structure of the above-mentioned metal film is a structure of copper metal film / molybdenum alloy film, molybdenum alloy film / copper metal film, molybdenum alloy film / copper metal film / molybdenum alloy film, copper metal film / molybdenum alloy film / copper metal film, or a four-layer film structure of molybdenum alloy film and copper metal film cross-stacked. The bottom active layer of the above-mentioned metal film is selected from at least one of amorphous silicon, polycrystalline silicon, single crystal silicon and metal oxide.
[0059] Even if the underlying active layer is a metal oxide, the damage to the active layer during the etching process is relatively small.
[0060] The present invention has the following beneficial effects:
[0061] The etching solution of the present invention uses hydrogen peroxide as the main oxidant, which can provide hydrogen ions and adjust the etching rate. The etching solution of the present invention is compatible with active layers such as amorphous silicon, polycrystalline silicon, single crystal silicon and metal oxides through the mutual cooperation of hydrogen peroxide, chelating agent, copper corrosion inhibitor, copper etchant, molybdenum alloy etchant and metal oxide damage inhibitor, so that the etching solution of the present invention can be compatible with active layers such as amorphous silicon, polycrystalline silicon, single crystal silicon and metal oxides, so that copper and molybdenum alloys can be etched at the same time, and the damage to various active layers is also reduced to a minimum value. BRIEF DESCRIPTION OF THE DRAWINGS
[0062] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the drawings required for use in the embodiments are briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present invention and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other related drawings can be obtained based on these drawings without creative work.
[0063] Figure 1 The etching cross-sectional diagram is shown after Cu / MoTi / a-Si and MoTi / Cu / MoTi / IGZO are etched using the etching solution shown in Example 3. DETAILED DESCRIPTION
[0064] In order to make the purpose, technical scheme and advantages of the embodiments of the present invention clearer, the technical scheme in the embodiments of the present invention will be described clearly and completely below. If the specific conditions are not specified in the embodiments, they are carried out according to conventional conditions or conditions recommended by the manufacturer. If the manufacturer of the reagents or instruments used is not specified, they are all conventional products that can be purchased commercially.
[0065] An embodiment of the present invention provides an etching solution, comprising the following components:
[0066] H2O2 16.00wt%-24.00wt%;
[0067] Chelating agent 1.00wt%-5.00wt%;
[0068] Copper corrosion inhibitor 0.01wt%-2.50wt%;
[0069] Copper etchant 0.10wt%-4.00wt%;
[0070] Molybdenum alloy etchant 0.01wt%-3.00wt%;
[0071] Metal oxide damage inhibitor 0.01wt%-3.00wt%;
[0072] The remaining amount of water.
[0073] The etching solution of the present invention uses hydrogen peroxide as the main oxidant, which can provide hydrogen ions and adjust the etching rate. The etching solution of the present invention is compatible with active layers such as amorphous silicon, polycrystalline silicon, single crystal silicon and metal oxides through the mutual cooperation of hydrogen peroxide, chelating agent, copper corrosion inhibitor, copper etchant, molybdenum alloy etchant and metal oxide damage inhibitor. When copper and molybdenum alloy can be etched at the same time, the damage to various active layers is also reduced to a minimum value.
[0074] In an optional embodiment, the H2O2 in the etching solution is 16.00wt%-24.00wt%, specifically 16.00wt%, 18.00wt%, 20.00wt%, 22.00wt%, 24.00wt% or any value between 16.00wt% and 24.00wt%, preferably 18.00wt%-21.00wt%. When hydrogen peroxide is added to the above range, it has appropriate oxidation ability for metal films with more than two layers of structure, has a suitable etching speed, and the process is easy to control; and the number of pieces processed at the same time is appropriate, which is helpful to improve the process margin.
[0075] In an optional embodiment, the concentration of the chelating agent in the etching solution is 1.00wt%-5.00wt%, specifically 1.00wt%, 2.00wt%, 3.00wt%, 4.00wt%, 5.00wt% or any value between 1.00wt%-5.00wt%, preferably 2.00wt%-4.00wt%; when the chelating agent is added to the above range, it is beneficial to improve the stability of the etching solution and the number of pieces processed.
[0076] In an optional embodiment, the chelating agent is selected from at least one of iminodiacetic acid, sodium iminodiacetic acid, 1,2-cyclohexanediaminetetraacetic acid, inosinic acid, sodium iminodisuccinate, nitrotriacetic acid, ethylenediaminetetraacetic acid, ethylenetrinitro, aminotrisaccharide (methylenephosphonic acid), diglyphosate, ethylenediaminetetraacetic acid (methylenephosphonic acid), diethylenetriaminepenta (trimethylphosphonic acid), glutamic acid, aminobutyric acid and glycine; the chelating agent renders the metal ions oxidized during the etching process inert, thereby minimizing the activity of free metal ions and inhibiting the decomposition of hydrogen peroxide, which is beneficial to maintaining a high etching efficiency while keeping the etching solution stable, and a high number of pieces processed, so there is also economic benefit.
[0077] In an optional embodiment, the chelating agent is selected from at least one of iminodiacetic acid and sodium iminodisuccinate. Preferably, the mass ratio of iminodiacetic acid and sodium iminodisuccinate in the above-mentioned chelating agent is 2.3 / 0.8-2.5 / 0.6, and the concentration of the chelating agent in the etching solution is 3.00wt%-3.20wt%, which is beneficial to further improve the stability of the etching solution.
[0078] In an optional embodiment, the concentration of the copper corrosion inhibitor in the etching solution is 0.01wt%-2.50wt%, specifically 0.01wt%, 0.10wt%, 0.50wt%, 1.00wt%, 1.50wt%, 2.00wt%, 2.50wt% or any value between 0.01wt%-2.50wt%, preferably 0.20wt%-1.20wt%. When the amount of copper corrosion inhibitor added is within this range, the etching efficiency will not be reduced, and the wiring corrosion can also be suppressed.
[0079] The copper corrosion inhibitor is selected from heterocyclic compounds, such as azole compounds, and specifically can be selected from at least one of 3-amino-1,2,3-triazole, 3-amino-1,2,4-triazole, 4-amino-1,2,3-triazole, 4-amino-1,2,4-triazole, 5-methyltetrazolyl, 5-aminotetrazolyl and imidazole. When the copper corrosion inhibitor is selected from the above components, the etching speed of the copper metal film can be adjusted, and even if the number of processed pieces increases, the critical dimension bias (CD bias) of the metal routing can be maintained, which can improve the process margin.
[0080] In an optional embodiment, the copper corrosion inhibitor is selected from at least one of 5-aminotetrazolyl and 3-amino-1,2,4-triazole. Preferably, the mass ratio of 5-aminotetrazolyl and 3-amino-1,2,4-triazole in the above copper corrosion inhibitor is 0.20 / 0.15-0.40 / 0.10, and the concentration of the copper corrosion inhibitor in the etching solution is 0.30wt%-0.45wt%, which is more conducive to the stability of the etching solution and the etching efficiency.
[0081] In an optional embodiment, the concentration of copper etchant in the etching solution is 0.10wt%-4.00wt%, specifically 0.10wt%, 0.50wt%, 1.00wt%, 1.50wt%, 2.00wt%, 2.50wt%, 3.00wt%, 3.50wt%, 4.00wt% or any value between 0.10wt%-4.00wt%, preferably 0.50wt%-1.50wt%. The etching speed is moderate, the etching facet diagram is better, and the process efficiency and margin are also improved. In an optional embodiment, the above-mentioned copper etchant is selected from at least one of sulfuric acid, maleic acid, phosphoric acid, sulfate and phosphate, preferably selected from at least one of sulfuric acid, potassium sulfate, ammonium sulfate, sodium sulfate, ammonium bisulfate, maleic acid, sodium bisulfate and potassium bisulfate, which is conducive to adjusting the etching rate to a suitable range.
[0082] In an optional embodiment, the copper etchant is selected from at least one of sulfuric acid and maleic acid; preferably, the mass ratio of sulfuric acid to maleic acid in the above copper etchant is 0.5 / 0.4-0.75 / 0.2; the copper etchant in the etching solution is 0.80wt%-1.20wt%, which is more conducive to adjusting the etching efficiency to a suitable range.
[0083] In an optional embodiment, the concentration of the molybdenum alloy etchant in the etching solution is 0.01wt%-3.00wt%; specifically, it can be 0.01wt%, 0.10wt%, 0.50wt%, 1.00wt%, 1.50wt%, 2.00wt%, 2.50wt%, 3.00wt% or any value between 0.01wt%-3.00wt%, preferably 0.20wt%-2.00wt%. The concentration of the molybdenum alloy etchant within this range helps to maintain the good etching performance of the etching solution on the molybdenum alloy; and when the active layer is a metal oxide semiconductor, the damage to the active layer can be minimized.
[0084] In an optional embodiment, the platinum alloy etchant is selected from fluorides and nitrates, specifically selected from at least one of hydrofluoric acid, ammonium fluoride, sodium fluoride, potassium fluoride, ammonium difluoride, sodium difluoride, potassium difluoride, ammonium nitrate, sodium nitrate, potassium nitrate and calcium nitrate. The platinum alloy etchant is optimized by adding fluorine compounds and nitrates, thereby helping to maintain the good etching performance of the etching solution on the platinum alloy and the ability to remove residues, thereby improving process redundancy.
[0085] In an optional embodiment, the molybdenum alloy etchant is selected from at least one of hydrofluoric acid and ammonium nitrate; preferably, the mass ratio of hydrofluoric acid and ammonium nitrate in the above-mentioned molybdenum alloy etchant is 0.05 / 0.06-0.07 / 0.05, and the molybdenum alloy etchant in the etching solution is 0.10wt%-0.12wt%. The combination of hydrofluoric acid and ammonium nitrate can reduce the amount of fluorine used, thereby reducing damage to the active layer, and at the same time helps to maintain a suitable etching rate and residue removal ability, thereby obtaining a better etching profile.
[0086] In an optional embodiment, the concentration of the metal oxide damage inhibitor in the etching solution is 0.01wt%-3.00wt%, specifically 0.01wt%, 0.10wt%, 0.50wt%, 1.00wt%, 1.50wt%, 2.00wt%, 2.50wt%, 3.00wt% or any value between 0.01wt%-3.00wt%, preferably 0.05wt%-0.50wt%. When the concentration of the metal oxide damage inhibitor is within the above range, the damage of the etching solution to the metal oxide can be suppressed, the influence on the active layer is reduced, and the process redundancy is improved. When the concentration of the metal oxide damage inhibitor in the etching solution is too large and exceeds the above range, the etching rate of the molybdenum alloy film will be greatly reduced, which will lead to poor etching.
[0087] In an optional embodiment, the metal oxide damage inhibitor is selected from at least one of hexamethylenetetramine, n-hexylamine, arginine, histidine and lysine, preferably n-hexylamine, which is more conducive to reducing the damage to the active layer during the etching process.
[0088] In an optional embodiment, the metal oxide damage inhibitor is n-hexylamine, and the metal oxide damage inhibitor is contained in the etching solution at 0.10 wt % to 0.15 wt %, which is more conducive to reducing the damage to the active layer during the etching process.
[0089] In an optional embodiment, the water is deionized water with a resistivity of ≥18 MΩ·cm to reduce the introduction of impurities and reduce the influence of impurities on the etching effect.
[0090] In an optional embodiment, 1.40wt%-1.60wt% of polyethylene glycol is also included, specifically 1.40wt%, 1.50wt%, 1.60wt% or any value between 1.40wt% and 1.60wt%, which will form a dense protective film on the surface of the active layer, thereby helping to reduce damage to the active layer.
[0091] The present invention also provides an application of the etching solution of any one of the aforementioned embodiments in etching more than two metal films, wherein the metal films include a copper-containing metal film and a molybdenum alloy film, and the molybdenum alloy film also includes at least one of titanium, nickel, and niobium.
[0092] The etching solution of the present invention can be used to etch a multilayer structure metal film containing a copper metal film and a molybdenum alloy film, wherein the molybdenum alloy film can be selected from molybdenum-titanium alloy, molybdenum-nickel alloy, molybdenum-niobium alloy, molybdenum-titanium-nickel alloy, molybdenum-titanium-niobium alloy, and molybdenum-titanium-nickel-niobium alloy. In particular, when the molybdenum alloy is a molybdenum-titanium alloy, the molybdenum-titanium alloy can inhibit the diffusion of copper ions into the insulating film, so it has good device characteristics.
[0093] In an optional embodiment, the structure of the above-mentioned metal film is a structure of copper metal film / molybdenum alloy film, molybdenum alloy film / copper metal film, molybdenum alloy film / copper metal film / molybdenum alloy film, copper metal film / molybdenum alloy film / copper metal film, or a four-layer film structure of molybdenum alloy film and copper metal film cross-stacked. The bottom active layer of the above-mentioned metal film is selected from at least one of amorphous silicon, polycrystalline silicon, single crystal silicon and metal oxide.
[0094] The metal film can be a two-layer film, such as a copper metal film / molybdenum alloy film structure in which a copper metal film is used as a bottom film and a molybdenum alloy is used as a top film, or vice versa. It can also be a molybdenum alloy film / copper metal film structure. It can also be a three-layer film, such as a multilayer structure of more than three layers of molybdenum alloy film and copper metal film cross-stacked, specifically molybdenum alloy film / copper metal film / molybdenum alloy film, copper metal film / molybdenum alloy film / copper metal film. It can also be a structure with more than four layers, such as a structure with more than four layers of film stacked by molybdenum alloy film / copper metal film / molybdenum alloy film.
[0095] When the metal film is a molybdenum alloy film / copper metal film / molybdenum alloy film, the adhesion between the top and bottom connection films of more than two metal films or the diffusion of copper into the insulating film can be improved, so the device performance is better.
[0096] The metal oxides mentioned above that can be used as the bottom active layer can use metal oxides commonly used in this field, such as indium gallium zinc oxide (IGZO) InxAyBzO, where A and B are selected from gallium (Ga), zinc (Zn), tin (Sn), titanium (Ti), lead (Hf), zirconium (Zr), tantalum (Ta); x, y, z represent the proportion of each metal. The metal oxide can be a ternary or quaternary oxide, and can also be an amorphous structure or a crystalline structure.
[0097] The features and performance of the present invention are further described in detail below in conjunction with the embodiments.
[0098] The present application provides an etching solution, the composition of which is shown in Table 1, and the etching solution is obtained by uniformly mixing the components.
[0099] Table 1
[0100]
[0101] The letters in the remarks table are as follows:
[0102] *IDA:Iminodiacetic acid
[0103] *Na-IDS: iminodisuccinate sodium salt
[0104] *ATZ: 5-aminotetrazole
[0105] *TA: 3-amino-1,2,4-triazole
[0106] *SA:sulfuric acid
[0107] *MA:Maleic acid
[0108] *AN:ammonium nitrate
[0109] *HA: 2-hexamine
[0110] *HMA: 1,6-hexanediamine (hexame thylenediamine)
[0111] *PEG600: polyethylene glycol
[0112] Embodiment 20
[0113] The difference between this embodiment and embodiment 1 is that IDA is replaced by glutamic acid of equal mass fraction.
[0114] Embodiment 21
[0115] The difference between this embodiment and embodiment 1 is that Na-IDS is replaced by aminobutyric acid of equal mass fraction.
[0116] Embodiment 22
[0117] The difference between this embodiment and embodiment 1 is that ATZ is replaced by 5-methyltetrazolyl in an equal mass fraction.
[0118] Embodiment 23
[0119] The difference between this embodiment and embodiment 1 is that TA is replaced by 5-methyltetrazolyl in an equal mass fraction.
[0120] Embodiment 24
[0121] The difference between this embodiment and embodiment 1 is only that SA is replaced by sodium bisulfate of equal mass fraction.
[0122] Embodiment 25
[0123] The difference between this embodiment and embodiment 1 is that MA is replaced by potassium sulfate with an equal mass fraction.
[0124] Embodiment 26
[0125] The difference between this embodiment and embodiment 1 is that HF is replaced by ammonium fluoride with the same mass fraction.
[0126] Embodiment 27
[0127] The difference between this embodiment and embodiment 1 is that AN is replaced by calcium nitrate of equal mass fraction.
[0128] [Experimental example]
[0129] Experimental Example 1: Etching Performance Evaluation
[0130] The double-layer film is formed by evaporating an organic insulating film on a glass substrate, and then evaporating an oxide semiconductor on it to form a Cu / MoTi film (thickness: ).
[0131] The three-layer film is an organic insulating film evaporated on a glass substrate, an oxide film IGZO evaporated on it, and then MoTi / Cu / MoTi (thickness: ).
[0132] On the evaporated double-layer metal film and triple-layer metal film, a PR process (coating, exposure, and development) is performed using a mask with a certain circuit pattern to form a circuit pattern on the double-layer or triple-layer metal film, and then the glass is cut into 4x3cm pieces using a diamond knife to make samples.
[0133] 1 kg of the etching solution prepared in each embodiment and comparative example is placed in a beaker, and the above sample is etched when the temperature (30°C) set by the constant temperature bath is reached. The total etching time is 50% over-etched based on the detection end point (EPD), such as the etching time of MoTi / Cu / MoTi is 300 seconds. After cleaning and drying the etched substrate, a scanning electron microscope is used to confirm the etching profile. The side etching in the profile confirmation is observed from the end of the photoresist to the residual copper metal film.
[0134] Furthermore, in order to determine whether IGZO damage occurs, the step difference of the etched sample is measured using a step difference measuring instrument.
[0135] Experimental Example 2: Bath life evaluation
[0136] The method for determining the stability of the etching solution is as follows: a copper ion-containing component is added to the etching solution of each embodiment, so that the copper ion concentration in the etching solution increases with a concentration gradient of 1000 ppm, and then the etching solution containing the copper ion component is used to dissolve copper metal. When any one of the critical size or slope angle of the etched multi-layer metal film changes by 10% compared to the critical size or slope angle of the multi-layer metal film etched by the etching solution without the copper ion component, the copper ion concentration after the copper ion component is added to the etching solution is used as the upper limit of the bath life.
[0137] The data of Experimental Examples 1 and 2 are shown in Table 2.
[0138] Table 2
[0139]
[0140]
[0141] With reference to Table 2 above, the etching solutions of the embodiments have excellent selective etching performance for copper metal films and molybdenum alloy films. Specifically, the critical dimensions, slope angles, tails and tips are suitable, the damage to the active layer is small, and it is beneficial to reduce process defects; it has a higher bath life, and is applicable to multi-layer metal films and various active layers.
[0142] According to Table 2, each etching solution in Examples 1-10 has excellent selective etching performance for copper metal film and molybdenum alloy film, and has good comprehensive performance. Compared with Example 1: In Example 11, n-hexylamine is replaced with 1,6-hexanediamine, resulting in an increase in the Cu slope angle and tailing, and an increase in the MoTi tip size; in Example 13 and Example 15, which do not add ammonium nitrate or hydrogen fluoride, compared with Examples 1-10, the MoTi tail is longer, which may increase the poor etching of double-layer and triple-layer films; in Example 14, when no metal oxide damage inhibitor is added, IGZO damage increases, which will increase the probability of poor characteristics of process devices; in Example 12, when sodium iminodisuccinate is not added, the tank life is reduced; in Examples 16 and 17, 5-aminotetrazolyl or 3-amino-1,2,4-triazole is not added, resulting in an increase in the Cu slope angle and tailing, and an increase in the MoTi tip size; in Examples 18 and 19, sulfuric acid or maleic acid is not added, resulting in too small critical size, Cu slope angle and The MoTi tip size increases; Example 20 replaces IDA with glutamic acid of equal mass fraction, and Example 21 replaces Na-IDS with aminobutyric acid of equal mass fraction, resulting in increased IGZO damage and decreased tank life; Example 22 replaces ATZ with 5-methyltetrazole of equal mass fraction, and Example 23 replaces TA with 5-methyltetrazole of equal mass fraction, resulting in a Cu slope angle that is too small; Example 24 replaces SA with sodium bisulfate of equal mass fraction, and Example 25 replaces MA with potassium sulfate of equal mass fraction, resulting in a critical size that is too small, a Cu slope angle that is too large, and a decreased tank life; Example 26 replaces HF with ammonium fluoride of equal mass fraction, and Example 27 replaces AN with calcium nitrate of equal mass fraction, resulting in a slight decrease in the Cu slope angle. Compared with Example 1, the risks of poor etching in Examples 11-27 are all increased.
[0143] Figure 1 When a copper ion-containing component is added to the above-mentioned etching solution in Example 3 to a copper ion concentration of 500 ppm, the etching profiles obtained by etching the double-layer film (Cu / MoTi / a-Si) and the triple-layer film (MoTi / Cu / MoTi / IGZ0) have appropriate critical dimensions, Cu slope angles, MoTi tailing, and MoTi tip ranges, less damage to IGZO, and better etching profiles.
[0144] The above are only preferred embodiments of the present invention and are not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. An etching solution, characterized in that: Includes the following components: H2O2 16.00wt%-24.00wt%; Chelating agent 1.00wt%-5.00wt%; Copper corrosion inhibitor 0.01wt%-2.50wt%; Copper etchant 0.10wt%-4.00wt%; Molybdenum alloy etchant 0.01wt%-3.00wt%; Metal oxide damage inhibitor 0.01wt%-3.00wt%; The remaining amount of water.
2. The etching solution according to claim 1, characterized in that Includes the following components: H2O2 18.00wt%-21.00wt%; and / or, chelating agent 2.00wt%-4.00wt%; and / or, copper corrosion inhibitor 0.20wt%-1.20wt%; and / or, copper etchant 0.50wt%-1.50wt%; and / or, 0.20wt%-2.00wt% of molybdenum alloy etchant; And / or, metal oxide damage inhibitor 0.05wt%-0.50wt%.
3. The etching solution according to claim 1, characterized in that The chelating agent is selected from at least one of iminodiacetic acid, sodium iminodiacetic acid, 1,2-cyclohexanediaminetetraacetic acid, inosinic acid, sodium iminodisuccinate, nitrotriacetic acid, ethylenediaminetetraacetic acid, ethylenetrinitro, aminotrisaccharide (methylenephosphonic acid), diglycophosphine, ethylenediaminetetraacetic acid (methylenephosphonic acid), diethylenetriaminepenta (trimethylphosphonic acid), glutamic acid, aminobutyric acid and glycine; and / or, the copper corrosion inhibitor is selected from heterocyclic compounds; and / or, the copper etchant is selected from at least one of sulfuric acid, maleic acid, phosphoric acid, sulfates and phosphates; and / or, the molybdenum alloy etchant is selected from fluorides and nitrates; And / or, the metal oxide damage inhibitor is selected from at least one of hexamethylenetetramine, n-hexylamine, arginine, histidine and lysine.
4. The etching solution according to claim 1, characterized in that: The copper corrosion inhibitor is selected from azole compounds; and / or, the copper etchant is selected from at least one of sulfuric acid, potassium sulfate, ammonium sulfate, sodium sulfate, ammonium bisulfate, maleic acid, sodium bisulfate and potassium bisulfate; and / or, the molybdenum alloy etchant is selected from at least one of hydrofluoric acid, ammonium fluoride, sodium fluoride, potassium fluoride, ammonium bifluoride, sodium bifluoride, potassium bifluoride, ammonium nitrate, sodium nitrate, potassium nitrate and calcium nitrate; And / or, the metal oxide damage inhibitor includes n-hexylamine.
5. The etching solution according to claim 1, characterized in that: The copper corrosion inhibitor is selected from at least one of 3-amino-1,2,3-triazole, 3-amino-1,2,4-triazole, 4-amino-1,2,3-triazole, 4-amino-1,2,4-triazole, 5-methyltetrazole, 5-aminotetrazole and imidazole; And / or, the water is deionized water with a resistivity of ≥18 MΩ·cm; And / or, further comprising 1.40wt%-1.60wt% of polyethylene glycol.
6. The etching solution according to claim 1, characterized in that The chelating agent is selected from at least one of iminodiacetic acid and sodium iminodisuccinate; and / or, the copper corrosion inhibitor is selected from at least one of 5-aminotetrazolyl and 3-amino-1,2,4-triazole; And / or, the copper etchant is selected from at least one of sulfuric acid and maleic acid; And / or, the molybdenum alloy etchant is selected from at least one of hydrofluoric acid and ammonium nitrate.
7. The etching solution according to claim 6, characterized in that: Includes the following components: Chelating agent 3.00wt%-3.20wt%; and / or, copper corrosion inhibitor 0.30wt%-0.45wt%; and / or, copper etchant 0.80wt%-1.20wt%; and / or, 0.10wt%-0.12wt% of molybdenum alloy etchant; And / or, 0.10 wt% to 0.15 wt% of metal oxide damage inhibitor.
8. The etching solution according to claim 7, characterized in that The mass ratio of iminodiacetic acid to sodium iminodisuccinate in the chelating agent is 2.3 / 0.8-2.5 / 0.6; and / or, the mass ratio of 5-aminotetrazolyl to 3-amino-1,2,4-triazole in the copper corrosion inhibitor is 0.20 / 0.15-0.40 / 0.10; And / or, the mass ratio of sulfuric acid to maleic acid in the copper etchant is 0.5 / 0.4-0.75 / 0.2; And / or, the mass ratio of hydrofluoric acid to ammonium nitrate in the molybdenum alloy etchant is 0.05 / 0.06-0.07 / 0.
05.
9. Use of the etching solution according to any one of claims 1 to 8 in etching two or more metal films, characterized in that: The metal film includes a copper-containing metal film and a molybdenum alloy film, and the molybdenum alloy film also includes at least one of titanium, nickel and niobium.
10. The use according to claim 9, characterized in that: The structure of the metal film is a structure of copper metal film / molybdenum alloy film, molybdenum alloy film / copper metal film, molybdenum alloy film / copper metal film / molybdenum alloy film, copper metal film / molybdenum alloy film / copper metal film, or a structure of more than four layers of molybdenum alloy film and copper metal film cross-stacked, and the bottom active layer of the metal film is selected from at least one of amorphous silicon, polycrystalline silicon, single crystal silicon and metal oxide.