Method for improving softness and strength performance of facial tissue
By mixing and embossing polyamide epoxychlorophenyl resin, dimerglyceride dioleate and glycerol-water solvent with wood pulp slurry, the problems of low adhesion and high cost of existing facial tissue paper are solved, and the problem of low adhesion and high cost of existing tissue paper is achieved. The softness and strength performance of facial tissue paper is significantly improved, and is suitable for large-scale production.
Patent Information
- Application Number
- CN202411336507.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-24
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2044-09-24
AI Technical Summary
The existing facial tissue paper has low adhesion and high cost due to the use of amino silicone oil as a softener, and the formula is complicated.
The process is simplified by the process of drying and embossing the process of using polyamide epoxychlorohydrin, dioleate dimer glycerol-water solvent and wood pulp slurry. , reduces costs.
It significantly improves the softness and strength properties of facial tissue paper, is low in cost and is suitable for large-scale production.
Smart Images

Figure BDA0005058511170000061
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of daily paper, and in particular relates to a method for improving the softness and strength properties of facial tissue paper. Background Art
[0002] Facial tissue is inseparable from people's daily life. In recent years, both the production and consumption of facial tissue have been increasing year by year, indicating that people's demand for daily paper is increasing. With the improvement of living standards, people's requirements for its quality and experience are also increasing.
[0003] Most of the facial tissues used daily use amino silicone oil as a softener, which has the disadvantages of low adhesion and the need for emulsification, which leads to high costs and complex formulas. Summary of the invention
[0004] In view of this, the object of the present invention is to provide a method for improving the softness and strength of facial tissue. The method provided by the present invention has low cost, simple formula and easy operation, and the prepared facial tissue has significantly improved softness and strength compared with the facial tissue prepared by using amino silicone oil as a softener in the prior art.
[0005] In order to achieve the above object, the present invention provides the following scheme:
[0006] The present invention provides a method for improving the softness and strength properties of facial tissue paper, comprising the following steps:
[0007] The polyamide epichlorohydrin resin, diglycerol dioleate, glycerol-water solvent and wood pulp slurry are mixed, and first decomposition and papermaking are performed in sequence to obtain a formed facial tissue base paper;
[0008] The addition amount of the polyamide epichlorohydrin resin is 3 to 12 kg / t of the absolute dry mass of the wood pulp slurry; the addition amount of the diglycerol dioleate is 2 to 8 kg / t of the absolute dry mass of the wood pulp slurry.
[0009] Preferably, the mass concentration of glycerol in the glycerol-water solvent is 70-80%; and the mass ratio of diglycerol dioleate to the glycerol-water solvent is 1:1.
[0010] Preferably, the wood pulp slurry includes bleached coniferous kraft pulp slurry and bleached hardwood pulp slurry.
[0011] Preferably, after the papermaking is completed, the obtained facial tissue base paper is dried and embossed in sequence.
[0012] Preferably, the embossing pressure is 0.5 MPa.
[0013] Preferably, the preparation of the wood pulp slurry comprises the following steps:
[0014] The wood pulp board is soaked in the first water, the obtained pulp board is torn into shredded paper pieces, and then the second water is added, and the second decomposition and beating are carried out in sequence, the water is dried, and then the pulp is broken up to obtain the wood pulp slurry.
[0015] Preferably, when the wood pulp slurry includes bleached coniferous kraft pulp slurry and bleached hardwood pulp slurry, the wood pulp pulp board includes bleached coniferous kraft pulp board and bleached hardwood pulp pulp board, the mass ratio of the bleached coniferous kraft pulp board and the bleached hardwood pulp board is (7-8):(2-3) based on absolute dry pulp.
[0016] Preferably, the second decongestion time is 4 to 6 minutes.
[0017] Preferably, the beating is performed to a beating degree of 28 to 32° SR.
[0018] Preferably, the volume ratio of the mass of the wood pulp board to the first water is 360g:5L; the volume ratio of the mass of the wood pulp board to the second water is 360g:18L.
[0019] The invention provides a method for improving the softness and strength properties of facial tissue paper, comprising the following steps: mixing polyamide epichlorohydrin resin, diglycerol dioleate, glycerol-water solvent and wood pulp slurry, and sequentially performing first deflaking and papermaking to obtain formed facial tissue paper base paper; the addition amount of the polyamide epichlorohydrin resin is 6-12 kg / t of the absolute dry pulp mass of the wood pulp slurry; the addition amount of the diglycerol dioleate is 2-8 kg / t of the absolute dry pulp mass of the wood pulp slurry.
[0020] Polyamide epichlorohydrin resin (PAE) is a water-soluble, cationic, thermosetting resin that does not contain formaldehyde polymers, is non-toxic and odorless, can be manufactured under neutral, slightly alkaline and acidic conditions, and has a wide range of applicable pH values; PAE can significantly improve the dry and wet strength of the page, and can be used in the production of all types of paper with wet strength requirements. Polyamide epichlorohydrin resin and diglycerol dioleate can enhance the softness of facial tissue and the physical strength of paper. Diglycerol dioleate can be evenly dispersed in a glycerol-water solvent, and does not hinder the dispersion of PAE in the solution system, so that both diglycerol dioleate and PAE can be evenly dispersed in a glycerol-water solvent system without the need for emulsification, which simplifies the facial tissue preparation process and reduces costs.
[0021] Furthermore, the present invention can significantly improve the softness of facial tissue through embossing. DETAILED DESCRIPTION
[0022] The present invention provides a method for improving the softness and strength properties of facial tissue paper, comprising the following steps:
[0023] The polyamide epichlorohydrin resin, diglycerol dioleate, glycerol-water solvent and wood pulp slurry are mixed, and first decomposition and papermaking are carried out in sequence to obtain formed facial tissue base paper.
[0024] Unless otherwise specified, the materials and equipment used in the present invention are commercially available.
[0025] In the present invention, the wood pulp slurry preferably includes bleached coniferous kraft pulp slurry and bleached hardwood pulp slurry. In the present invention, the preparation of the wood pulp slurry preferably includes the following steps:
[0026] The wood pulp board is soaked in the first water, the obtained pulp board is torn into shredded paper pieces, and then the second water is added, and the second decomposition and beating are carried out in sequence, the water is dried, and then the pulp is broken up to obtain the wood pulp slurry.
[0027] In the present invention, when the wood pulp slurry preferably includes bleached coniferous kraft pulp slurry and bleached hardwood pulp slurry, the wood pulp board preferably includes bleached coniferous kraft pulp slurry and bleached hardwood pulp slurry, and the mass ratio of the bleached coniferous kraft pulp slurry and the bleached hardwood pulp slurry is preferably (7-8): (2-3), and more preferably 8:2, based on absolute dry pulp. In the present invention, the mass ratio of the wood pulp board to the volume of the first water is preferably 360g:5L; the mass ratio of the wood pulp board to the volume of the second water is preferably 360g:18L. In the present invention, the soaking time is preferably ≥4h; the temperature of the residual water is preferably 20°C; the second deflaking time is preferably 4-6min, and more preferably 5min.
[0028] In the present invention, it is preferred that the pulp is beaten after the second deflocculent process until there are no small pulp lumps; the beating is preferably performed to a beating degree of 28 to 32°SR, and more preferably 29 to 31°SR.
[0029] After the breaking up, the present invention preferably puts the obtained mixed slurry into a sealed bag, and then puts it into a refrigerator to even out the moisture, and then refrigerates it for later use after measuring the moisture content. The present invention can calculate the mass of the required mixed slurry by measuring the moisture content through the quantitative amount of facial tissue paper.
[0030] After obtaining the wood pulp slurry, the present invention mixes polyamide epichlorohydrin resin, diglycerol dioleate, glycerol-water solvent and wood pulp slurry, and sequentially performs first deflaking and papermaking to obtain formed facial tissue base paper.
[0031] In the present invention, the mixing of polyamide epichlorohydrin resin, diglycerol dioleate, glycerol-water solvent and wood pulp slurry preferably includes: first mixing diglycerol dioleate and glycerol-water solvent, then dropping polyamide epichlorohydrin resin, and then secondly mixing the obtained PAE-diglycerol dioleate composite liquid and wood pulp slurry.
[0032] In the present invention, the mass concentration of glycerol in the glycerol-water solvent is preferably 70-80%, and more preferably 72-78%; the mass ratio of diglycerol dioleate to glycerol-water solvent is preferably 1:1.
[0033] In the present invention, the addition amount of dioleic acid dipolyglycerol ester is 2-8 kg / t of the absolute dry pulp mass of the wood pulp slurry, preferably 2.5-6.5 kg / t, and more preferably 4-6 kg / t; the addition amount of polyamide epichlorohydrin resin is 3-12 kg / t of the absolute dry pulp mass of the wood pulp slurry, preferably 5-11.5 kg / t, and more preferably 7-10.5 kg / t. In the present invention, the basis weight of the facial tissue base paper is preferably 15 g / m 2 .
[0034] Polyamide epichlorohydrin resin (PAE) is a water-soluble, cationic, thermosetting resin that does not contain formaldehyde polymers, is non-toxic and odorless, can be manufactured under neutral, slightly alkaline and acidic conditions, and has a wide range of pH values. PAE can significantly improve the dry and wet strength of the page and can be used in the production of all types of paper with wet strength requirements. Polyamide epichlorohydrin resin and dioleic acid diglycerol ester can enhance the softness of facial tissue and the physical strength of paper. Dioleic acid diglycerol ester can be evenly dispersed in the glycerol-water solvent and does not hinder the dispersion of PAE in the solution system, so that dioleic acid diglycerol ester and PAE can be evenly dispersed in the glycerol-water solvent system.
[0035] After the papermaking is completed, the present invention also preferably includes sequentially drying and embossing the obtained facial tissue base paper.
[0036] In the present invention, the embossing pressure is preferably 0.5 MPa. The present invention can significantly improve the softness of the facial tissue by embossing.
[0037] In order to further illustrate the present invention, a method for improving the softness and strength properties of facial tissue provided by the present invention is described in detail below in conjunction with embodiments, but they should not be construed as limiting the scope of protection of the present invention.
[0038] The pulp in the embodiments of the present invention was obtained from Zhejiang Jingxing Paper Co., Ltd.; dioleic acid dipolyglycerol ester was obtained from Shandong Binzhou Jinsheng New Materials Technology Co., Ltd.; PAE was obtained from Vinda; deionized water was homemade in the laboratory; glycerin was purchased from Maclean's reagent; and embossing equipment was provided by Vinda.
[0039] Example 1
[0040] A method for improving the softness and strength properties of facial tissue is:
[0041] Weigh 360g of bleached coniferous kraft pulp and bleached broadleaf pulp (based on absolute dry pulp) in a mass ratio of 8:2, soak the pulp in 5L of water for more than 4h, and then tear the pulp into small pieces of about 4cm×4cm for beating; add 18L of deionized water at a temperature of 20℃ into the pulp tank of the Wally beater, start the beater, slowly add the pulp into the beater, control the disintegration time to about 5min, mix and beat until there are no small pulp lumps; after beating, take out the pulp and dry the water, put it into a sealed bag after beating it with a beating instrument, put it in a refrigerator to even out the water content, and then measure the water content and refrigerate it for use;
[0042] The diglycerol dioleate is placed in a glycerol solution with a mass concentration of 70% (the mass ratio of the diglycerol dioleate to the glycerol solution with a mass concentration of 70% is 1:1), PAE is added and stirred evenly to obtain a PAE-diglycerol dioleate composite liquid; wherein the amount of diglycerol dioleate is 2kg / t, and the amount of PAE added is 3kg / t, both of which are relative to the amount of absolute dry pulp;
[0043] The obtained PAE-dioleic acid dipolyglycerol composite liquid and the refrigerated mixed pulp are placed in a deflaker for deflaking, mixed evenly, transferred to a fourdrinier paper machine for pulp forming on the net, and the base paper is dried for standby use;
[0044] The dried facial tissue is embossed using an embossing machine with a pressure of 0.5 MPa, and the left side of the control slider is flush with the scale "3.0" (this slider on the embossing machine is used to control the embossing depth, the larger the value, the greater the embossing depth), to obtain the facial tissue.
[0045] According to the above method, three parallel tests were performed, with Vinda's facial tissue base paper as a blank control.
[0046] Example 2
[0047] The same raw materials and preparation method as in Example 1 were used, except that the amount of diglycerol dioleate was changed to 4 kg / t and the amount of PAE added was 6 kg / t.
[0048] According to the above method, three parallel experiments were performed.
[0049] Example 3
[0050] The same raw materials and preparation method as in Example 1 were used, except that the amount of diglycerol dioleate was changed to 8 kg / t and the amount of PAE added was 9 kg / t.
[0051] According to the above method, three parallel experiments were performed.
[0052] Example 4
[0053] The same raw materials and preparation method as in Example 1 were used, except that the amount of diglycerol dioleate was changed to 8 kg / t and the amount of PAE added was 12 kg / t.
[0054] According to the above method, three parallel experiments were performed.
[0055] Example 5
[0056] The same raw materials and preparation method as in Example 1 were used, except that the amount of diglycerol dioleate was changed to 8 kg / t and the amount of PAE added was 6 kg / t.
[0057] According to the above method, three parallel experiments were performed.
[0058] Comparative Example 1
[0059] The same raw materials and preparation method as in Example 1 were used, the amount of dioleyl diglycerol was changed to 0 kg / t, the amount of PAE added was 0 kg / t, and the embossing treatment was cancelled. It was equivalent to base paper.
[0060] According to the above method, three parallel experiments were performed.
[0061] Comparative Example 2
[0062] The same raw materials and preparation method as in Example 1 were used, except that the amount of diglycerol dioleate was changed to 0 kg / t, the amount of PAE added was 3 kg / t, and the embossing treatment was cancelled.
[0063] According to the above method, three parallel experiments were performed.
[0064] Comparative Example 3
[0065] The same raw materials and preparation method as in Example 1 were used, except that the amount of diglycerol dioleate was changed to 4 kg / t and the amount of PAE added was 0 kg / t.
[0066] According to the above method, three parallel experiments were performed.
[0067] Comparative Example 4
[0068] The same raw materials and preparation method as in Example 1 were used, and the embossing treatment was omitted.
[0069] According to the above method, three parallel experiments were performed.
[0070] Comparative Example 5
[0071] The same raw materials and preparation method as in Example 1 were used, except that the amount of diglycerol dioleate was changed to 0 kg / t and the amount of PAE added was 3 kg / t.
[0072] According to the above method, three parallel experiments were performed.
[0073] Comparative Example 6
[0074] The same raw materials and preparation method as in Example 1 were used, except that the amount of diglycerol dioleate was changed to 4 kg / t and the amount of PAE added was 3 kg / t.
[0075] According to the above method, three parallel experiments were performed.
[0076] Performance Testing
[0077] The facial tissues having both softness and strength properties prepared in Examples 1 to 5 and Comparative Examples 1 to 6 were placed under conditions of temperature (23±1)°C and humidity (50±2)% for more than 4 hours, and their tensile strength (GB / T12914-2018) and softness HF value (GB / T 8942-2016) were tested. The test results are shown in Table 1.
[0078] Table 1 Retention tensile index and HF value of facial tissue paper prepared in Examples 1 to 5 and Comparative Examples 1 to 6
[0079]
[0080] It can be seen from Table 1 that the facial tissue prepared by the improved method provided by the present invention has good softness and strength properties, and the preparation method provided by the present invention has low cost and is suitable for large-scale production.
[0081] Comparative Example 1 shows that the base paper has relatively poor tensile strength and softness compared to the facial tissue paper treated in Example 1.
[0082] Comparative Example 2 shows that after adding PAE, the tensile properties of the paper are significantly higher than those of Comparative Example 1.
[0083] Comparative Example 3 shows that after adding diglycerol dioleate, the softness performance of the paper is obviously better than that of Comparative Example 1.
[0084] Comparative Example 4 shows that embossing has an effect of improving the softness and tensile properties of facial tissue.
[0085] Compared with Comparative Example 2, Comparative Example 5 again shows that the strength of paper is improved after embossing.
[0086] Comparative Example 6, compared with Comparative Example 5, once again shows that the softness of paper is improved after being treated with diglycerol dioleate.
[0087] Although the above embodiment describes the present invention in detail, it is only a part of the embodiments of the present invention, not all of the embodiments. People can also obtain other embodiments based on this embodiment without creativity, and these embodiments all fall within the protection scope of the present invention.
Claims
1. A method for improving the softness and strength properties of facial tissue, comprising the following steps: The polyamide epichlorohydrin resin, diglycerol dioleate, glycerol-water solvent and wood pulp slurry are mixed, and first decomposition and papermaking are performed in sequence to obtain a formed facial tissue base paper; The addition amount of the polyamide epichlorohydrin resin is 3 to 12 kg / t of the absolute dry mass of the wood pulp slurry; the addition amount of the diglycerol dioleate is 2 to 8 kg / t of the absolute dry mass of the wood pulp slurry.
2. The method according to claim 1, characterized in that The mass concentration of glycerol in the glycerol-water solvent is 70-80%; the mass ratio of dioleic acid dipolyglycerol ester to the glycerol-water solvent is 1:
1.
3. The preparation method according to claim 1, characterized in that: The wood pulp slurry includes bleached softwood kraft pulp slurry and bleached hardwood pulp slurry.
4. The method according to any one of claims 1 to 3, characterized in that: After the papermaking is completed, the method further includes drying and embossing the obtained facial tissue base paper in sequence.
5. The method according to claim 4, characterized in that The embossing pressure is 0.5 MPa.
6. The method according to claim 1 or 3, characterized in that: The preparation of the wood pulp slurry comprises the following steps: The wood pulp board is soaked in the first water, the obtained pulp board is torn into shredded paper pieces, and then the second water is added, and the second decomposition and beating are carried out in sequence, the water is dried, and then the pulp is broken up to obtain the wood pulp slurry.
7. The method according to claim 6, characterized in that When the wood pulp slurry includes bleached coniferous kraft pulp slurry and bleached hardwood pulp slurry, and the wood pulp board includes bleached coniferous kraft pulp board and bleached hardwood pulp board, the mass ratio of the bleached coniferous kraft pulp board and the bleached hardwood pulp board is (7-8):(2-3) based on absolute dry pulp.
8. The method according to claim 6, characterized in that The second decongestion time is 4 to 6 minutes.
9. The method according to claim 6, characterized in that The beating is performed until the beating degree is 28-32°SR.
10. The method according to claim 6, characterized in that The mass ratio of the wood pulp board to the volume of the first water is 360 g:5 L; the mass ratio of the wood pulp board to the volume of the second water is 360 g:18 L.
Citation Information
Patent Citations
Impregnation liquid and transparent paper sheets prepared from impregnation liquid as well as method for rapidly preparing transparent paper sheets
CN107022924A
Processing technology of high-toughness paper for daily use
CN111691228A
Sanitary paper and method for producing the same
JP2013044071A