Heavy rare earth metal electroplating solution as well as preparation method and application thereof

By using the formulation of heavy rare earth metal plating solution and controlling the electroplating conditions, the problem of electrodeposition of rare earth elements in aqueous solution is solved, and the effect of low-cost and efficient preparation of rare earth metal plating is achieved.

CN119020834APending Publication Date: 2024-11-26CHINA JILIANG UNIV +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411421313.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-12
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

Rare earth elements are difficult to electrodeposit and precipitate in aqueous solution, and are prone to hydrolysis reactions, resulting in complex and high cost of electrodeposition. The prior art is difficult to effectively control the composition and production costs of rare earth alloys.

Method used

The formula of heavy rare earth metal plating solution is adopted, including soluble heavy rare earth salts, stabilizers, complexing agents and polar solvents, to control the temperature and pH of the plating solution, use metal plating plates as the anode, and apply a constant current to plating to form a fine And bright heavy rare earth metal plating.

Benefits of technology

It is realized that a uniform flat heavy rare earth metal plating with a thickness of 1.0 to 5.0 μm is prepared under low cost and simple operation, which solves the problem of deposition of rare earth elements in aqueous solution and reduces production costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119020834A_ABST
    Figure CN119020834A_ABST
Patent Text Reader

Abstract

The invention relates to a heavy rare earth metal electroplating solution and a preparation method and application thereof, the heavy rare earth metal electroplating solution is electroplated on the surface of a metal material matrix, and the electroplating solution comprises the following raw materials: soluble heavy rare earth salt, a stabilizer, a complexing agent, a polar solvent and deionized water; the soluble heavy rare earth salt is one or more of dysprosium trichloride hexahydrate or terbium trichloride hexahydrate; the stabilizer is one or more of boric acid or glycine; the complexing agent is one or more of citric acid, sodium dodecyl sulfate and ethylenediamine tetraacetic acid; the polar solvent is one or more of sodium citrate and ammonium chloride; the mass concentration of heavy rare earth ions forming the heavy rare earth metal electroplating solution is 20-40 g / L, the temperature of the electroplating solution is 30-55 DEG C, and the pH value of the electroplating solution is 2.0-4.0. According to the method, the effect of forming the heavy rare earth metal coating on the surface layer of the magnetic material substrate can be achieved, and the obtained heavy rare earth alloy coating is fine and smooth in surface, bright and free of dark areas.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of metal electroplating, and in particular to a heavy rare earth metal electroplating solution and a preparation method and application thereof. Background Art

[0002] In the periodic table of chemical elements, there are 17 elements in total, including 15 lanthanide elements and two closely related elements, scandium and yttrium, which are called rare earth elements. Rare earth elements have similar electronic structure characteristics. Their 4f electron layer is not full, which can produce a variety of different electronic energy levels. They have large atomic magnetic moments and strong spin-orbit coupling, which give them unique optical, electrical and magnetic physical and chemical properties. They have received great attention in the field of high-tech materials. The most studied methods for preparing rare earth alloys are physical vapor deposition and electrodeposition. The physical method for preparing rare earth alloy materials has high production costs, complex technology, difficult composition control, and high equipment requirements. In contrast, electrodeposition is an economical and convenient method for preparing rare earth alloy materials. The standard reduction potential of rare earth elements is relatively negative. For example, the electrode potential of neodymium is about -2.4. Therefore, it is difficult for rare earth metals to be electrodeposited in aqueous solution, and hydrogen evolution has a great influence on the deposition process. Therefore, it is necessary to increase the hydrogen evolution overpotential and shift the rare earth element deposition potential positively to partially or completely inhibit hydrogen evolution, which is conducive to the electrodeposition of rare earth elements. Furthermore, rare earth elements are very prone to hydrolysis in aqueous solution, and the solution becomes turbid, making electrodeposition difficult. At present, adding a complexing agent to shift the reduction potential of rare earth elements positively to inhibit hydrogen evolution is an effective method for depositing metal elements from aqueous solution. Summary of the invention

[0003] To achieve the above-mentioned purpose and other related purposes, the present invention provides a heavy rare earth metal electroplating solution and a preparation method and application thereof.

[0004] To achieve the above-mentioned purpose and other related purposes, the technical solution provided by the present invention is: a heavy rare earth metal electroplating solution, the raw material formula of the heavy rare earth metal electroplating solution includes the following raw materials: a soluble heavy rare earth salt, a stabilizer, a chelating agent, a polar solvent and deionized water; the soluble heavy rare earth salt is at least one of dysprosium trichloride hexahydrate and terbium trichloride hexahydrate; in the heavy rare earth metal electroplating solution, the concentration of heavy rare earth ions is 20-40 g / L, and the pH value is 2.0-4.0.

[0005] The preferred technical solution is: the stabilizer is at least one of boric acid and glycine, and the concentration is 20-40 g / L.

[0006] The preferred technical solution is: the complexing agent is at least one of citric acid, sodium dodecyl sulfate and ethylenediaminetetraacetic acid, and the concentration is 40-50 g / L.

[0007] The preferred technical solution is: the polar solvent is at least one of sodium citrate and ammonium chloride, and the concentration is 20-40 g / L.

[0008] To achieve the above-mentioned purpose and other related purposes, the technical solution provided by the present invention is: a method for preparing a heavy rare earth metal electroplating solution, characterized in that: raw materials are weighed according to the raw material formula described in any one of claims 1-4, and the heavy rare earth metal electroplating solution is obtained after mixing evenly.

[0009] To achieve the above-mentioned purpose and other related purposes, the technical solution provided by the present invention is: an application of a heavy rare earth metal electroplating solution, firstly, the metal plated part is deoiled and degreased, polished, ultrasonically cleaned with cold water, ultrasonically cleaned with anhydrous ethanol and vacuum dried to obtain a metal material workpiece to be plated; then, a metal platinum plate is used as an anode and the metal material workpiece to be plated is used as a cathode, and they are placed in an electroplating tank containing the heavy rare earth metal electroplating solution according to claim 6, the temperature of the heavy rare earth metal electroplating solution is controlled to be 30-55°C, the pH value of the heavy rare earth metal electroplating solution is 2.0-4.0, a constant current is applied for electroplating, and the electroplating time is 10-45 minutes. After the electroplating is completed, a heavy rare earth metal coating is formed on the surface of the metal material workpiece to be plated.

[0010] The preferred technical solution is: the current density during electroplating is 5.0-10.0A / dm 2 .

[0011] The preferred technical solution is: the coating thickness on the surface of the metal material workpiece to be plated is 1.0 to 5.0 μm.

[0012] Due to the application of the above technical solution, the present invention has the following advantages compared with the prior art:

[0013] The heavy rare earth metal electroplating solution of the present invention adopts a soluble heavy rare earth salt, a stabilizer, a complexing agent, a polar solvent and deionized water, and controls the temperature and pH value of the electroplating solution to achieve the effect of forming a heavy rare earth metal coating on the surface of the magnetic material substrate. The obtained heavy rare earth alloy coating has a fine surface, a bright coating and no dark area.

[0014] 2. The electroplating process using the heavy rare earth metal electroplating solution proposed in the present invention is simple to operate and has low manufacturing cost. By using the heavy rare earth metal electroplating solution described above, electroplating for 10 to 45 minutes at a temperature of 40 to 55°C and a pH value of 2.0 to 4.0 can produce a heavy rare earth metal coating with a thickness of 1.0 to 5.0 μm. BRIEF DESCRIPTION OF THE DRAWINGS

[0015] Figure 1 This is a SEM image of the heavy rare earth metal coating of Example 2 of the present invention.

[0016] Figure 2This is an energy spectrum scanning diagram of the heavy rare earth metal coating of Example 2 of the present invention. DETAILED DESCRIPTION

[0017] The following is a description of the implementation of the present invention by means of specific embodiments. Those skilled in the art can easily understand other advantages and effects of the present invention from the contents disclosed in the embodiments.

[0018] See also Figure 1-2 . It should be noted that the structures, proportions, sizes, etc. illustrated in the drawings of this specification are only used to match the contents disclosed in the specification for people familiar with this technology to understand and read, and are not used to limit the limiting conditions under which the present invention can be implemented. Therefore, they have no substantive technical significance, and any structural modification, change in proportional relationship or adjustment of size. The following examples are provided to better understand the present invention, but are not intended to limit the present invention. The experimental methods in the following examples are all conventional methods unless otherwise specified. The experimental materials used in the following examples are all purchased from conventional biochemical reagent stores unless otherwise specified.

[0019] In a specific embodiment of the present invention, the metal-plated material is purchased from the market, and the base size is 15.0 mm × 10.0 mm × 4.5 mm. Before use, the metal-plated base is preferably degreased and deoiled. The degreasing and degreasing treatment is to place the purchased metal material in a beaker filled with glacial acetic acid and ultrasonically wash it for 30 to 60 minutes, more preferably for 40 to 60 minutes, and more preferably for 45 to 50 minutes, and then take the metal base out of the beaker for polishing. The grinding is performed sequentially as primary grinding, secondary grinding and tertiary grinding; the mesh number of the primary grinding is preferably 700-900 mesh, more preferably 750-850 mesh, more preferably 780-820 mesh; the mesh number of the secondary grinding is preferably 1400-1600 mesh, more preferably 1450-1550 mesh, more preferably 1480-1520 mesh; the mesh number of the tertiary grinding is preferably 2900-3100 mesh, more preferably 2950-3050 mesh, more preferably 2980-3020 mesh.

[0020] The present invention provides a heavy rare earth metal electroplating solution, comprising the following components: a soluble heavy rare earth salt A, a stabilizer B, a complexing agent C, a polar solvent D and deionized water;

[0021] The soluble heavy rare earth salt A is selected from one or more of dysprosium trichloride hexahydrate and terbium trichloride hexahydrate, and the mass concentration of the soluble heavy rare earth salt A is 20-40 g / L.

[0022] The stabilizer B is one or more of boric acid and glycine, and the mass concentration of the stabilizer B is 20-40 g / L.

[0023] The complexing agent C is one or more of citric acid, sodium dodecyl sulfate and ethylenediaminetetraacetic acid, and the mass concentration of the complexing agent C is 40-50 g / L.

[0024] The polar solvent D is one or more of sodium citrate and ammonium chloride, and the mass concentration of the polar solvent D is 20-40 g / L.

[0025] The mass concentration of the heavy rare earth ions forming the heavy rare earth metal electroplating solution is 20-40 g / L, the plating solution temperature is 30-55° C., and the plating solution pH value is 2.0-4.0.

[0026] In the present invention, dysprosium trichloride hexahydrate is used as the main salt to participate in the reaction, boric acid and glycine are used as buffer stabilizers to stabilize the plating solution components, citric acid, sodium dodecyl sulfate and ethylenediaminetetraacetic acid are used as complexing agents to make the heavy rare earth ion deposition potential move forward to facilitate electrodeposition, and sodium citrate and ammonium chloride are added to enhance the conductivity of the solution.

[0027] The present invention also provides a method for preparing a heavy rare earth electroplating solution, comprising the following steps:

[0028] (1) weighing the components of the electroplating solution according to the formula to prepare the heavy rare earth metal electroplating solution;

[0029] (2) Before electroplating, the metal parts are degreased, polished, cleaned with cold water ultrasonic, cleaned with anhydrous ethanol ultrasonic and vacuum dried;

[0030] (3) using a metal platinum plate as an anode and a magnetic material workpiece to be plated as a cathode, placing the plate in the electroplating solution of an electroplating tank, controlling the temperature of the electroplating solution to be 30 to 55° C., the pH value of the electroplating solution to be 2.0 to 4.0, applying a constant current for electroplating, and the electroplating time to be 10 to 45 minutes. After the electroplating is completed, a heavy rare earth metal coating is formed on the surface of the cathode metal plated workpiece;

[0031] In the present invention, the metal plated material is purchased and has a size of 15.mm×10.0mm×4.5mm. In step (2), the metal material substrate is preferably degreased and deoiled before use. The degreasing and degreasing treatment is to put the purchased metal substrate into a beaker filled with glacial acetic acid and ultrasonically shake and wash it for 30 to 60 minutes, more preferably for 40 to 60 minutes, and more preferably for 45 to 50 minutes, and then take the magnet out of the beaker for polishing. The grinding is performed sequentially as primary grinding, secondary grinding and tertiary grinding; the mesh number of the primary grinding is preferably 700-900 mesh, more preferably 750-850 mesh, more preferably 780-820 mesh; the mesh number of the secondary grinding is preferably 1400-1600 mesh, more preferably 1450-1550 mesh, more preferably 1480-1520 mesh; the mesh number of the tertiary grinding is preferably 2900-3100 mesh, more preferably 2950-3050 mesh, more preferably 2980-3020 mesh.

[0032] In the present invention, after the grinding and polishing in step (2) is completed, the surface of the metal material substrate is bright and flat, and the ground metal material substrate is adhered to the surface of the pure copper sheet with the oxide layer removed by conductive copper adhesive that is conductive on both sides, as the working electrode phase of electrochemical deposition.

[0033] In the present invention, the electrochemical deposition in step (3) is performed by using an electrochemical workstation with a three-electrode working system to co-deposit the plating solution in a constant current deposition manner; the working electrode of the electrochemical deposition is a pure copper sheet adhered with a neodymium iron boron magnet, the counter electrode is a metal platinum sheet electrode, and the reference electrode is a saturated calomel electrode.

[0034] In the step (3), the temperature of the electroplating solution is controlled to be 30-55°C, more preferably 32-50°C, and even more preferably 33-46°C.

[0035] In the step (3), the pH value of the plating solution is controlled to be 2.0 to 4.0, more preferably 2.2 to 3.8, and even more preferably 2.2 to 3.5.

[0036] In the step (3), the electroplating time is controlled to be 10 to 45 minutes, more preferably 20 to 35 minutes, and more preferably 25 to 33 minutes.

[0037] In the step (3), the current density of the electroplating is 5.0 to 10.0 A / dm2, more preferably 6.0 to 8.2 A / dm2, and more preferably 7.0 to 8.1 A / dm2.

[0038] In the step (3), the thickness of the surface coating of the cathode is 1.0 to 5.0 μm, more preferably 1.5 to 4.0 μm, and even more preferably 2.5 to 3.6 μm.

[0039] The technical solutions provided by the present invention are described in detail below in conjunction with the embodiments, but they should not be construed as limiting the protection scope of the present invention.

[0040] The NdFeB magnets used in the embodiments of the present invention are all from the industrial production line, and the magnets are N52M (coercivity 990-1000 kA / m, remanence 1.35-1.42 T) of the same batch and brand. Dysprosium trichloride hexahydrate (AR), boric acid (AR), glycine (AR), citric acid (AR), sodium dodecyl sulfonate (AR), ethylenediaminetetraacetic acid (AR), sodium citrate (AR) and ammonium chloride (AR).

[0041] Example 1: A heavy rare earth metal electroplating solution and its preparation method and application

[0042] 3 g of dysprosium trichloride hexahydrate, 2.5 g of boric acid, 1.5 g of glycine, 2 g of citric acid, 3 g of sodium citrate, 1 g of sodium dodecyl sulfate, 1 g of ethylenediaminetetraacetic acid and 1 g of ammonium chloride were added to deionized water, and the mixture was stirred at 850 r / min for 30 min at 20° C. to prepare an electroplating solution. The pH of the electroplating solution was adjusted to 3.0 using 1 mol / L NaOH solution, and was recorded as Plating Solution 1.

[0043] The other conditions were kept constant, and the plating solution temperatures were set to 30°C, 40°C, 45°C and 50°C, respectively, to obtain plating solution 2, plating solution 3, plating solution 4 and plating solution 5. The cyclic voltammetry test curves of each plating solution were tested using Shanghai Chenhua 760E electrochemical workstation, and the results are shown in Table 1.

[0044] Table 1 Comparison of cyclic voltammetry results of each group of plating solutions at different temperatures

[0045]

[0046]

[0047] As can be seen from Table 1, with the increase of the plating solution temperature, the cathode overpotential of Dy3+ shows a trend of decreasing first and then increasing. When the constant temperature of the plating solution is 45°C, the cathode overpotential of Dy3+ is the smallest among the five groups of experiments, and the corresponding deposition current value also reaches the minimum value at the same time, indicating that under the same deposition conditions, it is easier to reduce and deposit Dy3+ from the solution when the constant temperature of 45°C is used for electrodeposition. The decomposition potential of water also increases first and then decreases with the increase of the plating solution temperature, so 45°C is selected as the optimal electroplating temperature.

[0048] Example 2: A heavy rare earth metal electroplating solution and its preparation method and application

[0049] 3 g of dysprosium trichloride hexahydrate, 2.5 g of boric acid, 1.5 g of glycine, 2 g of citric acid, 3 g of sodium citrate, 1 g of sodium dodecyl sulfate, 1 g of ethylenediaminetetraacetic acid and 1 g of ammonium chloride were added to deionized water, and the mixture was stirred at 850 r / min for 30 min at a temperature of 45° C. to prepare an electroplating solution. The pH of the electroplating solution was adjusted to 1.0 using 1 mol / L NaOH solution, and was recorded as Plating Solution 1.

[0050] The other conditions were controlled unchanged, and the pH values ​​of the plating solutions were set to 2.0, 3.0, 4.0, 5.0, 6.0 and 7.0, respectively, to obtain plating solutions 2, 3, 4, 5, 6 and 7. The cyclic voltammetry test curves of the plating solutions were tested using Shanghai Chenhua 760E electrochemical workstation, and the results are shown in Table 2.

[0051] Table 2 Comparison of cyclic voltammetry results of each group of plating solutions at different pH values

[0052] sample <![CDATA[Dy 3+ Deposition Potential]]> Water decomposition potential Plating solution 1 -0.613V -1.035V Plating solution 2 -0.609V -1.216V Plating solution 3 -0.598V -1.367V Plating solution 4 -0.576V -1.393V Plating solution 5 -0.593V -1.427V Plating solution 6 -0.694V -1.441V Plating solution 7 -0.787V -1.459V

[0053] It can be seen from Table 2 that with the increase of the pH of the plating solution, Dy 3+ The cathode overpotential of the solution showed a trend of decreasing first and then increasing. With the increase of the pH value of the plating solution, the decomposition potential of water in the solution also gradually increased, from -1.035V at pH = 1.0 to -1.459V at pH = 7.0. When the pH value of the plating solution was 4.0, the Dy 3+ The cathode overpotential is small, and at this pH concentration, the decomposition potential of water is large, and the hydrogen evolution reaction has little effect on the deposition process. Therefore, pH = 4.0 is selected as the optimal electroplating pH value.

[0054] Example 3: A heavy rare earth metal electroplating solution and its preparation method and application

[0055] 3g of dysprosium trichloride hexahydrate, 2.5g of boric acid, 1.5g of glycine, 2g of citric acid, 3g of sodium citrate, 1g of sodium dodecyl sulfate, 1g of ethylenediaminetetraacetic acid and 1g of ammonium chloride were added to deionized water, stirred at a speed of 850r / min for 30min at a temperature of 45°C to prepare an electroplating solution, and a 1mol / L NaOH solution was used to adjust the pH of the electroplating solution to 4.0; the NdFeB magnet was polished using 800-mesh, 1500-mesh and 3000-mesh sandpapers in sequence; then, the electroplating solution was uniformly deposited on the surface of the NdFeB substrate by constant current electrodeposition, wherein the current was set to 5mA, the time was set to 10min, and the solution temperature was set to 45°C; after the deposition was completed, the magnet was taken out, rinsed with deionized water, and then the surface was washed with anhydrous ethanol, and sent to a vacuum drying oven, and dried at 0.10Pa and 50°C for 60min, which was recorded as magnet 1.

[0056] The other conditions were kept constant, and the constant current electrodeposition time was set to 20 min, 30 min, and 45 min, respectively, to obtain magnets 2, 3, and 4. The coating morphology and film thickness of each sample were tested by scanning electron microscopy, and the results are shown in Table 3.

[0057] Table 3 Comparison of film thickness results of various magnets

[0058] sample Film thickness(μm) Is the coating uniform and flat? Magnet 1 1.295 yes Magnet 2 1.758 yes Magnet 3 2.166 yes Magnet 4 4.243 yes

[0059] It can be seen from Table 3 that as the deposition time increases, the thickness of the deposited layer also increases accordingly, which shows the feasibility of the operation of this experiment.

[0060] The invention relates to the technical field of metal electroplating, and discloses a heavy rare earth metal electroplating solution and a use process thereof, which is electroplated on the surface of a metal material substrate, and the raw materials of the electroplating solution include: a soluble heavy rare earth salt, a stabilizer, a complexing agent, a polar solvent and deionized water; the soluble heavy rare earth salt is one or more of dysprosium chloride or terbium chloride; the stabilizer is one or more of boric acid or glycine; the complexing agent is one or more of citric acid, sodium dodecyl sulfate and ethylenediaminetetraacetic acid; the polar solvent is one or more of sodium citrate and ammonium chloride; the mass concentration of heavy rare earth ions forming the heavy rare earth metal electroplating solution is 20-40 g / L, the plating solution temperature is 30-55° C., and the plating solution pH is 2.0-4.0. The alloy coating prepared by the electroplating solution provided by the invention is uniform, flat and dense, and the alloy elements are evenly distributed.

[0061] Example 4: A heavy rare earth metal electroplating solution and its preparation method and application

[0062] A heavy rare earth metal electroplating solution, wherein the raw material formula of the heavy rare earth metal electroplating solution comprises the following raw materials: a soluble heavy rare earth salt, a stabilizer, a chelating agent, a polar solvent and deionized water; the soluble heavy rare earth salt is at least one of dysprosium trichloride hexahydrate and terbium trichloride hexahydrate; in the heavy rare earth metal electroplating solution, the concentration of heavy rare earth ions is 20 g / L and the pH value is 2.0.

[0063] A preferred embodiment is that the stabilizer is a mixture of boric acid and glycine in a mass ratio of 1:1, with a concentration of 20 g / L.

[0064] A preferred embodiment is that the complexing agent is a mixture of citric acid, sodium dodecyl sulfate and ethylenediaminetetraacetic acid in a mass ratio of 1:1:2, with a concentration of 40 g / L.

[0065] A preferred embodiment is that the polar solvent is ammonium chloride with a concentration of 20 g / L.

[0066] The raw materials are weighed according to the above raw material formula, and mixed evenly to obtain a heavy rare earth metal electroplating solution.

[0067] The invention discloses an application of a heavy rare earth metal electroplating solution. Firstly, a metal plated part is subjected to degreasing and degreasing, grinding and polishing, cold water ultrasonic cleaning, anhydrous ethanol ultrasonic cleaning and vacuum drying treatment to obtain a metal material workpiece to be plated; then a metal platinum plate is used as an anode and the metal material workpiece to be plated is used as a cathode, and the two are placed in an electroplating tank containing the heavy rare earth metal electroplating solution; the temperature of the heavy rare earth metal electroplating solution is controlled to be 30 DEG C, the pH value of the heavy rare earth metal electroplating solution is controlled to be 2.0, a constant current is applied for electroplating, and the electroplating time is 10 minutes. After the electroplating is completed, a heavy rare earth metal coating is formed on the surface of the metal material workpiece to be plated.

[0068] The preferred embodiment is: the current density during electroplating is 5.0A / dm 2 .

[0069] A preferred implementation is that the coating thickness on the surface of the metal material workpiece to be plated is 1.0 μm.

[0070] Example 5: A heavy rare earth metal electroplating solution and its preparation method and application

[0071] A heavy rare earth metal electroplating solution, wherein the raw material formula of the heavy rare earth metal electroplating solution comprises the following raw materials: a soluble heavy rare earth salt, a stabilizer, a chelating agent, a polar solvent and deionized water; the soluble heavy rare earth salt is at least one of dysprosium trichloride hexahydrate and terbium trichloride hexahydrate; in the heavy rare earth metal electroplating solution, the concentration of heavy rare earth ions is 40 g / L and the pH value is 4.0.

[0072] A preferred embodiment is that the stabilizer is glycine with a concentration of 40 g / L.

[0073] A preferred embodiment is that the complexing agent is sodium dodecyl sulfate with a concentration of 50 g / L.

[0074] A preferred embodiment is that the polar solvent is a mixture of sodium citrate and ammonium chloride in a mass ratio of 1:3, with a concentration of 40 g / L.

[0075] The raw materials are weighed according to the raw material formula in the claim, and mixed evenly to obtain a heavy rare earth metal electroplating solution.

[0076] The invention discloses an application of a heavy rare earth metal electroplating solution. Firstly, a metal plated part is subjected to degreasing and degreasing, grinding and polishing, cold water ultrasonic cleaning, anhydrous ethanol ultrasonic cleaning and vacuum drying treatment to obtain a metal material workpiece to be plated; then a metal platinum plate is used as an anode and the metal material workpiece to be plated is used as a cathode, and the two are placed in an electroplating tank containing the heavy rare earth metal electroplating solution; the temperature of the heavy rare earth metal electroplating solution is controlled to be 55° C., the pH value of the heavy rare earth metal electroplating solution is controlled to be 4.0, a constant current is applied for electroplating, and the electroplating time is 45 minutes. After the electroplating is completed, a heavy rare earth metal coating is formed on the surface of the metal material workpiece to be plated.

[0077] The preferred embodiment is: the current density during electroplating is 10.0A / dm 2 .

[0078] A preferred implementation is that the coating thickness on the surface of the metal material workpiece to be plated is 5.0 μm.

[0079] The above description is only used to explain the preferred embodiments of the present invention, and is not intended to limit the present invention in any form. Therefore, any modifications or changes made to the present invention under the same inventive spirit should still be included in the scope of protection intended by the present invention.

Claims

1. A heavy rare earth metal electroplating solution, characterized in that: The raw material formula of the heavy rare earth metal electroplating solution includes the following raw materials: a soluble heavy rare earth salt, a stabilizer, a chelating agent, a polar solvent and deionized water; the soluble heavy rare earth salt is at least one of dysprosium trichloride hexahydrate and terbium trichloride hexahydrate; in the heavy rare earth metal electroplating solution, the concentration of heavy rare earth ions is 20 to 40 g / L, and the pH value is 2.0 to 4.

0.

2. The heavy rare earth metal electroplating solution according to claim 1, characterized in that: The stabilizer is at least one of boric acid and glycine, and the concentration is 20-40 g / L.

3. The heavy rare earth metal electroplating solution according to claim 1, characterized in that: The complexing agent is at least one of citric acid, sodium dodecyl sulfate and ethylenediaminetetraacetic acid, and the concentration is 40-50 g / L.

4. The heavy rare earth metal electroplating solution according to claim 1, characterized in that: The polar solvent is at least one of sodium citrate and ammonium chloride, and the concentration is 20-40 g / L.

5. A method for preparing a heavy rare earth metal electroplating solution, characterized in that: The raw materials are weighed according to the raw material formula described in any one of claims 1 to 4, and mixed evenly to obtain a heavy rare earth metal electroplating solution.

6. An application of a heavy rare earth metal electroplating solution, characterized in that: First, the metal plated parts are degreased, polished, ultrasonically cleaned with cold water, ultrasonically cleaned with anhydrous ethanol, and vacuum dried to obtain metal material workpieces to be plated; then, a metal platinum plate is used as an anode and the metal material workpiece to be plated is used as a cathode, and they are placed in an electroplating tank containing the heavy rare earth metal electroplating solution according to claim 6, the temperature of the heavy rare earth metal electroplating solution is controlled to be 30-55°C, the pH value of the heavy rare earth metal electroplating solution is controlled to be 2.0-4.0, a constant current is applied for electroplating, and the electroplating time is 10-45 minutes. After the electroplating is completed, a heavy rare earth metal coating is formed on the surface of the metal material workpiece to be plated.

7. The use of the heavy rare earth metal electroplating solution according to claim 6, characterized in that: The current density during electroplating is 5.0~10.0A / dm 2 .

8. The use of the heavy rare earth metal electroplating solution according to claim 6, characterized in that: The coating thickness on the surface of the metal material workpiece to be plated is 1.0 to 5.0 μm.