Photosensitive resin composition, photosensitive insulating layer, dry film photoresist of flexible circuit board, and ink coating
By adding a double block copolymer to the photosensitive resin, the problem of poor compatibility of the photosensitive resin composition of the flexible circuit board is solved, and its flexibility and development effect are improved. It is suitable for dry film of the flexible circuit board Photoresist and ink coating.
Patent Information
- Application Number
- CN202310611727.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-26
- Publication Date
- 2024-11-26
AI Technical Summary
The existing photosensitive resin compositions used in flexible circuit boards have poor structural compatibility, which makes it difficult for the elastomer to be compatible with polar resins, affecting its flexibility and development and imaging effects.
Using biblock copolymers as additives, such as polycaprolactone-b-polybutyl acrylate, the microphase separation is initiated by mixing with the resin material to form an ordered microstructure, and improve the flexibility of the photosensitive insulating layer. and dispersive effect.
It effectively improves the flexibility of the photosensitive insulating layer, while maintaining good adhesiveness and corrosion resistance, and is suitable for dry film photoresist and ink coatings of flexible circuit boards.
Smart Images

Figure BDA0004253065460000011 
Figure BDA0004253065460000021 
Figure BDA0004253065460000041
Abstract
Description
Technical Field
[0001] The invention relates to a photosensitive resin composition, in particular to a photosensitive resin composition used for a flexible circuit board, a photosensitive insulating layer, a dry film photoresist and an ink coating of the flexible circuit board. Background Art
[0002] Photosensitive resin compositions generally refer to materials that can initiate chemical reactions under the action of light, such as polymer materials that undergo cross-linking reactions and solidify after being exposed to light. Photosensitive resin compositions can be used in dry film photoresists or resist ink coatings for printed circuit boards (PCBs). In addition, photosensitive resin compositions used in flexible circuit boards must also be flexible to meet the requirements of finished products. Summary of the invention
[0003] One aspect of the present invention provides a photosensitive resin composition, which includes a resin material and an additive.
[0004] Another aspect of the present invention is to provide a photosensitive insulating layer.
[0005] Another aspect of the present invention is to provide a dry film photoresist for a flexible printed circuit board.
[0006] Yet another aspect of the present invention is to provide an ink coating for a flexible circuit board.
[0007] According to one aspect of the present invention, a photosensitive resin composition is provided, which comprises at least one resin material and an additive. The additive comprises a diblock copolymer, and the diblock copolymer comprises poly(ε-caprolactone)-b-poly(n-butyl acrylate), PCL-b-PnBA.
[0008] According to one embodiment of the present invention, the diblock copolymer has a structure of formula (1).
[0009]
[0010] According to an embodiment of the present invention, the diblock copolymer is prepared by reacting 2-hydroxyethyl 2-bromoisobutyrate (HEBiB), caprolactone and n-butyl acrylate.
[0011] According to an embodiment of the present invention, the at least one resin material includes acrylic resin, epoxy resin and polyurethane resin.
[0012] According to an embodiment of the present invention, the at least one resin material comprises an acrylic resin having a structure of formula (2).
[0013]
[0014] According to an embodiment of the present invention, the resin material having the structure of formula (2) is made from acrylic acid, methyl methacrylate and hydroxyethyl methacrylate.
[0015] According to an embodiment of the present invention, based on 100 wt % of the photosensitive resin composition, the additive is greater than 0 wt % to 30 wt %.
[0016] According to another aspect of the present invention, a photosensitive insulating layer is provided. The photosensitive insulating layer is formed by curing the photosensitive resin composition of the above aspect.
[0017] According to another aspect of the present invention, a dry film photoresist for a flexible circuit board is provided, which includes the photosensitive insulating layer of the above aspect.
[0018] According to yet another aspect of the present invention, an ink coating for a flexible circuit board is provided, which comprises the photosensitive insulating layer of the above aspect.
[0019] The photosensitive resin composition of the present invention is used to mix additives with resin materials to enhance the flexibility of the prepared photosensitive insulating layer and maintain good adhesion and chemical resistance. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] The present invention will be better understood by reading the following detailed description in conjunction with the accompanying drawings. It should be noted that, as is standard practice in the industry, many features are not drawn to scale. In fact, for the sake of clarity of discussion, the dimensions of many features may be scaled arbitrarily.
[0021] Figure 1 The nuclear magnetic resonance spectrum of the intermediate product according to the synthesis example of the present invention.
[0022] Figure 2A and Figure 2B It is a conversion chart of the intermediate process according to the synthesis example of the present invention.
[0023] Figure 3 The nuclear magnetic resonance spectrum of the intermediate product according to the synthesis example of the present invention.
[0024] Figure 4A and Figure 4B It is a conversion chart of the intermediate process according to the synthesis example of the present invention. DETAILED DESCRIPTION
[0025] As used herein, "around", "about", "approximately" or "substantially" generally means within 20 percent, within 10 percent, or within 5 percent of the stated value or range.
[0026] The existing photosensitive resin compositions used for flexible circuit boards are mostly made by mixing acrylic resin with epoxy resin, and reacting with photoinitiators such as α-hydroxy ketone, acylphosphine oxide, α-amino ketone and oxime ester to crosslink and cure. Since the structure of the resin composition contains groups such as olefinic bonds (C=C), hydroxyl groups (-OH) and / or carboxyl groups (-COOH), it usually has high shrinkage and hard and brittle properties. Therefore, in order to improve the flexural properties required for application in flexible circuit boards, the existing method is to add elastomers (such as rubber) to the photosensitive resin to enhance softness and flexibility. However, there is a problem of poor compatibility between elastomers and polar resins, and the problem of being difficult to remove after the development operation due to the large molecular weight, which in turn affects the development and imaging effect of the photosensitive resin.
[0027] Therefore, the present invention provides a photosensitive resin composition, which improves the compatibility problem by adding an additive including a diblock copolymer to a resin material, and induces microphase separation in a photosensitive crosslinking reaction, thereby allowing the additive to have an ordered microstructure in the resin material to achieve a good dispersion effect, thereby effectively improving the flexibility of the prepared photosensitive insulating layer, while still maintaining other important physical properties, such as adhesion and chemical resistance. Furthermore, the photosensitive resin composition of the present invention can form a photosensitive insulating layer after a curing reaction, which can be applied as a dry film photoresist or ink coating for a flexible circuit board.
[0028] The photosensitive resin composition of the present invention comprises a resin material and an additive. In some embodiments, based on 100wt% of the photosensitive resin composition, the additive is greater than 0wt% to 30wt%. When the content of the additive is within the aforementioned specific range, the flexibility of the photosensitive resin composition and the photosensitive insulating layer formed after curing can be effectively improved.
[0029] In some embodiments, the additive comprises a diblock copolymer. In some embodiments, the diblock copolymer is poly(ε-caprolactone)-b-poly(n-butyl acrylate), PCL-b-PnBA having a structure of formula (1). In formula (1), for example, the ratio of n to m may be about 1.8:1. In some embodiments, the number average molecular weight (M) of poly(ε-caprolactone)-b-poly(n-butyl acrylate) is about 1.8:1. n ) is from about 14,000 to about 24,000.
[0030]
[0031] In some embodiments, polycaprolactone-b-polybutyl acrylate having a structure of formula (1) can be synthesized by the following method. First, 2-Hydroxyethyl 2-bromoisobutyrate (HEBiB) as a bifunctional initiator is synthesized by the following reaction formula (A), which can be obtained by mixing ethylene glycol (EG) and triethylamine (TEA) evenly, adding 2-bromoisobutyryl bromide (BiB) to the solution under an ice bath, and moving to an oil bath pot (e.g., about 25° C.) to react for about 24 hours. After the reaction, deionized water is added to cool and terminate the reaction, and then chloroform is used for multiple extractions (e.g., three times). After washing with saturated sodium bicarbonate and deionized water, the solvent is removed by reduced pressure distillation. Finally, column chromatography is performed with ethyl acetate / n-hexane to purify and separate HEBiB. In one embodiment, the ratio of BiB, ethylene glycol, and triethylamine is about 1:16:1.
[0032] Reaction formula (A)
[0033]
[0034] Next, the first segment of PCL-b-PnBA is subjected to a ring-opening polymerization reaction using reaction formula (B) to synthesize the macromolecular initiator PCL-Br. The synthesized initiator HEBiB, the monomer ε-caprolactone, the catalyst diphenyl phosphate, and the solvent (e.g., toluene) are placed in an oil bath (e.g., about 40° C.) to react for about 24 hours, diluted with tetrahydrofuran (THF), and precipitated with ice methanol to collect the product. In one specific example, the ratio of ε-caprolactone, diphenyl phosphate, and HEBiB is 160:1:1.
[0035] Reaction formula (B)
[0036]
[0037] Then, PCL-b-PnBA is synthesized using reaction formula (C). The initiator PCL-Br, the monomer n-butyl acrylate, the catalyst (e.g., copper, copper bromide and pentamethyldiethylenetriamine (PMDETA)) and the solvent (e.g., anisole) are placed in an oil bath (e.g., about 100°C) for about 48 hours of reaction after removing oxygen interference using a freeze-thaw pump circulation method. After the reaction is completed, it is placed in an ice bath and exposed to air to stop the polymerization reaction. The product is diluted with THF and precipitated with ice methanol to collect the product. In one specific example, the ratio of the monomer n-butyl acrylate, the initiator PCL-Br, copper bromide, copper and PMDETA is 500:1:0.67:1.33:2.
[0038] Reaction (C)
[0039]
[0040] In some embodiments, the resin material included in the photosensitive resin composition may be one or more of an acrylic resin, an epoxy resin, and a polyurethane resin. In some embodiments, the acrylic resin may have a structure of formula (2). In formula (2), for example, the ratio of x to y may be about 1:1.63. In some embodiments, the average molecular weight of the acrylic resin having the structure of formula (2) is about 11,000 to about 19,000.
[0041]
[0042] In some embodiments, the acrylic resin having the structure of formula (2) can be synthesized by the following method. First, the first resin is synthesized by reaction formula (C), which is to add azobisisobutyronitrile (AIBN) and acrylic acid and methyl methacrylate (MMA) as monomers into a reaction container, and add dimethylacetamide (DMAc) or dimethylformamide (DMF) as a solvent, stir evenly, introduce nitrogen to remove oxygen interference, and place in an oil bath for reaction, during which MMA is added in a semi-batch manner for copolymerization. After the reaction is completed, the reaction container is taken out of the oil bath and the reaction is terminated, and then the polymer is diluted with THF and precipitated with ethyl acetate, and the product is collected.
[0043] Reaction (C)
[0044]
[0045] Next, the acrylic resin of formula (2) is synthesized using reaction formula (D). The first resin synthesized above is added to propylene glycol methyl ether acetate (1-methoxy-2-propanol acetate, PGMEA) and stirred until dissolved. After adding pyridine as a catalyst, the reactor is placed in an oil bath (e.g., about 100°C). Then, a mixed solution of hydroxyethyl methacrylate (2-hydroxyethylmethacrylate, HEMA) and an inhibitor is slowly dripped into the reactor, and the reactor is maintained as an open system to avoid the occurrence of polymerization. After reacting at a temperature of about 100°C for about 2 hours to complete the double bond modification, the oil bath is removed, and after it cools to room temperature and is diluted with THF, the mixed solution is added to ether for reprecipitation to collect the product. In one specific example, the ratio of the first resin, HEMA and pyridine is 1:0.7:0.7.
[0046] Reaction formula (D)
[0047]
[0048] Since the photosensitive resin composition of the present invention has better flexibility and does not affect the original physical properties, it can be used for dry film photoresist and ink coating of flexible circuit boards, which includes a photosensitive insulating layer formed by curing the photosensitive resin composition through light.
[0049] Several embodiments are used below to illustrate the application of the present invention, but they are not used to limit the present invention. Those skilled in the art can make various changes and modifications without departing from the spirit and scope of the present invention.
[0050] Synthesis of Polycaprolactone-b-Polybutyl Acrylate
[0051] First, ethylene glycol and triethylamine were placed in a round-bottom flask and mixed evenly at a molar ratio of 16:1. Then, 2-bromo-2-methylpropionyl bromide (BiB) was added dropwise in an ice bath, wherein the molar ratio of BiB to ethylene glycol was 1:16. Next, the round-bottom flask was moved to an oil bath preheated to 25°C to react for about 24 hours. After the reaction was completed, deionized water was added to cool and terminate the reaction, and then three extractions were performed with chloroform. After washing with saturated sodium bicarbonate and deionized water, the solvent was removed by vacuum distillation. Finally, column chromatography was performed with ethyl acetate / n-hexane to purify and separate 2-hydroxyethyl-2-bromoisobutyric acid ethyl ester (HEBiB). The product was analyzed by nuclear magnetic resonance spectroscopy (NMR), and the results are as follows Figure 1 As shown, a to d marked on the spectrum can correspond to the hydrogens marked a to d on the HEBiB structure, respectively, so it can be seen that the obtained product is indeed HEBiB.
[0052] Next, ε-caprolactone, diphenyl phosphate and the above HEBiB were mixed at a molar ratio of 160:1:1 and added to a Schlenk bottle together with toluene, and placed in an oil bath at 40°C for 24 hours. After the reaction was completed, it was diluted with tetrahydrofuran and reprecipitated with ice methanol, the product was collected and the residual solvent was removed in a vacuum oven.
[0053] Samples were taken at specific times during the reaction and the conversion of the monomers was measured using a gas chromatograph (GC). The molecular weight of the product after the residual solvent was removed was measured using a gel permeation chromatography (GPC), where the number average molecular weight (M n ) is about 16900, and the polydispersity index (PDI) is 1.08. The conversion rate results are as follows Figure 2A and Figure 2B As shown, Figure 2A is the relationship between conversion rate (Conv.) and time, Figure 2B The relationship between ln(M0 / M) and time is shown in Figure 2, where M0 is the initial concentration of the monomer and M is the measured monomer concentration in the sample. It can be seen that the conversion rate continues to increase over time. The product is also analyzed by NMR. The NMR spectrum is shown in Figure 2. Figure 3 As shown, a to e marked on the spectrum can correspond to the hydrogens marked a to e on the structure, respectively, so it can be seen that the obtained product is indeed the structure of PCL-Br after ring-opening polymerization.
[0054] Then, n-butyl acrylate, PCL-Br, copper bromide, copper and pentamethyldiethylenetriamine (PMDETA) were mixed in a molar ratio of 500:1:0.67:1.33:2 and added to a Schlenk flask together with anisole. After freeze-thaw pump circulation to remove oxygen interference, the flask was placed in an oil bath at 100°C for 48 hours. After the reaction was completed, the Schlenk flask was placed in an ice bath and exposed to air to stop the polymerization reaction. The product was diluted with tetrahydrofuran and reprecipitated with ice methanol. The product was collected and the residual solvent was removed in a vacuum oven.
[0055] Samples were taken at specific times during the reaction to measure the conversion of the monomers using a gas chromatograph. The molecular weight of the product after the residual solvent was removed was measured using a gel permeation chromatograph, where the number average molecular weight (M n ) is about 23788, and the polymer dispersion coefficient is 1.29. The conversion rate results are as follows Figure 4A and Figure 4B As shown, Figure 4A is the relationship between conversion rate and time. Figure 4BIt is a graph showing the relationship between ln(M0 / M) and time, from which it can be seen that the conversion rate continues to increase with time.
[0056] Embodiments 1 to 6
[0057] In Examples 1 to 3, 5 wt % of the above-synthesized polycaprolactone-b-polybutyl acrylate is added to the resin material, and in Examples 4 to 6, 30 wt % of the polycaprolactone-b-polybutyl acrylate is added to the resin material, respectively. The resin material of Examples 1 and 4 is an acrylic resin of formula (2) with an average molecular weight of 15690; the resin material of Examples 2 and 5 is bisphenol A epoxy diacrylate (Bis-A-Epoxy Acrylate) (i.e., epoxy resin) with a model number of ZAR-1035 and an average molecular weight of 13000; and the resin material of Examples 3 and 6 is a polyurethane resin with a model number of UXE-3086 and an average molecular weight of 10000.
[0058] Comparative Examples 1 to 3
[0059] The photosensitive resin compositions of Comparative Examples 1 to 3 respectively include the same resin materials as those of Examples 1 to 3, except that Comparative Examples 1 to 3 do not include the synthesized polycaprolactone-b-polybutyl acrylate.
[0060] Evaluation test
[0061] The photosensitive resin compositions of Examples 1 to 6 and Comparative Examples 1 to 3 were respectively used to form photosensitive insulating layers on a copper substrate, and adhesion test, opening ability test (developability test) and folding test (bending life test) were performed. The test results are shown in Table 1.
[0062] The adhesion test is a 100-grid test, in which 11 cuts are made in the horizontal and vertical directions at an interval of 1 mm, in which only the resin layer is cut but the copper foil layer is not cut. Then, a 100-grid tape (3M#600) is applied and pressed, and then pulled up vertically quickly. This is repeated twice, and the adhesion of the photosensitive insulating layer on the copper substrate is determined based on the ink shedding situation.
[0063] The steps of the opening capacity test are as follows. First, the photosensitive resin composition is mixed with the photoinitiator Irgacure907 and the photoinitiator ITX at a solid content ratio of 100:3:1 to dissolve the photoinitiator. After standing for a period of time, the wet film is applied on the copper substrate at an interval of about 50μm to about 120μm, and placed in an oven and baked at 75°C for 30 minutes to remove the solvent, thereby obtaining a dry film with a film thickness of about 25±5μm. Next, the wavelength is 365nm and the energy is 200mJ / cm 2 Up to 1000mJ / cm 2The light source was used for 21-step energy scale exposure. After standing for 30 minutes, it was developed with 1% sodium carbonate and the number of 21-step grids at different energies was recorded. Then, after exposure and development with reasonable exposure energy, it was baked at 150°C for 60 to 120 minutes. After confirming that there was no solvent residue, the development opening test was performed.
[0064] The test steps of the dead fold test are as follows. First, cut the sample into 10mm width, fold the sample with the photosensitive insulating layer facing outward and the copper substrate facing inward, and place a 1kg weight on the folding point for 10 seconds and then flatten it. Fold it in the opposite direction and press it for another 10 seconds. This is called a 360-degree dead fold. Check the test piece after each dead fold until the product fails.
[0065] Table 1
[0066] Adhesion test Opening capacity (μm) Dead fold test (number of times) Embodiment 1 ND 200 3 Embodiment 2 5B 100 12 Embodiment 3 5B 200 8 Embodiment 4 5B 200 5 Embodiment 5 5B 100 12 Embodiment 6 5B 200 10 Comparative Example 1 5B 500 0 Comparative Example 2 5B 100 4 Comparative Example 3 5B 200 5
[0067] According to the test results of the adhesion test, as shown in Table 1 above, except for the result of Example 1 which could not be measured, the 100-grid test results of Examples 2 to 6 and Comparative Examples 1 to 3 were all 5B as defined by ASTM D3359, that is, the cutting edge was smooth and complete, and the coating film was completely free of shedding.
[0068] According to the test results of the opening ability, as shown in Table 1 above, if the photosensitive resin compositions using the same resin material are compared, the test results of Examples 2 and 5 using epoxy resin and Comparative Example 2 are the same; and the test results of Examples 3 and 6 using polyurethane resin and Comparative Example 3 are also the same; the test results of Examples 1 and 4 using acrylic resin are different from those of Comparative Example 1. In particular, Examples 1 and 4 have a development opening of 100 μm due to the addition of polycaprolactone-b-polybutyl acrylate to the acrylic resin, but Comparative Example 1 cannot be developed smoothly in a 100 μm nine-square grid, so its development opening can be defined as 200 μm. Therefore, Examples 1 and 4 adding polycaprolactone-b-polybutyl acrylate do have a better effect than Comparative Example 1.
[0069] According to the test results of the dead fold test, the dead fold test is judged by the number of times without cracks, that is, the more times, the better the flexibility. According to the above Table 1, comparing the photosensitive resin composition using the same resin material, in terms of the test results of Examples 1 and 4 using acrylic resin and Comparative Example 1, the more additives are added, the more bending times can be increased; for Examples 2 and 5 using epoxy resin and Comparative Example 2, there is no significant difference in the effect of adding 5% and 30% additives, but both are better than Comparative Example 2 without additives; and Examples 3 and 6 using polyurethane resin and Comparative Example 3 are similar to acrylic resin, that is, when more additives are added, the flexibility is better.
[0070] According to the above embodiments, the photosensitive resin composition provided by the present invention includes a resin material and a specific additive, which can effectively improve the flexibility of the prepared photosensitive insulating layer and maintain good adhesion and chemical resistance. Therefore, the photosensitive resin composition of the present invention is also suitable for use in dry film photoresist or ink coating of flexible circuit boards.
[0071] Although the present invention has been disclosed as above with several embodiments, they are not intended to limit the present invention. Those skilled in the art may make various changes and modifications without departing from the spirit and scope of the present invention. Therefore, the scope of protection of the present invention shall be determined by the definition of the attached claims.
Claims
1. A photosensitive resin composition, characterized in that: Include: At least one resin material; and The additive comprises a diblock copolymer, and the diblock copolymer comprises polycaprolactone-b-polybutyl acrylate.
2. The photosensitive resin composition according to claim 1, characterized in that: The diblock copolymer has the structure of formula (1):
3. The photosensitive resin composition according to claim 2, characterized in that: The diblock copolymer is prepared by reacting 2-hydroxyethyl-2-bromoisobutyrate, caprolactone and n-butyl acrylate.
4. The photosensitive resin composition according to claim 1, wherein The at least one resin material includes acrylic resin, epoxy resin and polyurethane resin.
5. The photosensitive resin composition according to claim 1, wherein The at least one resin material comprises an acrylic resin having a structure of formula (2):
6. The photosensitive resin composition according to claim 5, characterized in that: The resin material having the structure of formula (2) is prepared from acrylic acid, methyl methacrylate and hydroxyethyl methacrylate.
7. The photosensitive resin composition according to claim 1, wherein Based on 100 wt % of the photosensitive resin composition, the additive is greater than 0 wt % to 30 wt %.
8. A photosensitive insulating layer, characterized in that: The photosensitive resin composition according to any one of claims 1 to 7 is formed by curing the photosensitive resin composition.
9. A dry film photoresist for a flexible circuit board, characterized in that: The invention comprises the photosensitive insulating layer as claimed in claim 8.
10. An ink coating for a flexible circuit board, characterized in that: The invention comprises the photosensitive insulating layer as claimed in claim 8.