Carbon-doped aramid fiber as well as production method and application thereof
Through the wet spinning process, the activated carbon dispersion is mixed with the aromatic polyamide solution to produce aramid doped fibers with high fracture strength and high adsorption activity, which solves the problem of insufficient performance of aramid doped fibers in the prior art. Suitable for anti-virus clothing and other products, and reduces production costs.
Patent Information
- Application Number
- CN202310590743.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-24
- Publication Date
- 2024-11-26
AI Technical Summary
The prior art has failed to effectively provide aramid doped fibers with high fracture strength and good adsorption activity and their production methods, and the industrial production costs are high and the activated carbon particle size requirements are strict, which limits its application.
By mixing activated carbon powder with dispersant and organic solvent to form an activated carbon dispersion and fully mixing it with the aromatic polyamide solution, aramid doped fibers are prepared by wet spinning process, and the components and process parameters of the spinning liquid are controlled to obtain High fracture strength and high adsorption activity.
The fracture strength of aramid doped fiber is greater than 1.8cN/dtex and the adsorption amount of benzene reaches 15%, reducing the particle size requirements of activated carbon, suitable for industrial production, and is used in anti-virus clothing and other products.
Abstract
Description
Technical Field
[0001] The invention relates to aramid carbon-doped fiber and a production method and application thereof. Background Art
[0002] Breathable anti-virus clothing is a kind of dual-use skin protection equipment for both military and civilian use that can pass air and moisture, but can prevent external toxic gases, droplet-shaped poisons, bacteria and radioactive dust from causing harm to the human body. Breathable anti-virus clothing is usually composed of two to three layers of materials, among which the adsorption layer with adsorption function plays a key role in anti-virus.
[0003] CN113106615A discloses an anti-toxic knitted fabric and a production method thereof, the production method comprising the steps of weaving carbon-doped yarn and coated silk into a knitted grey cloth; the carbon-doped yarn is a single yarn prepared from carbon-doped nitrile fiber and other optional fibers. The anti-toxic knitted fabric obtained in this patent document has good anti-toxic performance and air permeability. The patent document mentions that the carbon-doped yarn is formed by carbon-doped nitrile fiber and other optional fibers, and the other fibers are selected from one of sulfone fiber, polyimide fiber, polyester fiber, aramid fiber, hemp fiber and cotton fiber. However, the embodiments of this patent document do not involve other fibers, let alone aramid fibers, but only use carbon-doped yarns formed by carbon-doped nitrile fiber. In addition, this patent document does not involve aramid carbon-doped fibers.
[0004] CN111270386A discloses a breathable textile fabric and a preparation method thereof, the textile fabric comprises interwoven antibacterial warp yarn, weft yarn and second warp yarn; in parts by weight, the antibacterial warp yarn comprises 4-10 parts of water-absorbing fiber, 3-9 parts of jute fiber, 2-4 parts of silk fiber and 2-4 parts of antibacterial coating; the weft yarn comprises 5-12 parts of ultrafine activated carbon fiber, 4-12 parts of polyester fiber, 3-9 parts of aramid fiber and 1-3 parts of ramie fiber; the second warp yarn comprises 3-9 parts of nano carbon fiber, 3-8 parts of bamboo charcoal fiber and 2-6 parts of 15D polyester staple fiber. The weft yarn production process comprises mixing ultrafine activated carbon fiber, polyester fiber, aramid fiber, ramie fiber and distilled water, ultrasonically oscillating for 6-10 minutes, and then spinning to obtain the weft yarn. Although the patent document mentions aramid fiber and activated carbon fiber, it also uses other fibers, including polyester fiber and ramie fiber, not just aramid fiber mixed with carbon. Moreover, the patent document does not mention the strength, elongation at break and adsorption performance of the weft yarn.
[0005] CN1209507C discloses a flame retardant fiber containing an adsorbent material and a preparation method thereof. The preparation method comprises mixing a resin and an adsorbent material, dissolving the mixture in an organic solvent, and wet spinning the mixture to form a fiber containing the adsorbent material. The resin described in the patent document is a copolymer of acrylonitrile-vinyl chloride or a copolymer of acrylonitrile-vinylidene chloride, and aramid fiber is not involved. Moreover, the method in the patent document is a laboratory preparation method, not an industrial production method. The particle size of the activated carbon or activated carbon fiber used is required to be less than 1 μm, and the production cost is high, which is not conducive to industrial production.
[0006] CN104233903A discloses an activated carbon fiber paper and a preparation method thereof, wherein the activated carbon fiber paper uses aramid fibrid as a carrier on which activated carbon fibers are loaded; the absolute dry mass of the aramid fibrid accounts for 10-50% of the absolute dry mass of the activated carbon fiber paper. The patent document does not firmly attach and embed the activated carbon into the aramid fibrid, and thus cannot form fibers that can be used in anti-virus clothing.
[0007] So far, there is still no report on aramid carbon-doped fibers with both high breaking strength and good adsorption activity and their production methods. Summary of the invention
[0008] In view of this, one object of the present invention is to provide a method for producing aramid carbon-doped fibers, which can produce aramid carbon-doped fibers with both high breaking strength and high adsorption activity. Another object of the present invention is to provide an aramid carbon-doped fiber produced according to the above production method, the aramid carbon-doped fiber has a breaking strength greater than or equal to 1.8 cN / dtex, and a benzene adsorption capacity of up to 15%. Another object of the present invention is to provide an application of the aramid carbon-doped fibers as described above. The present invention achieves the above objects through the following technical solutions.
[0009] In one aspect, the present invention provides a method for producing aramid carbon-doped fiber, comprising the following steps:
[0010] 1) mixing activated carbon powder, a dispersant and an organic solvent to obtain an activated carbon dispersion;
[0011] 2) fully mixing the activated carbon dispersion and the aromatic polyamide solution to obtain a spinning solution;
[0012] 3) The spinning solution is spun by a wet spinning process to obtain aramid carbon-doped fibers.
[0013] According to the production method of the present invention, preferably, the dispersant is selected from one or more of polyethylene glycol alkylphenyl ether, hexadecyltrimethylammonium bromide and polyvinylpyrrolidone.
[0014] According to the production method of the present invention, preferably, the dispersant is selected from one of polyethylene glycol alkylphenyl ether, cetyltrimethylammonium bromide and polyvinyl pyrrolidone.
[0015] According to the production method of the present invention, preferably, the mass ratio of the dispersant to the organic solvent is 0.002 to 0.1:1; and the organic solvent is selected from one or more of N,N-dimethylformamide, N,N-dimethylacetamide and dimethyl sulfoxide.
[0016] According to the production method of the present invention, preferably, the organic solvent is selected from one of N,N-dimethylformamide, N,N-dimethylacetamide and dimethyl sulfoxide.
[0017] According to the production method of the present invention, preferably, the concentration of activated carbon in the activated carbon dispersion is 10-30wt%; the particle size of the activated carbon powder is less than or equal to 10μm; the aromatic polyamide in the aromatic polyamide solution is poly(meta-phenylene isophthalamide), and the content of poly(meta-phenylene isophthalamide) is 15-30wt%.
[0018] According to the production method of the present invention, preferably, the ratio of the mass of the solute in the activated carbon dispersion to the mass of the total solute in the spinning solution is 10-30:100.
[0019] According to the production method of the present invention, preferably, the wet spinning process comprises the following steps:
[0020] The spinning solution is filtered, sprayed out through a spinneret, coagulated in a coagulation bath to form fibers, and then drawn, dried and heat-treated;
[0021] Among them, the drawing multiple is 7 to 20; the drying temperature is 110 to 170° C., and the drying time is 30s to 5min; the heat treatment temperature is 300 to 550° C., and the heat treatment time is 1 to 7min.
[0022] On the other hand, the present invention also provides an aramid carbon-doped fiber produced according to the production method as described above, wherein the breaking strength of the aramid carbon-doped fiber is greater than or equal to 1.8 cN / dtex, and the benzene adsorption capacity can reach 15%.
[0023] In another aspect, the present invention also provides the use of the aramid carbon-doped fiber as described above. The aramid carbon-doped fiber can be used in special protective products such as anti-virus clothing, masks, protective clothing, foot protection, hand protection, and civilian products such as curtains, seat cushions, and filters.
[0024] The production method of the present invention can produce aramid carbon-doped fibers with high breaking strength and good adsorption activity, with a breaking strength of not less than 1.8 cN / dtex and a benzene adsorption of up to 15%. Moreover, the production method of the present invention has low requirements on the particle size of the activated carbon used, and the particle size of the activated carbon can be below 10 μm, preferably below 5 μm, which is conducive to industrial production. According to the preferred technical solution of the present invention, a spinning solution capable of spinning is obtained by using a specific type of dispersant to form an activated carbon dispersion and by mixing a specific amount of the activated carbon dispersion with an aromatic polyamide solution, and then spinning to obtain aramid carbon-doped fibers with good performance. DETAILED DESCRIPTION
[0025] The present invention is further described below in conjunction with specific embodiments, but the protection scope of the present invention is not limited thereto.
[0026] The production method of the present invention can be used to prepare aramid carbon-doped fibers having both high strength and good adsorption activity.
[0027] The production method of aramid carbon-doped fiber of the present invention comprises the following steps: (1) obtaining activated carbon dispersion liquid; (2) obtaining spinning liquid; and (3) obtaining aramid carbon-doped fiber.
[0028] <Obtaining activated carbon dispersion>
[0029] Activated carbon powder, a dispersant and an organic solvent are mixed to obtain an activated carbon dispersion. The activated carbon powder can be obtained by crushing and grinding activated carbon particles. The particle size of the activated carbon powder is less than or equal to 10 μm, preferably less than or equal to 8 μm, and more preferably less than or equal to 5 μm. This can be beneficial for obtaining aramid carbon-doped fibers with good adsorption performance and relatively uniform adsorption performance. Relatively uniform adsorption performance means that the activated carbon is relatively evenly dispersed, and there will be no uneven adsorption performance caused by uneven distribution of the activated carbon.
[0030] In the present invention, the dispersant is selected from one or more of polyethylene glycol alkyl phenyl ether, hexadecyl trimethyl ammonium bromide and polyvinyl pyrrolidone. Preferably, the dispersant is selected from one of polyethylene glycol alkyl phenyl ether, hexadecyl trimethyl ammonium bromide and polyvinyl pyrrolidone. More preferably, the dispersant is polyethylene glycol alkyl phenyl ether. According to a preferred embodiment of the present invention, the dispersant is polyethylene glycol alkyl phenyl ether. The number of carbon atoms in the alkyl group of polyethylene glycol alkyl phenyl ether can be 6 to 16, preferably 8 to 12, and more preferably 8 to 10.
[0031] In the present invention, the organic solvent is selected from one or more of N,N-dimethylformamide, N,N-dimethylacetamide and dimethyl sulfoxide. Preferably, the organic solvent is selected from one of N,N-dimethylformamide, N,N-dimethylacetamide and dimethyl sulfoxide. More preferably, the organic solvent is N,N-dimethylformamide or N,N-dimethylacetamide. According to a preferred embodiment of the present invention, the organic solvent is N,N-dimethylacetamide.
[0032] In the present invention, the mass ratio of the dispersant to the organic solvent is 0.002 to 0.1:1, preferably 0.005 to 0.07:1, and more preferably 0.005 to 0.05:1. This is beneficial to improving the breaking strength and adsorption activity of the obtained aramid carbon-doped fiber.
[0033] The concentration of the activated carbon in the activated carbon dispersion of the present invention is 10-30wt%, preferably 12-25wt%, more preferably 15-20wt%, which is beneficial to spinning and obtaining aramid carbon-doped fibers with better adsorption performance.
[0034] According to a preferred embodiment of the present invention, granular activated carbon is crushed and ground to a particle size of less than 5 μm to obtain activated carbon powder; 1 part by weight of polyethylene glycol octylphenyl ether dispersant is added to 100 parts by weight of N,N-dimethylacetamide and mixed evenly, and then activated carbon powder is added and stirred to be fully mixed to obtain an activated carbon dispersion, wherein the content of activated carbon is 15 to 20 wt%.
[0035] <Obtaining Spinning Solution>
[0036] The activated carbon dispersion liquid and the aromatic polyamide solution are fully mixed to obtain a spinning solution.
[0037] In the present invention, the aromatic polyamide in the aromatic polyamide solution may be poly-p-phenylene terephthalamide or poly-m-phenylene isophthalamide, preferably poly-m-phenylene isophthalamide.
[0038] In the present invention, the aromatic polyamide solution of poly(metaphenylene isophthalamide) can be obtained by a method known in the art, or can be commercially available.
[0039] Wherein, the content of poly(m-phenylene isophthalamide) in the aromatic polyamide solution is 15-30wt%, preferably 15-25wt%, more preferably 17-22wt%. The molecular weight of poly(m-phenylene isophthalamide) is 80000-150000. The salt content in the aromatic polyamide solution is 8-13wt%, preferably 8-11wt%, more preferably 8-10wt%. Preferably, the aromatic polyamide solution is purchased from Yantai Taihe New Materials Co., Ltd.; the molecular weight of poly(m-phenylene isophthalamide) is 80000-150000; the content of poly(m-phenylene isophthalamide) in the aromatic polyamide solution is 20wt%, and the salt content is 9wt%.
[0040] The mass ratio of the solute in the activated carbon dispersion to the total solute in the spinning solution is 10 to 30:100, preferably 13 to 25:100, and more preferably 15 to 25:100. That is, the usage ratio of the two is the mass ratio of the activated carbon in the activated carbon dispersion to the total mass of the activated carbon and the polyisophthalamide polymer in the spinning solution. This is conducive to obtaining aramid carbon-doped fibers with excellent breaking strength and adsorption activity.
[0041] According to a preferred embodiment of the present invention, an activated carbon dispersion is added to an aromatic polyamide solution and mixed thoroughly to obtain a spinning solution; wherein the ratio of the mass of the solute in the activated carbon dispersion to the mass of the total solute in the spinning solution is 10 to 30:100.
[0042] <Obtaining Aramid Carbon-doped Fiber>
[0043] The spinning solution is spun by a wet spinning process to obtain aramid carbon-doped fibers.
[0044] In the present invention, the wet spinning process comprises the following steps:
[0045] The spinning solution is filtered, sprayed out through a spinneret, coagulated in a coagulation bath to form fibers, and then drawn, dried and heat-treated.
[0046] Among them, the drafting multiple is 7 to 20, preferably 7 to 15, and more preferably 7 to 13. The drying temperature is 110 to 170°C, preferably 110 to 160°C, and more preferably 110 to 150°C. The drying time is 30s to 5min, preferably 30s to 3min, and more preferably 30s to 1min. The heat treatment temperature is 300 to 550°C, preferably 300 to 500°C, and more preferably 300 to 450°C. The heat treatment time is 1 to 7min, preferably 1 to 5min, and more preferably 1 to 3min. This is conducive to obtaining aramid carbon-doped fibers with better performance.
[0047] In the present invention, the coagulation bath may be N,N-dimethylacetamide, N,N-dimethylformamide, or methylpyrrolidone, and preferably the coagulation bath is N,N-dimethylacetamide.
[0048] The present invention also provides aramid carbon-doped fibers produced by the above production method. The obtained aramid carbon-doped fibers have a breaking strength of not less than 1.8 cN / dtex and a benzene adsorption capacity of up to 15%.
[0049] The higher the benzene adsorption of the obtained aramid carbon-doped fiber, the better the adsorption performance. The greater the breaking strength value of the obtained aramid carbon-doped fiber, the higher the strength of the aramid carbon-doped fiber and the better the subsequent performance. During the production process of aramid carbon-doped fiber, as the carbon content increases, the adsorption performance improves, but the fiber breaking strength decreases, the production efficiency decreases, the cost increases, and the subsequent spinning and weaving become more difficult.
[0050] The aramid carbon-doped fiber obtained by the invention can have both good adsorption performance and high breaking strength.
[0051] <Test Method>
[0052] Test of benzene adsorption:
[0053] Principle of determination: Under the specified test conditions, a gas stream containing a certain concentration of benzene vapor is continuously passed through the carbon-doped fiber. The carbon-doped fiber increases its mass after absorbing the benzene vapor, and the increase in mass is represented by the elongation of the quartz spring. Because the elongation of the quartz spring is proportional to the increase in mass of the carbon-doped fiber, the adsorption amount of the carbon-doped fiber under the standard benzene vapor concentration can be measured.
[0054] The specific operation steps are as follows: 1) using a height gauge to measure the height h0 of a tray (the tray is used to place the carbon-doped fiber, and the tray is connected to a spring); 2) adding a sample to be tested (the carbon-doped fiber prepared in the present invention) to the tray and covering the bottom of the tray, and measuring the height h1 of the tray; 3) turning on a benzene vapor generator, allowing the sample to be tested to pass through the generator for no less than 10 minutes until adsorption equilibrium is reached, and measuring the height h2 of the tray after adsorption; 4) using a calculation formula to calculate:
[0055] Benzene adsorption amount % = (h2-h1) / (h1-h0)×100%.
[0056] The sources of some raw materials in the embodiments and comparative examples are introduced below:
[0057] Aromatic polyamide solution: purchased from Yantai Taihe New Materials Co., Ltd.; the molecular weight of poly(m-phenylene isophthalamide) is 80,000-150,000; the content of poly(m-phenylene isophthalamide) in the aromatic polyamide solution is 20 wt %, and the salt content is 9 wt %.
[0058] Polyacrylonitrile-vinylidene chloride solution: purchased from Fushun Ruihua Fiber Co., Ltd.
[0059] Example 1
[0060] 1) The granular activated carbon is crushed and ground to a particle size of 5 μm or less to obtain activated carbon powder. 1 part by weight of polyethylene glycol octylphenyl ether is added to 100 parts by weight of N,N-dimethylacetamide and mixed evenly, and then the activated carbon powder is added and stirred to be fully mixed to obtain an activated carbon dispersion, wherein the content of the activated carbon is 16 wt%.
[0061] 2) Adding the activated carbon dispersion into the aromatic polyamide solution and mixing them thoroughly to obtain a spinning solution.
[0062] 3) The spinning solution is spun by a wet spinning process, the spinning solution is filtered, sprayed out through a spinneret, coagulated in a coagulation bath to form fibers, and then stretched, dried and heat-treated; wherein the stretching multiple is 8, the drying temperature is 120°C, and the drying time is 60s; the heat treatment temperature is 300°C, and the heat treatment time is 1.5min, to obtain aramid carbon-doped fibers.
[0063] Example 2
[0064] The only difference from Example 1 is that in step 2), the amount of activated carbon dispersion added is different.
[0065] Example 3
[0066] The only difference from Example 1 is that in step 1), polyethylene glycol octylphenyl ether is replaced by polyvinyl pyrrolidone.
[0067] Example 4
[0068] The only difference from Example 1 is that in step 1), polyethylene glycol octylphenyl ether is replaced by hexadecyltrimethylammonium bromide.
[0069] Comparative Example 1
[0070] The only difference from Example 1 is that in step 2), the amount of activated carbon dispersion added is different.
[0071] Comparative Example 2
[0072] The only difference from Example 1 is that in step 2), the amount of activated carbon dispersion added is different.
[0073] Comparative Example 3
[0074] The only difference from Example 1 is that in step 1), polyethylene glycol octylphenyl ether is not added.
[0075] Comparative Example 4
[0076] The only difference from Example 1 is that in step 1), polyethylene glycol octylphenyl ether is replaced by sodium dodecylbenzene sulfonate.
[0077] Comparative Example 5
[0078] The difference from Example 1 is that in step 2), the aromatic polyamide solution is replaced by a polyacrylonitrile-vinylidene chloride solution. In step 3), there is no heat treatment process.
[0079] Comparative Example 6
[0080] The only difference from Example 1 is that in step 2), the aromatic polyamide solution is replaced by a polyacrylonitrile-vinylidene chloride solution; in step 3), the amount of activated carbon dispersion added is different; and there is no heat treatment process.
[0081] Table 1
[0082] serial number M Breaking strength (cN / dtex) Benzene adsorption (%) Example 1 20:100 2.35 10.2 Example 2 28:100 1.81 15.0 Example 3 20:100 2.27 8.9 Example 4 20:100 2.24 9.2 Comparative Example 1 35:100 1.53 16.3 Comparative Example 2 7:100 3.53 3.4 Comparative Example 3 20:100 2.13 8.5 Comparative Example 4 20:100 2.17 8.4 Comparative Example 5 20:100 1.35 6.3 Comparative Example 6 16:100 1.52 5.0
[0083] Note: M refers to the ratio of the mass of activated carbon in the added activated carbon dispersion to the mass of the total solute in the spinning solution.
[0084] It can be seen from the examples and comparative examples 1-2 that the aramid carbon-doped fiber obtained by the production method of the present invention has high fracture strength and high adsorption activity. The carbon-doped amount can be adjusted according to actual needs to obtain products with different strengths and adsorption properties.
[0085] It can be seen from the examples and comparative examples 3 to 4 that the dispersant has an important influence on the breaking strength and benzene adsorption of the aramid carbon-doped fiber and is not a conventional choice.
[0086] In addition, it can be seen from the examples and comparative examples 5 to 6 that when the aromatic polyamide solution is replaced by the polyacrylonitrile-vinylidene chloride solution, the breaking strength and benzene adsorption amount are significantly lower, and the adsorption activity and breaking strength are far inferior to the aramid carbon-doped fiber produced by the present invention.
[0087] The present invention is not limited to the above-mentioned embodiments. Without departing from the essential content of the present invention, any deformation, improvement and substitution that can be conceived by those skilled in the art shall fall within the scope of the present invention.
Claims
1. A method for producing aramid carbon-doped fiber, It is characterized in that The following steps are involved: 1) mixing activated carbon powder, a dispersant and an organic solvent to obtain an activated carbon dispersion; 2) fully mixing the activated carbon dispersion and the aromatic polyamide solution to obtain a spinning solution; 3) The spinning solution is spun by a wet spinning process to obtain aramid carbon-doped fibers.
2. The production method according to claim 1, It is characterized in that The dispersant is selected from one or more of polyethylene glycol alkylphenyl ether, hexadecyltrimethylammonium bromide and polyvinyl pyrrolidone.
3. The production method according to claim 2, It is characterized in that The dispersant is selected from one of polyethylene glycol alkylphenyl ether, hexadecyltrimethylammonium bromide and polyvinyl pyrrolidone.
4. The production method according to claim 1, It is characterized in that The mass ratio of the dispersant to the organic solvent is 0.002 to 0.1:1; the organic solvent is selected from one or more of N,N-dimethylformamide, N,N-dimethylacetamide and dimethyl sulfoxide.
5. The production method according to claim 1, It is characterized in that The organic solvent is selected from one of N,N-dimethylformamide, N,N-dimethylacetamide and dimethyl sulfoxide.
6. The production method according to claim 1, It is characterized in that The concentration of activated carbon in the activated carbon dispersion is 10-30wt%; the particle size of the activated carbon powder is less than or equal to 10μm; the aromatic polyamide in the aromatic polyamide solution is poly(m-phenylene isophthalamide), and the content of poly(m-phenylene isophthalamide) is 15-30wt%.
7. The production method according to claim 1, It is characterized in that The ratio of the mass of the solute in the activated carbon dispersion to the mass of the total solute in the spinning solution is 10 to 30:
100.
8. The production method according to any one of claims 1 to 7, It is characterized in that The wet spinning process comprises the following steps: The spinning solution is filtered, sprayed out through a spinneret, coagulated in a coagulation bath to form fibers, and then drawn, dried and heat-treated; Among them, the drawing multiple is 7 to 20; the drying temperature is 110 to 170° C., and the drying time is 30s to 5min; the heat treatment temperature is 300 to 550° C., and the heat treatment time is 1 to 7min.
9. Aramid carbon-doped fiber obtained by the production method according to any one of claims 1 to 8, It is characterized in that The breaking strength of the aramid carbon-doped fiber is greater than or equal to 1.8 cN / dtex, and the benzene adsorption capacity can reach 15%.
10. Use of the aramid carbon-doped fiber according to claim 9.