Method for rapidly screening cycle life of nickel-series battery
By charging and recording the voltage slowly reducing time, the existing battery cycle life test is solved, and fast and accurate battery cycle life screening is achieved, suitable for large-scale full inspection.
Patent Information
- Application Number
- CN202411153660.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-21
- Publication Date
- 2024-11-26
AI Technical Summary
The existing battery cycle life test methods are time-consuming and destructive, and cannot be used for large-scale full testing, and the battery cannot be used again after the test is completed.
By sealing the battery cell of the nickel-based battery, it is charged and transformed into, and recording the time when the voltage is slowly reduced in the first week, it is used to filter the advantages and disadvantages of the battery cycle life, and the test cycle is short and does not affect the battery performance.
It realizes rapid screening of battery cycle life, suitable for large-scale full inspection and screening, with short test cycles and no damage to battery performance.
Smart Images

Figure CN119024199A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of battery screening, and in particular to a method for quickly screening the quality of the cycle life of nickel-based batteries. Background Art
[0002] Cycle life refers to the number of times a battery can be used in a certain charge and discharge mode, also known as the service life of the battery. Cycle life is one of the important indicators of battery performance. The charge and discharge cycle test is a common cycle life measurement method for nickel batteries, including the following steps: Step (1), charging: charge the battery, and after it is fully charged, let it stand for 1 hour; Step (2), discharging: discharge the battery at a constant current to the cut-off voltage; Step (3) repeat steps (1) and (2) until the battery life ends. This test method has the following disadvantages: the charge and discharge test life cycle is long and is a destructive test. After the test, the battery life ends and cannot be used again; it can only be used for random inspection tests and cannot be used for large-scale full inspection tests. Summary of the invention
[0003] In view of the shortcomings of the prior art, the present invention provides a method for quickly screening the cycle life of nickel-based batteries to solve the problems existing in the battery cycle life testing method in the prior art.
[0004] In order to achieve the above object, the technical solution adopted by the present invention is as follows:
[0005] A method for quickly screening the cycle life of nickel-based batteries comprises the following steps:
[0006] Step 1: seal the nickel battery cell and let it stand;
[0007] Step 2: Charge and form the battery after it has been left to rest;
[0008] Step 3: Record the duration of the first week charging formation voltage slowly decreasing, and screen the battery cycle life according to the duration of the first week charging formation voltage slowly decreasing.
[0009] Preferably, in step 1, the standing condition is standing at room temperature for 36-54 hours.
[0010] Preferably, in step 2, the charging condition is to charge at a charging rate of 0.01C-0.1C for 150-200 minutes.
[0011] Preferably, in step three, if the time during which the charging formation voltage slowly decreases in the first week is less than 4 minutes, batteries with poor cycle life are screened out, and if the time during which the charging formation voltage slowly decreases in the first week is more than 5 minutes, batteries with good cycle life are screened out.
[0012] Compared with the prior art, the present invention has the following beneficial effects:
[0013] This method has a short test cycle, has no impact on battery performance, and can be used for large-scale full inspection and screening. BRIEF DESCRIPTION OF THE DRAWINGS
[0014] Figure 1 This is a comparative diagram of the duration of the slow decrease in charging voltage during the first week;
[0015] Figure 2 The present invention is used to perform a cycle life curve corresponding to a 0.5C constant current charge-0.5C constant current discharge cycle for a No. 1 battery, a No. 2 battery, a No. 3 battery, a No. 4 battery, a No. 5 battery, and a No. 6 battery using the method of the present invention. DETAILED DESCRIPTION
[0016] The technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.
[0017] Example
[0018] This embodiment discloses a method for quickly screening the cycle life of nickel-based batteries, comprising the following steps:
[0019] Step 1: Take 6 sealed but unactivated nickel-based batteries, mark them as 1# battery, 2# battery, 3# battery, 4# battery, 5# battery, and 6# battery, and after sealing the batteries, leave them at room temperature for 48 hours;
[0020] Step 2: Charge the battery after standing for the first week, the charging rate is 0.05C (C represents the battery charge and discharge capacity rate), and the charging time is 180 minutes; record the duration of the first week charging formation voltage slowly decreasing;
[0021] Step 3: Continue to complete the charge and discharge formation.
[0022] The time for the first week formation voltage of each nickel-based battery to slowly decrease is shown in Table 1:
[0023] Table 1
[0024]
[0025] As can be seen from Table 1, during the first week of charging, the voltage curve of the 1# battery showed a slow decrease for about 1 minute; during the first week of charging, the voltage curve of the 2# battery showed a slow decrease for about 3 minutes; during the first week of charging, the voltage curve of the 3# battery showed a slow decrease for about 4 minutes; during the first week of charging, the voltage curve of the 4# battery showed a slow decrease for about 5 minutes; during the first week of charging, the voltage curve of the 5# battery showed a slow decrease for about 7 minutes; during the first week of charging, the voltage curve of the 6# battery showed a slow decrease for about 9 minutes.
[0026] Furthermore, during the first week of charging of nickel-based batteries, CoO, Co(OH)2, etc. are converted into CoOOH conductive networks as conductive agents, and the charging voltage curve shows a slowly decreasing stage. If this stage lasts for a short time (less than 4 minutes), the conversion of the CoOOH conductive network is insufficient, resulting in large internal polarization of the battery and poor cycle life; if this stage lasts for a long time (more than 5 minutes), the conversion of the CoOOH conductive network is sufficient, the internal polarization of the battery is small, and the cycle life is good. Therefore, according to the test results in Table 1, the quality of the cycle life of nickel-based batteries can be quickly screened.
[0027] Taking every 50 cycles as one test cycle, the capacity percentage of 1# battery, 2# battery, 3# battery, 4# battery, 5# battery and 6# battery was measured (at an ambient temperature of 20℃±5℃, the battery was first discharged at a constant current of 0.2C to a termination voltage of 1.0V, then charged at 0.1C for 16 hours, left for 60 minutes, and then discharged at a constant current of 0.2C to a termination voltage of 1.0V to test the discharge capacity; capacity percentage = discharge capacity of the current cycle ÷ discharge capacity of the first cycle), and the measurement results are shown in Table 2:
[0028] Table 2
[0029]
[0030]
[0031] It can be seen from Table 2 that the cycle life of battery 1#, battery 2#, and battery 3# is relatively short, while the cycle life of battery 4#, battery 5#, and battery 6# is relatively long. When the cycle number of battery 1# is 350, the capacity percentage is as low as 60.4%, and the cycle life is the worst, which corresponds to the fact that the voltage curve of battery 1# exhibits the lowest duration of slow decrease during the first week of charging in Table 1; the cycle life of battery 2# to battery 6# gradually increases, which corresponds to the fact that the voltage curve of battery 2# to battery 6# exhibits the lowest duration of slow decrease during the first week of charging in Table 1, which indicates that the method for screening batteries of the present invention is accurate and reliable.
[0032] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.
Claims
1. A method for rapidly screening the cycle life of nickel-based batteries, characterized in that: The following steps are involved: Step 1: seal the nickel battery cell and let it stand; Step 2: Charge and form the battery after it has been left to rest; Step 3: Record the duration of the first week charging formation voltage slowly decreasing, and screen the battery cycle life according to the duration of the first week charging formation voltage slowly decreasing.
2. The method for rapidly screening the cycle life of nickel-based batteries according to claim 1, characterized in that: In the step 1, the standing condition is standing at room temperature for 36-54 hours.
3. The method for rapidly screening the cycle life of nickel-based batteries according to claim 1, characterized in that: In the step 2, the charging condition is to charge at a charging rate of 0.01C-0.1C for 150-200 minutes.
4. The method for rapidly screening the cycle life of nickel-based batteries according to claim 1, characterized in that: In the step three, the battery with poor cycle life is screened out if the time for the charging formation voltage to slowly decrease in the first week is less than 4 minutes, and the battery with good cycle life is screened out if the time for the charging formation voltage to slowly decrease in the first week is more than 5 minutes.