Method for solving uneven continuous dyeing of loose cotton
By using loosening treatment, atomizing permeable agent, optimized dyeing liquid ratio and multiple impregnation and rolling technology in continuous dyeing of loose cotton, the problems of uneven dyeing and sewage treatment are solved, and efficient and environmentally friendly dyeing effect is achieved , improves dyeing uniformity and production efficiency.
Patent Information
- Application Number
- CN202411285540.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-13
- Publication Date
- 2024-11-26
AI Technical Summary
There is a problem of uneven dyeing in the continuous dyeing technology of loose cotton, resulting in poor color consistency, uneven dye absorption, and the sewage generated during the traditional dyeing process is difficult to treat, which pollutes the environment.
Through the loosening treatment, a uniform cotton mesh is formed, and the permeable agent is sprayed with an atomization device to optimize the volume ratio of dye liquid to alkali agent. Mechanical centrifugal dehydration and multiple impregnation and rolling technology are used to control the liquid tape rate, combining organic alternative alkali and Inorganic bases regulate pH and use phosphate penetrants to ensure uniform distribution and firm adhesion of dyes.
It significantly improves dye uniformity and depth, reduces dye hydrolysis, reduces sewage treatment difficulty, reduces cost, meets environmental protection requirements, and improves production efficiency and product quality.
Smart Images

Figure SMS_1 
Figure SMS_2 
Figure SMS_3
Abstract
Description
Technical Field
[0001] The present application relates to the field of dyeing, and more specifically, to a method for solving the problem of uneven continuous dyeing of loose cotton. Background Art
[0002] For a long time, China's color spinning industry has used more than 1 million tons of dyed fibers every year. Although the technology of dyeing cotton with traditional dye vats is mature, the dyeing cost is high and the dye consumption is large. Secondly, there is the problem of sewage generated during the dyeing process. Traditional dye vat dyeing is often accompanied by the discharge of high-salt wastewater, which contains a large amount of difficult-to-degrade organic matter and salt. It is not only difficult to treat, but also pollutes the environment.
[0003] In the face of the various drawbacks of traditional dyeing technology and increasingly stringent environmental protection requirements, loose cotton continuous dyeing technology came into being. Loose cotton continuous dyeing refers to the process of dyeing loose cotton (i.e., unspun cotton fibers) through continuous equipment and technology, which subverts the order of traditional textile printing and dyeing, that is, dyeing the raw materials first and then spinning them, thus realizing the integration and continuous production of dyeing and spinning, greatly improving production efficiency and reducing labor costs. Compared with traditional dye vat dyeing, loose cotton continuous dyeing technology adopts salt-free, normal temperature and low water ratio, which reduces the salt content in sewage from the source and reduces the difficulty and cost of wastewater treatment.
[0004] Although there are many advantages to continuous dyeing of loose cotton, the current technology still has many shortcomings. First, it is difficult to accurately control the liquid carrying rate due to the thick cotton layer. Different parts of the cotton layer absorb different amounts of dye during the dyeing process, resulting in poor color consistency after dyeing. Secondly, loose cotton contains wax and water repellent, which makes it difficult for the dye to quickly and evenly enter the cotton layer in a short time. In addition, the pH of the dye is high when it is dyed at room temperature and the alkali agent is co-bathed, which easily hydrolyzes and causes color difference at the head and tail of the cotton net. Therefore, the current technology for continuous dyeing of loose cotton cannot meet the quality requirements of colored cotton for color spinning. Summary of the invention
[0005] In order to improve the uniformity of continuous dyeing of loose cotton and reduce color difference, the present application provides a method for solving the unevenness of continuous dyeing of loose cotton.
[0006] The present application provides a method for solving the problem of uneven continuous dyeing of loose cotton by adopting the following technical solution: A method for solving the problem of uneven continuous dyeing of loose cotton comprises the following steps: The cotton fibers are opened to form a cotton web of uniform thickness; The penetrant is mixed with water to obtain a penetrant solution with a concentration of 1-2 g / L, and the penetrant solution is sprayed onto the cotton mesh through an atomizing device; Alkali agent and dye solution are injected into the dye tank in a volume ratio of 1:(2-5), and when the liquid level is reached, the continuous dyeing equipment is started, and the cotton web is immersed in the dye tank, and after immersion, the cotton web is squeezed by a pressing roller; The cotton liquid content is quickly tested by mechanical centrifugal dehydration of the cotton web for 20-30 seconds, and the cotton web is squeezed by a padder to control the liquid content at 100-120%; After the dyed cotton roll is rolled up, when the radius of the cotton roll reaches 40-45cm, wrap the surface and both ends of the cotton roll with po film, place the cotton roll on a horizontal rack, keep the cotton roll rotating at a low speed of 1-20r / min, and place it at room temperature for 16-24h. After completion, take out the cotton roll, wash it with water and dry it.
[0007] By adopting the above technical scheme, cotton fiber is arranged into a cotton net with uniform thickness through opening treatment, which fundamentally solves the problem of unstable liquid carrying rate caused by inconsistent cotton layer thickness. Uniform cotton net is conducive to the uniform distribution of dye and penetrant in cotton fiber, thereby improving dyeing uniformity. Penetrant solution is evenly sprayed on cotton net by atomizing device, and this step significantly enhances the hydrophilicity of cotton fiber, so that dye can penetrate into cotton fiber inside more easily and quickly in subsequent dyeing process, effectively improving the problem of uneven dyeing caused by water repellent of cotton fiber. By controlling the volume ratio of dye liquor and alkali agent at 2-5:1, dyeing environment is optimized, and the influence of adverse factors such as dye liquor hydrolysis on dyeing effect is reduced. The proportioning of the present application helps the stable attachment of dye on cotton fiber, improves dyeing efficiency and quality. Through mechanical centrifugal dehydration, the cotton liquid carryover rate is quickly tested and controlled within the range of 100-120%. This step greatly improves the efficiency of cotton net liquid carryover rate testing and reduces the probability of dye hydrolysis in the dye tank. Secondly, the cotton net liquid carryover rate can be accurately controlled to ensure that the cotton fiber can fully absorb the dye during the dyeing process and will not be over-dyed or wasted due to excessive liquid carryover rate. After the dyed cotton roll is wrapped with po film, it is rotated at a low speed on a horizontal rack and placed at room temperature for a period of time, which helps the dye to further diffuse and evenly distribute inside the cotton fiber, and reduces the uneven dyeing caused by factors such as inner and outer layers and head and tail differences. At the same time, placing it at room temperature avoids the problem of dye migration or discoloration that may be caused by high temperature, and protects the dyeing results. The solution of the present application effectively solves the uneven problem in the continuous dyeing of loose cotton, and provides strong support for the mass production of continuous dyeing of loose cotton.
[0008] Furthermore, the dye solution includes a dye, a penetrant and deionized water. The penetrant and the dye are added to the deionized water and mixed evenly to obtain the dye solution. The concentration of the penetrant in the dye solution is 6-8 g / L.
[0009] By adopting the above technical scheme, the penetrant and the dye are pre-mixed in water to prepare a uniform dye solution, rather than being mixed together with the alkali agent, which can avoid the decrease in the penetration performance of the penetrant under super-alkaline conditions, thereby reducing the permeability of the cotton web; secondly, the amount of penetrant used is 6-8g / L, which can effectively ensure that the cotton web is quickly wetted during dyeing and ensure that the dye and alkali agent are quickly and evenly dyed, thereby improving the uniformity of dyeing.
[0010] Optionally, the alkali agent includes an organic substitute alkali and an inorganic alkali, the organic substitute alkali has a concentration of 1-10 g / L, and the inorganic alkali includes flake alkali with a concentration of 0.5-8 g / L and soda ash with a concentration of 10-30 g / L.
[0011] By adopting the above technical scheme, the synergistic effect of organic substitute alkali and inorganic alkali can more effectively adjust the pH value of the dye liquor, promote the adsorption of dye molecules on the surface of cotton fibers and the penetration into the fibers. This dual action mechanism enables the dye to be more evenly distributed on the cotton fibers, improving the depth and brightness of the dyeing. By controlling the concentration of organic substitute alkali and inorganic alkali, the ionic strength and charge distribution in the dye liquor can be optimized, and the aggregation or repulsion of dyes caused by charge repulsion or attraction can be reduced, thereby further improving the uniformity of dyeing. This is particularly important for solving the common uneven problems of left, middle and right, inner and outer layers, and head and tail differences in loose cotton dyeing. The addition of inorganic alkali helps to stabilize the pH value in the dye liquor and reduce the hydrolysis of dyes caused by pH fluctuations. The reduction in hydrolysis means that the effective utilization rate of dyes in the dyeing process is improved, reducing dye waste and environmental pollution. Organic substitute alkalis usually have better biodegradability and environmental protection. Their use can reduce chemical damage to cotton fibers and protect the original quality of fibers. At the same time, the appropriate use of inorganic alkalis also helps to enhance the hygroscopicity and softness of cotton fibers and improve the comfort of the final product.
[0012] Optionally, the penetrant comprises a phosphate ester.
[0013] By adopting the above technical scheme, the phosphate penetrant can quickly and evenly penetrate into the interior of the cotton fiber, so that the dye solution can contact the fiber more fully, thereby improving the uniformity of dyeing. The phosphate penetrant can react with the fiber components to form a phosphate compound, which can enhance the binding force between the dye and the fiber, help the dye to adhere more firmly to the fiber, and improve the fastness and durability of the dyeing. Spraying the phosphate penetrant solution onto the cotton net through an atomizing device can make the penetrant evenly distributed on the surface and inside of the cotton fiber, thereby reducing the phenomenon of uneven dyeing. As a relatively environmentally friendly surfactant, the wastewater generated during the use of the phosphate penetrant has little impact on the environment.
[0014] Optionally, the specific method for calculating the liquid carryover rate by mechanical centrifugal dehydration is: take samples at both ends and the center of the cotton web and weigh them respectively, record the wet weight as m1, put the cotton web sample into a centrifugal dehydrator for dehydration for 20-30s, take out and weigh the weight of the cotton web sample after dehydration as m2, calculate the liquid carryover rate = (m1-m2 / coefficient) / m2 / coefficient, when the difference in liquid carryover rate of the cotton web samples is greater than 10%, adjust the roller pressure so that the difference in liquid carryover rate between samples at different parts is less than 10%.
[0015] By adopting the above technical solution, the liquid carrying rate of each part of the cotton web can be quickly calculated through the weight change before and after mechanical dehydration, and the problem of inconsistent liquid carrying rate caused by factors such as uneven cotton web thickness, permeability difference or uneven padding pressure can be discovered and corrected in time. By adjusting the cotton layer density and roller pressure, the difference in liquid carrying rate between samples in different parts is less than 10%, ensuring that the cotton web can evenly absorb dyes during the dyeing process, which helps to reduce the problem of uneven dyeing caused by inconsistent liquid carrying rate. Secondly, it can effectively shorten the time for testing liquid carrying rate and reduce the probability of dye hydrolysis in the dye tank, thereby improving the uniformity of dyeing.
[0016] Optionally, the cotton mesh has a thickness of 10-20 cm and a density of 2-3 kg / m.
[0017] By adopting the above technical solution, the uniform thickness and density of the cotton mesh ensure that the dye can penetrate into the fiber more evenly, avoiding the problem of uneven dyeing caused by uneven thickness or density.
[0018] Optionally, a plurality of dyeing tanks are continuously arranged, and adjacent dyeing tanks are connected and arranged at intervals of a slope of 10-20 degrees, and the cotton web is squeezed once by a pressing roller after each immersion in the liquid tank.
[0019] By adopting the above technical solution, the continuous multiple dyeing tanks allow the cotton net to be dipped and rolled multiple times, reducing the waiting time and tank changing operation, thereby greatly improving the dyeing efficiency. The air in the cotton net is discharged through multiple squeezing, which greatly facilitates the penetration of the dye liquid. The slope design helps the dye liquid to be evenly distributed in the dyeing tank. Through the continuous multiple dipping and rolling processes, the dye adheres to the cotton net more firmly and evenly, improving the overall uniformity of dyeing.
[0020] Optionally, a polyester belt is used in the rolling mill, and the polyester belt is provided with a plurality of mesh holes passing through two sides.
[0021] By adopting the above technical scheme, the presence of the mesh allows the pressing liquid to quickly flow out of the cotton layer during the pressing process of the rolling mill, preventing the pressing liquid from concentratedly flowing out from both ends, resulting in a low liquid carryover rate in the middle part of the cotton mesh and a high liquid carryover rate on both sides, ensuring that the deviations in the left, middle and right liquid carryover rates are within a controllable range, and avoiding uneven dyeing due to large differences in liquid carryover rates.
[0022] Optionally, a metering pump and a liquid level controller are provided in the dyeing tank, and the dye solution and alkali agent are injected into the metering pump for storage. The liquid level controller is used to monitor the liquid level in the dyeing tank. When the liquid level is lower than 120L, the metering pump starts to replenish the liquid, and when the liquid level is lower than 60L, the continuous dyeing equipment stops.
[0023] By adopting the above technical solution, by real-time monitoring of the liquid level in the dye tank and automatic liquid replenishment when the liquid level is lower than the set threshold, the stability of the liquid level in the dye tank can be ensured, and the stability of the cotton net during dyeing can be ensured, avoiding uneven dyeing caused by different dyeing rates of the cotton net due to different liquid levels.
[0024] In summary, this application has the following beneficial effects: 1. Since the present application forms a uniform cotton web through a loosening process, the hydrophilicity of the cotton web is greatly improved by methods such as atomizing the penetrant before entering the dyeing tank, selecting a penetrant with strong alkali resistance, chemically preparing the penetrant together with the dye solution, and multiple immersion and rolling in the dyeing tank. The dye solution and alkali agent chemical preparation method and ratio are optimized, the mechanical centrifugal rapid test of the liquid carryover rate is reduced, and the machine is stopped for waiting for the test results, etc. to reduce the hydrolysis of the dye during the process. The rolling belt with mesh allows the liquid to be quickly discharged to avoid large deviations in the liquid carryover rate between the two sections and the middle, and the mechanical centrifugal rapid test of the liquid carryover rate ensures accurate control of the liquid carryover rate of the cotton layer. After dyeing, the cotton roll is wrapped and rotated at a low speed and placed at room temperature to promote uniform diffusion of the dye, which effectively solves the unevenness problem in continuous dyeing of loose cotton and provides reliable technical support for large-scale production.
[0025] 2. In this application, the synergistic effect of organic substitute alkali and inorganic alkali is preferably used to optimize the pH value of the dye solution and promote the uniform adsorption and penetration of dye molecules in cotton fibers, thereby significantly improving the uniformity, depth and brightness of dyeing. This mechanism reduces the problem of dye unevenness caused by charge action, effectively inhibits dye hydrolysis, and improves dye utilization and environmental protection. At the same time, this combination also protects the quality of cotton fibers, enhances their hygroscopicity and softness, and provides an efficient and environmentally friendly solution for loose cotton dyeing.
[0026] 3. The method of the present application has low bath ratio, normal temperature dyeing, no salt addition, and low difficulty in sewage treatment. The black comprehensive comparison with traditional vat dyeing is 500RMB / T lower. The dyeing is done at room temperature and without extrusion, the fiber is not damaged or agglomerated, the physical properties of the cotton fiber itself are retained, and the spinnability is good. Dyeing does not require the addition of sodium sulfate to promote dyeing, and the sewage does not contain salt, which greatly reduces the difficulty of sewage treatment. Secondly, the water content is lower than that of conventional vat dyeing, and the total amount of sewage is low, which meets the national green environmental protection requirements. DETAILED DESCRIPTION
[0027] The present application is further described in detail below in conjunction with the examples. It is particularly noted that if no specific conditions are specified in the following examples, the experiments are carried out according to conventional conditions or the conditions recommended by the manufacturer. Unless otherwise specified, the raw materials used in the following examples can be obtained from common commercial sources. Example
[0028] Example 1 A method for solving the problem of uneven continuous dyeing of loose cotton: The cotton fibers are loosened and processed into a web through a cotton plucking machine, a cotton box, and a web forming machine to form a cotton web of uniform thickness. The thickness of the cotton web is controlled at 15±2cm and the density is 2.5±0.2KG / m; The phosphoric acid diester is mixed with water to obtain a penetrant solution with a concentration of 1.5 g / L, and the penetrant solution is sprayed onto the cotton net through a high-level atomization device; Prepare alkali and dye liquor. The alkali is obtained by mixing organic substitute alkali, flake alkali, soda ash and water, wherein the concentration of organic substitute alkali triethanolamine is 5g / L, the concentration of flake alkali sodium hydroxide is 5G / L, and the concentration of soda ash sodium carbonate is 20g / L. Dye liquor is prepared by mixing dye, dispersant, phosphoric acid diester and water, wherein the mass concentration of dye is 6.0% reactive black WNN, 0.5% reactive red 195, the concentration of dispersant SM-1501 in the dye liquor is 2g / L, and the concentration of phosphoric acid diester is 6g / L, and the material is stirred for 30 minutes to obtain dye liquor.
[0029] The dye solution and alkali agent are injected into the dye tank in a volume ratio of 3.5:1. The dye tank of the continuous dyeing equipment is provided with a metering pump and a liquid level controller. The dye solution and alkali agent are injected into the metering pump for storage. The liquid level controller is used to monitor the liquid level in the dye tank. The continuous dyeing equipment is started and the whole machine is turned on. The whole machine speed is 4m / Min. The cotton net is immersed in the dye tank and pressurized by a roller after immersion. The dye tank is divided into 4 small liquid tanks, which are arranged with a slope of 20 degrees. The metering pump draws liquid from the highest liquid tank and injects it. After filling, it is reserved in the front tank in turn. The cotton is fed from the front cotton tank. 4 immersions and 4 rollings are adopted. The liquid is rolled in the liquid tank after each immersion. Once, when the cotton web enters the padding machine and is reeled up, stop the machine and take samples of the left, middle and right of the cotton roll, weigh them, record the wet weight m1, put the cotton sample into a small centrifugal dehydrator for dehydration for 20 seconds, take it out and weigh the weight after dehydration m2, calculate the liquid carryover rate = (m1-m2 / coefficient) / m2 / coefficient. The coefficient is related to the fiber type and physical properties. Generally, the test method for the same kind of cotton is the same, the coefficient is relatively stable, the overall liquid carryover rate is controlled at 100-120%, and the left, middle and right deviations do not exceed 10%. If the deviation is large, adjust the padding roller pressure and the cotton web density, take samples for testing again, and start the machine after the liquid carryover rate is adjusted to be stable.
[0030] After the cotton rolls are wound up and dyed, when the radius of the cotton rolls reaches 40-45cm, wrap the surface and both ends of the cotton rolls with plastic film, hang them on a horizontal rack, keep the cotton rolls rotating at a low speed of 10r / min, and place them at room temperature for 20 hours. After completion, the cotton rolls are hung into the continuous washing equipment, taken out for washing, and then put into the dryer for drying.
[0031] Example 2 A method for solving the problem of uneven continuous dyeing of loose cotton: the difference from Example 1 is that a single dyeing tank is used.
[0032] Example 3 A method for solving the problem of uneven continuous dyeing of loose cotton: the difference from Example 1 is that the liquid is not automatically replenished through a liquid level controller.
[0033] Example 4 A method for solving the problem of uneven continuous dyeing of loose cotton: the difference from Example 1 is that the polyester belt is not provided with through mesh holes.
[0034] Example 5 A method for solving the problem of uneven continuous dyeing of loose cotton: The method is different from Example 1 in that fatty alcohol polyoxyethylene ether is used as the penetrant.
[0035] Example 6 A method for solving the problem of uneven continuous dyeing of loose cotton: the difference from Example 1 is that the volume ratio of the alkali agent to the dye solution is 1:2.
[0036] Example 7 A method for solving the problem of uneven continuous dyeing of loose cotton: the difference from Example 1 is that the volume ratio of the alkali agent to the dye solution is 1:5.
[0037] Example 8 A method for solving the problem of uneven continuous dyeing of loose cotton: The method is different from Example 1 in that the concentration of phosphate in the penetrant solution is 1 g / L.
[0038] Example 9 A method for solving the problem of uneven continuous dyeing of loose cotton: The method is different from Example 1 in that the concentration of phosphate in the penetrant solution is 2 g / L.
[0039] Example 10 A method for solving the problem of uneven continuous dyeing of loose cotton: the difference from Example 1 is that the concentration of the organic substitute alkali in the alkali agent is 1 g / L, the concentration of flake alkali in the alkali agent is 0.5 g / L, and the concentration of soda ash is 10 g / L.
[0040] Embodiment 11 A method for solving the problem of uneven continuous dyeing of loose cotton: the difference from Example 1 is that the concentration of the organic substitute alkali in the alkali agent is 10 g / L, the concentration of flake alkali in the alkali agent is 8 g / L, and the concentration of soda ash is 30 g / L.
[0041] Comparative Example Comparative Example 1 A method for solving the problem of uneven continuous dyeing of loose cotton: the difference from Example 1 is that the alkali agent contains 1-8 g / L of inorganic alkali caustic soda and 20-50 g / L of soda ash.
[0042] Comparative Example 2 A method for solving the problem of uneven continuous dyeing of loose cotton: the difference from Example 1 is that the concentration of the penetrant is 0.5 g / L.
[0043] Comparative Example 3 A method for solving the problem of uneven continuous dyeing of loose cotton: the difference from Example 1 is that the concentration of the penetrant is 2.5 g / L.
[0044] Comparative Example 4 A method for solving the problem of uneven continuous dyeing of loose cotton: the difference from Example 1 is that the liquid carrying rate is controlled at 130%.
[0045] Comparative Example 5 A method for solving the problem of uneven continuous dyeing of loose cotton: the difference from Example 1 is that the liquid carrying rate is controlled at 90%.
[0046] Comparative Example 6 A method for solving the problem of uneven continuous dyeing of loose cotton: the difference from Example 1 is that the alkali agent and the dye solution are in a volume ratio of 1:1.
[0047] Comparative Example 7 A method for solving the problem of uneven continuous dyeing of loose cotton: the difference from Example 1 is that the volume ratio of the alkali agent to the dye solution is 1:6.
[0048] Comparative Example 8 A method for solving the problem of uneven continuous dyeing of loose cotton: the difference from Example 1 is that the penetrant solution is not sprayed before the cotton web enters the dyeing tank.
[0049] Performance testing Detection Methods Color difference detection: The dyed cotton yarns obtained in Examples 1-5 and Comparative Examples 1-5, with a yarn count of 32S / 1, were woven into 10cm*20cm cotton yarn fabrics. The color data of the edges and the center of both ends of the cotton yarn fabrics were tested using a Datacolor colorimeter. The standard sample (extra-dark black) value was used as a reference. The color data difference between the dyed cotton yarn color data obtained in the Examples and Comparative Examples and the color data of the standard sample was calculated, and the average color difference value was calculated, as follows: Table 1 Color difference detection data Table 2 Standard sample color data The following conclusions can be drawn from the above tests: According to Example 1 and Comparative Example 1 combined with Table 1, it can be seen that the synergistic effect of the organic substitute alkali and the inorganic alkali can more effectively adjust the pH value of the dye solution, ensure the pH stability of the dye solution, reduce the hydrolysis of the dye, and promote the adsorption of the dye molecules on the surface of the cotton fiber and the penetration into the fiber. This dual action mechanism enables the dye to be more evenly distributed on the cotton fiber, improves the depth and brightness of the dyeing, and solves the problem of uneven continuous dyeing of loose cotton.
[0050] According to Example 1 and Comparative Examples 2-3, it can be seen from Table 1 that by uniformly spraying the penetrant solution having a concentration of 1-2g / L onto the cotton net through an atomizing device, the hydrophilicity of the cotton fiber is significantly enhanced, so that the dye can more easily and quickly penetrate into the inside of the cotton fiber in the subsequent dyeing process, effectively improving the problem of uneven dyeing of the dye caused by the water repellency of the cotton fiber. When the penetrant concentration is too high, the cotton fiber cannot fully and effectively utilize all the penetrants. This will result in too much penetrant residue on the surface or inside of the cotton fiber. These residues may affect the subsequent dyeing process, such as unnecessary reactions with the dye, resulting in poor dyeing effect or color distortion. The penetrant concentration is too low, and the effect of improving the hydrophilicity will be greatly reduced, causing the dye to still be difficult to uniformly penetrate into the inside of the cotton fiber in the dyeing process, thereby being unable to effectively solve the problem of uneven dyeing of the dye.
[0051] According to Example 1 and Comparative Examples 4-5 combined with Table 1, it can be seen that controlling the cotton liquid carryover rate within the range of 100-120% ensures that the cotton fiber can fully absorb the dye during the dyeing process. If the liquid carryover rate is too high, the probability of dye hydrolysis is high during cold stacking. If it is too low, the padding pressure is too high and the padding liquid is too high, which affects the cotton web forming and causes a large difference in the cotton web liquid carryover rate.
[0052] According to Example 1 and Comparative Examples 6-7 combined with Table 1, it can be seen that by controlling the volume ratio of the alkali agent to the dye solution (1:2-5) and reducing the mixing time of the dye solution and the alkali solution, the dyeing environment is optimized and the influence of adverse factors such as dye solution hydrolysis on the dyeing effect is reduced. The ratio and mixing method of the present application help the dye to adhere stably to the cotton fiber and improve the dyeing quality.
[0053] According to Example 1 and Comparative Example 8 in combination with Table 1, it can be seen that the penetrant solution is evenly sprayed onto the cotton net through an atomizing device. This step significantly enhances the hydrophilicity of the cotton fiber, allowing the dye to penetrate into the cotton fiber more easily and quickly during the subsequent dyeing process, effectively improving the problem of uneven dyeing caused by the water repellency of the cotton fiber.
[0054] According to Examples 1-5 and Table 1, it can be seen that by finely controlling the concentration of organic substitute alkali and inorganic alkali, optimizing the ionic strength and charge distribution of the dye liquor, reducing dye aggregation or repulsion, combining atomization spraying of phosphate penetrant to ensure comprehensive and uniform penetration of cotton fibers, using mechanical dehydration to monitor the liquid rate and adjust the padding pressure to achieve a liquid rate difference of less than 10%, and ensuring dyeing uniformity. The continuous multi-trough immersion dyeing and rolling design improves efficiency, the slope design promotes uniform distribution of the dye liquor, the mesh design optimizes the outflow of the rolling liquid, and the automatic liquid replenishment system ensures the stability of the dye tank liquid level, which together improves the dyeing uniformity, efficiency and production line stability.
[0055] According to Example 1 and Examples 6-11 in combination with Table 1, it can be seen that the ratio of the alkali agent to the dye solution, the concentration of the penetrant, and the composition and content of the alkali agent in the present application can enable the loose cotton continuous dyeing method to achieve good results. The average △E of the color difference between the front and back sections and the left, middle and right sides of the overall cotton roll is ≤0.4, and the color uniformity achieves excellent results. Among them, the method in Example 1 is the best in the present application.
[0056] This specific embodiment is merely an explanation of the present application and is not a limitation of the present application. After reading this specification, those skilled in the art may make modifications to the present embodiment without any creative contribution as needed, but such modifications are protected by the patent law as long as they are within the scope of the claims of the present application.
Claims
1. A method for solving the problem of uneven continuous dyeing of loose cotton, characterized in that: The following steps are involved: The cotton fibers are opened to form a cotton web of uniform thickness; The penetrant is mixed with water to obtain a penetrant solution with a concentration of 1-2 g / L, and the penetrant solution is sprayed onto the cotton mesh through an atomizing device; Alkali agent and dye solution are injected into the dye tank in a volume ratio of 1:(2-5), and when the liquid level is reached, the continuous dyeing equipment is started, and the cotton web is immersed in the dye tank, and after immersion, the cotton web is squeezed by a pressing roller; The cotton web liquid content is quickly tested by mechanical centrifugal dehydration for 20-30 seconds, and the cotton web is squeezed by a padder to control the liquid content at 100-120%; After the dyed cotton roll is rolled up, when the radius of the cotton roll reaches 40-45cm, wrap the surface and both ends of the cotton roll with po film, place the cotton roll on a horizontal rack, keep the cotton roll rotating at a low speed of 1-20r / min, and place it at room temperature for 16-24h. After completion, take out the cotton roll, wash it with water and dry it.
2. The method for solving the problem of uneven continuous dyeing of loose cotton according to claim 1, characterized in that: The alkali agent includes an organic substitute alkali and an inorganic alkali, wherein the concentration of the organic substitute alkali is 1-10 g / L, and the inorganic alkali includes flake alkali with a concentration of 0.5-8 g / L and soda ash with a concentration of 10-30 g / L.
3. The method for solving the problem of uneven continuous dyeing of loose cotton according to claim 1, characterized in that: The penetrant includes a phosphate ester.
4. The method for solving the problem of uneven continuous dyeing of loose cotton according to claim 1, characterized in that: The specific method for calculating the liquid carrying rate through mechanical centrifugal dehydration is: take samples at both ends and the center of the cotton web and weigh them, record the wet weight as m1, put the cotton web sample into a centrifugal dehydrator for dehydration for 20-30s, take out and weigh the weight of the dehydrated cotton web sample as m2, calculate the liquid carrying rate = (m1-m2 / coefficient) / m2 / coefficient, when the difference in liquid carrying rate of the cotton web samples is greater than 10%, adjust the pressure of the rolling mill so that the difference in liquid carrying rate between samples at different parts is less than 10%.
5. The method for solving the problem of uneven continuous dyeing of loose cotton according to claim 1, characterized in that: The cotton mesh has a thickness of 10-20 cm and a density of 2-3 kg / m.
6. The method for solving the problem of uneven continuous dyeing of loose cotton according to claim 1, characterized in that: A plurality of dyeing tanks are arranged in series, and adjacent dyeing tanks are connected and arranged at intervals of a slope of 10-20 degrees. The cotton web is squeezed once by a pressing roller after being dipped in the liquid tank once.
7. The method for solving the problem of uneven continuous dyeing of loose cotton according to claim 6, characterized in that: The padder uses a polyester belt, and the polyester belt is provided with a plurality of mesh holes penetrating both sides.
8. The method for solving the problem of uneven continuous dyeing of loose cotton according to claim 1, characterized in that: The dyeing tank is provided with a metering pump and a liquid level controller. The dye solution and alkali agent are injected into the metering pump for storage. The liquid level controller is used to monitor the liquid level in the dyeing tank. When the liquid level is lower than 120L, the metering pump starts to replenish the liquid. When the liquid level is lower than 60L, the continuous dyeing equipment stops.