Passive radiation refrigeration coating textile as well as preparation method and application thereof
The porous passive radiation refrigeration coating is prepared on textiles through the combination of polylactic acid and pore-generating agent, which solves the complex process and aging problems in the prior art, and achieves efficient and environmentally friendly cooling effects, simplifies the preparation process and improves the coating performance.
Patent Information
- Application Number
- CN202411133776.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-19
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2044-08-19
AI Technical Summary
The existing passive radiation refrigeration coating textiles have complex processes, poor results, and the coating is prone to aging, and no ecological and environmental protection issues are considered.
Polylactic acid and pore-generating agent are dissolved in organic solvents, and pore-induced refrigeration coatings are prepared by coating and hot water bath cold water bath phase separation technology, simplifying the process, achieving high solar reflectivity and long-wave infrared emissivity, and using environmentally friendly Materials, simplify the preparation process.
It realizes the simple and rapid preparation of highly efficient passive radiation refrigeration coating, which has good ecological and environmental protection and economic benefits, provides cooling effect of 5 to 15℃, and has excellent wear resistance, acid and alkali resistance, water washing resistance and aging resistance.
Smart Images

Figure CN119021010A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of passive radiation cooling coating textiles, and in particular to a passive radiation cooling coating textile and a preparation method and application thereof. Background Art
[0002] Traditional refrigeration methods represented by air conditioning are energy-consuming refrigeration methods with high energy consumption and large CO2 emissions. There is an urgent need to develop new refrigeration technologies. Passive daytime radiative cooling (PDRC) is a non-refrigeration method that uses atmospheric windows (ATW) to radiate to the outside space (13K). It is a new energy-saving and emission-reduction technology with broad application prospects. In recent years, it has received great attention from scholars at home and abroad. Combining passive radiative cooling technology with textiles can create cool textiles that can cool down, thereby reducing the demand for energy-consuming cooling air conditioners.
[0003] At present, the existing passive radiation cooling coated textiles are mainly prepared by dipping, spraying and other methods on the basis of existing textiles. Chinese patent CN113136724A discloses a radiation cooling fabric, which is prepared by impregnating silk fabric with nano-alumina hydrosol, and then drying the nano-alumina particles to attach to the fiber. The particles with high refractive index are superimposed on the fiber to improve the fabric reflectivity, thereby achieving a cooling effect of 3.6°C lower than room temperature under sunlight. Chinese patent CN112853522A mixes inorganic micro-nano particles and base materials to obtain micro-nano particles and base material spinning solution; the micro-nano particles and base material spinning solution are subjected to dry-wet spinning to obtain radiation cooling fibers; the inorganic micro-nano particles have the characteristics of high refractive index, which can produce high scattering efficiency in the base material, so that the radiation cooling fiber has high solar radiation reflectivity. Chinese patent CN110387751A discloses a radiation self-cooling functional fiber fabric, which is constructed by layering a commercial high-reflection silver layer and an atmospheric window radiation layer on the surface of the textile, and dispersing nanoparticles in a resin adhesive middle layer to form a mid-infrared selective radiation layer; the use of a commercial silver layer increases its cost, and the mixing, proportion and specific efficacy of multiple particles are unclear and need to be studied. The prior art discloses a protective clothing fabric with radiation refrigeration technology, including a first material layer and a second material layer and an adhesive layer that bonds the first material layer and the second material layer. The material of the first material layer is a high-density fabric, which is used for protection against viruses, bacteria, etc. The material of the second material layer is a flexible radiation refrigeration film or a flexible radiation refrigeration fabric, which is used for passive radiation refrigeration. The preparation process is complicated and the cost is high, and the layered structure has high requirements for the bonding process and the supporting structure.
[0004] In summary, the current research process of passive radiation cooling coating textiles has the following problems: 1. The process of layered construction of passive radiation cooling coating textiles is complicated and the effect is not ideal. The coating often needs to use resin adhesives, which will affect its pores and the performance of nanoparticles, and the coating with added resin generally has a dense structure, which greatly reduces the reflectivity of the solar spectrum band; the radiation cooling film is bonded to the fabric by hot pressing to prepare the radiation cooling fabric, and the preparation process is complicated and the bonding process is also required to be high. 2. The coating of the prior art generally adopts the operation of direct immersion in water for phase separation, or immersion in a low-boiling point solvent and placing it in the environment to volatilize the solvent for phase separation. Oversized samples require a larger coagulation bath, and the coating solution may flow during the immersion in the coagulation bath, resulting in uneven coating thickness and discontinuous coating; the phase separation speed of the prior art is slow, which greatly reduces the efficiency of continuous production. 3. Although the passive radiation cooling coating textiles of the prior art have a certain cooling effect, the coated textiles are prone to aging in the environment, and the problem of ecological protection is not considered. Summary of the invention
[0005] In order to solve the above technical problems, the purpose of the present invention is to provide a passive radiation cooling coating textile and its preparation method and application. The preparation method is compatible with the existing technology, optimizes the coating structure of synthetic fiber fabrics, and realizes a passive radiation cooling coating textile structure that is also applicable to hydrophobic synthetic fiber fabrics. The process is simple, can be manufactured on a large scale at low cost, and has broad application prospects.
[0006] The above object of the present invention is achieved through the following technical solutions:
[0007] A first aspect of the present invention provides a method for preparing a passive radiation cooling coated textile, comprising the following steps:
[0008] (1) dissolving polylactic acid (PLA) and a porogen in an organic solvent and completely dissolving them at 70 to 110° C. to obtain a coating solution;
[0009] (2) cooling the coating solution obtained in step (1) to 55-80° C., and applying the cooled coating solution to the surface of the textile to obtain a coated textile;
[0010] (3) Immersing the coated textile obtained in step (2) in a hot water bath at 60 to 80° C., taking it out and immersing it in a cold water bath at 15 to 30° C. for phase separation, thereby obtaining a passive radiation cooling coated textile.
[0011] The process adopted by the present invention is a traditional coating process, which is simple and convenient, and a porous passive radiation cooling coating is produced by phase separation technology. Phase separation technology is a highly versatile method, which is widely used to produce porous membranes through various phase separation processes. The phase separation behavior of the film-forming system plays a vital role in determining the membrane morphology and performance. The present invention prepares a radiation cooling fabric with high solar reflectivity and long-wave infrared emissivity by optimizing the coating structure without loading nanoparticles, overcoming the problems of poor fastness of polymer coatings, complex preparation process, high cost, and difficulty in degradation in the prior art, and adopts a method of hot water bath followed by cold water bath to overcome the problem of long coating phase separation time, and finally realizes the simple and rapid preparation of daytime passive radiation cooling coating textiles.
[0012] The polylactic acid used in the present invention is an environmentally friendly biomass polymer material, which is a biodegradable biomass material. The -CH3, C=O, and COC of the molecular chain have strong absorption vibration peaks in the atmospheric window band. According to Kirchhoff's radiation law, high absorption can be converted into high thermal emissivity, so that it has high emission in the atmospheric window (8-13 μm), thereby realizing effective thermal radiation and achieving successful radiation cooling. The prior art generally forms a polylactic acid reflective layer by electrostatic spinning, and obtains a polylactic acid film with a multi-level structure by roll-to-roll electrostatic spinning to achieve high reflection and high emission. The present invention does not use the inorganic fillers or electrostatic spinning technology commonly used in the prior art. Through a simple coating process, it achieves significant reflection and emission capabilities, has unexpected beneficial effects, and has significant progress. In addition, polylactic acid has great advantages in environmental protection and has great benefits in solving energy crises and environmental and ecological problems.
[0013] Furthermore, in step (1), the porogen is selected from one or more of polyethylene glycol (PEG), ammonium polyphosphate, polyvinyl pyrrolidone (PVP) and urea.
[0014] Polyethylene glycol acts as a porogen and a plasticizer, which can effectively control the pore size and pore distribution of the coating, regulate the pore structure of the coating, increase the pore density, improve the softness of the coating, and enhance the chemical stability of the coating.
[0015] Furthermore, the solid-to-liquid ratio of the polylactic acid and polyethylene glycol is (3-10) g:(0.5-20) mL, preferably 1 g:(0.5-2) mL.
[0016] Furthermore, the mass ratio of the polylactic acid to polyvinyl pyrrolidone is (3-10):(0.5-5).
[0017] Furthermore, the porogen is preferably polyethylene glycol and polyvinyl pyrrolidone.
[0018] Furthermore, the solid-to-liquid ratio of the polyvinyl pyrrolidone and polyethylene glycol is (0.5-5) g:(0.5-20) mL, preferably (0.5-2) g:(1-20) mL.
[0019] Furthermore, the mass ratio of the polylactic acid to ammonium polyphosphate is (3-10):(0.5-5).
[0020] Furthermore, the mass ratio of the polylactic acid to urea is (3-10):(0.5-5).
[0021] Furthermore, the volume ratio of the polyethylene glycol to the organic solvent is 1:(2-7).
[0022] Furthermore, in step (1), the solid-to-liquid ratio of the polylactic acid to the organic solvent is (3-10) g:(17.5-50) mL, preferably 1 g:(3.5-4) mL.
[0023] In a specific embodiment, in step (1), polylactic acid, porogen and organic solvent are stirred at 100-1500 rpm for 1-3 hours under reflux condensation at 70-110° C. to mix the solution evenly, thereby preparing a coating solution.
[0024] Furthermore, in step (1), the organic solvent is selected from one or more of N,N-dimethylacetamide (DMAc), N,N-dimethylformamide, N-methylpyrrolidone and dimethyl sulfoxide.
[0025] Furthermore, in step (2), the textile is a high-density fiber fabric, including a hydrophobic synthetic fiber fabric, which can be one or more of polyester, nylon and acrylic.
[0026] Furthermore, in step (2), the coating has a thickness of 10 to 300 μm, preferably 30 to 250 μm, and more preferably 50 to 200 μm.
[0027] Preferably, in step (2), the coating solution is cooled to 60-80°C.
[0028] Furthermore, in step (3), the time of immersion in the hot water bath is 40 to 240 seconds, preferably 40 to 120 seconds.
[0029] Preferably, in step (3), the coated textile is immersed in a hot water bath at 65 to 75°C.
[0030] Furthermore, in step (3), the immersion time in the cold water bath is 1 to 24 hours.
[0031] Furthermore, in step (3), a drying step is also included after immersing in a cold water bath.
[0032] Furthermore, drying is performed by air-drying or drying in a tumble dryer.
[0033] The second aspect of the present invention provides a passive radiation cooling coated textile obtained by the preparation method described in the first aspect.
[0034] Passive radiation cooling coating textiles include textiles and passive radiation cooling coatings on their surfaces, wherein the passive radiation cooling coating is a polylactic acid biomass coating. The present invention uses textiles as a substrate, uses biomaterial polylactic acid as a coating skeleton, adds a porogen, and finally non-solvent-induced phase separation to construct an anisotropic porous self-adhesive radiation cooling coating (i.e., a passive radiation cooling coating) on the fabric surface. The polylactic acid biomass coating after phase separation has high reflectivity to the UV-VIS-NIR solar spectrum, and the internal hyperbranched network structure can be tightly adsorbed on the surface of each fiber, thereby having a good bonding strength with the underlying fabric.
[0035] The third aspect of the present invention provides the use of the passive radiation cooling coated textiles described in the second aspect in the preparation of passive radiation cooling materials, especially in flexible materials, such as clothing, curtains, tents, parasols, hats, car covers and canopies, etc. The passive radiation cooling coated textiles provide cooling effects while maintaining the characteristics of light and thin fabrics, thereby improving comfort, saving energy, and contributing to environmental protection.
[0036] Beneficial effects of the present invention:
[0037] 1. The process adopted by the present invention is a traditional coating process, and provides a hot and cold bath alternating process that can be continuously produced. The process is simple and can reduce the phase separation time in the porous structure passive radiation refrigeration coating, so that the passive radiation refrigeration coating has excellent radiation cooling performance, good ecological and environmental protection and economic benefits, and has great benefits in solving energy crises and environmental and ecological problems.
[0038] 2. The passive radiation cooling coating textile provided by the present invention uses textile as the base material and the biomaterial polylactic acid as the coating skeleton, and has the advantages of being environmentally friendly, durable and biodegradable. At the same time, the addition of porogens can effectively control the size of the coating pores and the distribution of the pores, regulate the pore structure of the coating, increase the density of the pores, improve the softness of the coating, and enhance the chemical stability of the coating.
[0039] 3. The passive radiation cooling coated textile provided by the present invention has the advantages of high solar spectrum reflectivity and long-wave infrared emissivity, and has excellent wear resistance, acid and alkali resistance, water washability, and aging resistance. BRIEF DESCRIPTION OF THE DRAWINGS
[0040] Figure 1Schematic diagram of the daytime passive radiation cooling performance test device; wherein, (a) is a schematic diagram of the radiation cooling performance test device, and (b) is a schematic diagram of the test environment.
[0041] Figure 2 Actual pictures of polyester fabric and the passive radiation cooling coated polyester fabric prepared in Example 1.
[0042] Figure 3 Spectral reflectance diagram of polyester fabric and passive radiation cooling coated polyester fabric prepared in Example 1. DETAILED DESCRIPTION
[0043] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those generally understood by those skilled in the art of the present invention. The terms used herein in the specification of the present invention are only for the purpose of describing specific embodiments and are not intended to limit the present invention. The term "and / or" used herein includes any and all combinations of one or more related listed items.
[0044] The present invention is further described below in conjunction with the accompanying drawings and specific embodiments so that those skilled in the art can better understand the present invention and implement it, but the embodiments are not intended to limit the present invention.
[0045] Unless otherwise specified, the experimental methods used in the following examples are all conventional methods, and the materials, reagents, etc. used are all available from commercial sources unless otherwise specified.
[0046] The present invention provides a method for preparing a passive radiation cooling coating textile, comprising the following steps:
[0047] (1) dissolving polylactic acid and a porogen in an organic solvent and completely dissolving them at 70 to 110° C. to obtain a coating solution;
[0048] (2) cooling the coating solution obtained in step (1) to 55-80° C., and applying the cooled coating solution to the surface of the textile to obtain a coated textile;
[0049] (3) Immersing the coated textile obtained in step (2) in a hot water bath at 60 to 80° C., taking it out and immersing it in a cold water bath at 15 to 30° C. for phase separation, thereby obtaining a passive radiation cooling coated textile.
[0050] The passive radiation cooling coated textile prepared by the present invention can strongly reflect the solar spectrum and further emit heat through the atmospheric window in the form of infrared radiation, so as to achieve the best passive radiation cooling effect. Compared with traditional fabrics, it can achieve a cooling effect of 5 to 15°C.
[0051] In a specific embodiment, the preparation method comprises the following steps:
[0052] (1) dissolving polylactic acid and a porogen in an organic solvent, stirring at 100 to 1500 rpm for 1 to 3 hours under reflux condensation at 70 to 110° C. to uniformly mix the solution to obtain a coating solution;
[0053] (2) cooling the coating solution obtained in step (1) to 55-80° C., applying the cooled coating solution to the surface of the textile, and obtaining the coated textile after 30-50 seconds;
[0054] (3) Immersing the coated textile obtained in step (2) in a hot water bath at 60 to 80° C. for 40 to 240 seconds, taking it out and immersing it in a cold water bath at 15 to 30° C. for phase separation for 1 to 24 hours, taking the coated textile out of the cold water bath and air-drying it at room temperature or drying it at 50 to 70° C. to obtain a passive radiation cooling coated textile.
[0055] In a specific embodiment, the coating thickness of the passive radiation cooling coated textile is 10 to 300 μm.
[0056] In a specific embodiment, the pore size of the passive radiation cooling coating is 0.5-10 μm, and the solar reflectivity is above 90%.
[0057] In a specific embodiment, in step (1), the stirring method is magnetic stirring, and the stirring process is carried out in a closed state.
[0058] In a specific embodiment, in step (1), the polyethylene glycol is polyethylene glycol 400 (PEG-400).
[0059] In a specific embodiment, in step (1), the relative molecular mass of polyethylene glycol is 350-1000.
[0060] In a specific embodiment, in step (2), the coating amount of the coating solution is 10 to 50 g / m 2 The coating amount refers to the mass of the functional coating fixed per unit area. When the coating amount is small, the passive radiation cooling coating cannot completely and effectively cover the base fabric, thus failing to achieve the desired cooling performance, while when the coating amount is too much, it tends to reduce the feel of the fabric.
[0061] In the following examples, polyethylene glycol is selected as PEG-400, and the textile is selected as polyester fabric (PET), with a gram weight of 97 g / m 2 , deionized water was used for hot and cold water baths.
[0062] In the following embodiments, AM1.5 solar spectrum is used for reflectivity testing, and the spectral reflectivity in the band of 200-2500nm is tested and characterized. The testing instrument used is UV3600 of Shimadzu Corporation of Japan, and the standard backplane used in the test is BaSO4 backplane.
[0063] The following examples are used to evaluate the performance of passive radiation cooling during the day. Figure 1 As shown, the temperature measurements were recorded using a LIANYISH-X (SH-16XL, Dongguan Lianyi Instrument Co., Ltd., China) multi-temperature tester. The radiative cooling performance test device used LIANYI K-type thermocouples with a relative error of less than 0.5 °C between the thermocouples to monitor the ambient, upper and lower surface temperatures. The test device consisted of a polystyrene foam box wrapped in aluminum foil to minimize heat transfer and reflect sunlight. The thermal process of the test fabric box was visualized in real time using an infrared thermal imager (T620, FLIR, Sweden).
[0064] Example 1
[0065] A method for preparing a passive radiation cooling coated polyester fabric comprises the following steps:
[0066] (1) Take 5g PLA, 5mL PEG-400 (M W =350-430) and 0.5 g PVP were placed in a round-bottom flask, 20 mL DMAc was added, and the solution was mixed evenly at 1500 rpm under reflux condensation at 95 ° C for 1 h to obtain a coating solution;
[0067] (2) cooling the coating solution to 60° C., applying the cooled coating solution to the surface of the polyester fabric, and obtaining the coated polyester fabric after 30 seconds;
[0068] (3) The coated polyester fabric was immersed in a hot water bath at 80°C for 40 seconds, taken out and immersed in a cold water bath at 15°C for phase separation for 1 hour, and the coated polyester fabric was taken out from the cold water bath and dried at room temperature to obtain a passive radiation cooling coated polyester fabric, wherein the thickness of the passive radiation cooling coating was 120 μm.
[0069] The polyester fabric (PET) and the passive radiation cooling coated polyester fabric (PLA-PET) prepared in Example 1 were tested and analyzed. Figure 2 The actual picture of polyester fabric and the passive radiation cooling coating polyester fabric prepared in Example 1, Figure 2It can be seen that the passive radiation cooling coating is continuous and uniform on the surface of the polyester fabric. Compared with the polyester fabric without coating, the coating is obviously white; the coating surface has a rough texture effect, which increases the diffuse reflection of the coating, thereby improving the solar spectrum reflectivity without loading nanoparticles, and the rough surface is convenient for subsequent preparation of hydrophobicity, and the soft feel can achieve excellent cooling effect; the average reflectivity of the 120μm coating in the solar spectrum band is as high as 96%; compared with the ambient temperature, in the summer with abundant solar radiation, the cooling effect can reach up to about 15°C.
[0070] Figure 3 The spectral reflectance diagram of polyester fabric and the passive radiation cooling coating polyester fabric prepared in Example 1 is shown in FIG. Figure 3 It can be seen that the reflectivity of the polyester fabric coated with the passive radiation cooling coating is greatly increased compared with the uncoated polyester fabric.
[0071] Example 2
[0072] A method for preparing a passive radiation cooling coated polyester fabric is basically the same as Example 1, except that in step (1), the porogen is only 5 mL PEG-400 (M W =350~430).
[0073] Example 3
[0074] A method for preparing a passive radiation cooling coated polyester fabric is basically the same as that of Example 1, except that in step (1), the porogen is only 0.5 g PVP.
[0075] Example 4
[0076] A method for preparing a passive radiation cooling coated polyester fabric is basically the same as that of Example 1, except that in step (1), the porogen is 0.5 g urea.
[0077] Example 5
[0078] A method for preparing a passive radiation cooling coated polyester fabric is basically the same as that of Example 1, except that in step (1), the porogen is 0.5 g of ammonium polyphosphate.
[0079] Example 6
[0080] A method for preparing a passive radiation cooling coated polyester fabric is basically the same as Example 1, except that in step (1), the porogen is 5 mL PEG-400 (M W =350~430) and 0.5g urea.
[0081] Example 7
[0082] A method for preparing a passive radiation cooling coated polyester fabric is basically the same as Example 1, except that in step (1), the porogen is 5 mL PEG-400 (M W =350~430) and 0.5g ammonium polyphosphate.
[0083] The average reflectivity of the passive radiative cooling coated polyester fabrics prepared in Test Examples 1 to 7 is shown in Table 1:
[0084] Table 1
[0085] Porogen Average reflectivity (%) Example 1 PEG-400+PVP 95.81 Example 2 PEG-400 92.54 Example 3 PVP 93.26 Example 4 Urea 88.70 Example 5 Ammonium Polyphosphate 90.12 Example 6 PEG-400+urea 92.11 Example 7 PEG-400+ammonium polyphosphate 91.85
[0086] As can be seen from Table 1, different porogens have a great influence on the average reflectivity of coated polyester fabrics. PEG-400 and PVP can serve as sites for droplet nucleation and growth during the phase separation process, promote the nucleation process, and stabilize the water droplets in the solution. They can effectively control the morphology of the porous structure coating and increase the porosity, increase the probability of diffuse reflection after the incident light enters, and increase the probability of infrared absorption / emission, which is beneficial to the radiation heat exchange between the porous coating and the atmosphere. In addition, PEG-400 is a liquid and PVP is a solid. When the two are phase separated, the generation sites and separation speeds are inconsistent, which is more conducive to the formation of a multilayer structure with different pore sizes. This structure will enhance the reflectivity of the coating. From the perspective of the feel of the coating, the coating is softer after adding PEG. The improvement in the softness of the coating is due to the excellent plasticity, strong adhesion and excellent wettability of PEG, which strengthens the bonding between the coating and the substrate.
[0087] Example 8
[0088] A method for preparing a passive radiation cooling coated polyester fabric is basically the same as that of Example 1, except that in step (3), the coated polyester fabric is immersed in a hot water bath at 80° C. for 20 seconds.
[0089] Example 9
[0090] A method for preparing a passive radiation cooling coated polyester fabric is basically the same as that of Example 1, except that in step (3), the coated polyester fabric is immersed in a hot water bath at 80° C. for 30 seconds.
[0091] Example 10
[0092] A method for preparing a passive radiation cooling coated polyester fabric is basically the same as that of Example 1, except that in step (3), the coated polyester fabric is immersed in a hot water bath at 80° C. for 60 seconds.
[0093] Embodiment 11
[0094] A method for preparing a passive radiation cooling coated polyester fabric is basically the same as that of Example 1, except that in step (3), the coated polyester fabric is immersed in a hot water bath at 80° C. for 120 seconds.
[0095] Example 12
[0096] A method for preparing a passive radiation cooling coated polyester fabric is basically the same as that of Example 1, except that in step (3), the coated polyester fabric is immersed in a hot water bath at 80° C. for 240 seconds.
[0097] The average reflectivity of the passive radiation cooling coated polyester fabrics prepared in Example 1 and Examples 8 to 12 is shown in Table 2:
[0098] Table 2
[0099]
[0100] It can be seen from Table 2 that the reflectance of the coating first increases with the increase of immersion time. This is because as the phase separation proceeds, the gaps inside the fabric become more obvious and multi-layered. When the time exceeds 40s, the reflectance fluctuates up and down, but there is no sign of further increase. This is because the solution and the hot water bath have a higher temperature, which accelerates the phase separation speed and is almost completed at 40s, so there is no significant increase trend afterwards.
[0101] Embodiment 13
[0102] A method for preparing a passive radiation cooling coated polyester fabric is basically the same as Example 1, except that the cooling temperature of the coating solution in step (2) and the temperature of the hot water bath in step (3) are changed.
[0103] The specific temperature and the corresponding average reflectivity are shown in Table 3:
[0104] Table 3
[0105]
[0106]
[0107]
[0108] As can be seen from Table 2, with the increase of the hot water bath, the reflectivity of the coating reaches the maximum value when the hot water temperature is 65-75℃. The higher the hot water bath temperature, the better the fastness of the coating. Moreover, the decrease of the hot water bath temperature does not achieve the ideal increase in the spectral reflectivity of the coating, but instead decreases it. Moreover, the decrease of the hot water bath temperature will also make the fastness of the coating worse. When the hot water bath temperature is higher than 80℃, the surface of the coating appears uneven, and as the hot water bath temperature increases, the uneven phenomenon will become more obvious. For the cooling temperature of the coating solution, the increase or decrease of the cooling temperature does not increase the emissivity of the coating. On the contrary, the reflectivity of the coating decreases when the cooling temperature is too high. This may be because the solution temperature is too high, and the influence of the hot water bath makes the phase separation speed too fast, thereby affecting the porous structure of the coating, reducing the porous structure, and then affecting the reflectivity of the coating. When the solution temperature is lower than 55℃, a large amount of crystallization occurs in the solution, and the binding ability with the fabric decreases significantly, which is not conducive to the formation of a stable coating.
[0109] Comparative Example 1
[0110] A method for preparing a passive radiation cooling coated polyester fabric is basically the same as that of Example 1, except that in step (3), the coated polyester fabric is not immersed in a hot water bath.
[0111] When phase separation is performed directly in a cold water bath without first performing a hot water bath, the resulting coating has a smooth surface, but weak bonding with the fabric, poor fastness, and powder is produced after drying. This is because direct phase separation in a cold water bath leads to rapid film formation on the surface, but the internal temperature drops sharply, causing PLA to crystallize and precipitate before film formation. The coating obtained by first taking a hot water bath and then a cold water bath has a good bonding fastness with the fabric and is very tough. This is because the hot water bath allows PLA to form a film at high temperature before crystallization and precipitation, so it has good fastness.
[0112] The present invention prepares radiation cooling fabrics with high solar reflectivity and long-wave infrared emissivity by optimizing the coating structure without loading nanoparticles, thereby overcoming the problems of poor fastness of polymer coatings, complex preparation process, high cost, and difficulty in degradation in the prior art. The method of hot water bath followed by cold water bath is adopted to overcome the problem of long phase separation time of the coating, thereby finally realizing the simple and rapid preparation of daytime passive radiation cooling coated textiles.
[0113] Obviously, the above embodiments of the present invention are only examples for clearly illustrating the present invention, and are not intended to limit the embodiments of the present invention. Those skilled in the art should understand that other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the embodiments here. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the claims of the present invention.
Claims
1. A method for preparing a passive radiative cooling coated textile, It is characterized in that The following steps are involved: (1) dissolving polylactic acid and a porogen in an organic solvent and completely dissolving them at 70 to 110° C. to obtain a coating solution; (2) cooling the coating solution obtained in step (1) to 55-80° C., and applying the cooled coating solution to the surface of the textile to obtain a coated textile; (3) Immersing the coated textile obtained in step (2) in a hot water bath at 60 to 80° C., taking it out and immersing it in a cold water bath at 15 to 30° C. for phase separation, thereby obtaining a passive radiation cooling coated textile.
2. The preparation method according to claim 1, It is characterized in that In step (1), the porogen is selected from one or more of polyethylene glycol, ammonium polyphosphate, polyvinyl pyrrolidone and urea.
3. The preparation method according to claim 2, It is characterized in that In step (1), the solid-to-liquid ratio of the polylactic acid and polyethylene glycol is (3-10) g: (0.5-20) mL.
4. The preparation method according to claim 2, It is characterized in that In step (1), the mass ratio of polylactic acid to polyvinyl pyrrolidone is (3-10):(0.5-5).
5. The preparation method according to claim 1, It is characterized in that In step (1), the solid-to-liquid ratio of the polylactic acid to the organic solvent is (3-10) g: (17.5-50) mL.
6. The preparation method according to claim 1, It is characterized in that In step (2), the coating thickness is 10 to 300 μm.
7. The preparation method according to claim 1, It is characterized in that In step (3), the time of immersion in the hot water bath is 40 to 240 seconds.
8. The preparation method according to claim 1, It is characterized in that In step (3), the time of immersion in the cold water bath is 0.01 to 1 h.
9. The passive radiation cooling coated textile obtained by the preparation method according to any one of claims 1 to 8.
10. Use of the passive radiation cooling coated textile according to claim 9 in the preparation of passive radiation cooling materials.
Citation Information
Patent Citations
Porous radiation refrigeration film and preparation method thereof
CN116515219A
Fabric and preparation method thereof
CN118109925A
Method for preparing environment-friendly durable radiation refrigeration coated fabric through pre-gel technology
CN118390310A
Cited By
Polyvinyl alcohol-based aerogel with radiation cooling and fireproof characteristics as well as preparation method and application of polyvinyl alcohol-based aerogel
CN120059289A
Flame-retardant radiant refrigeration fabric and preparation method and application thereof