Niobium-aluminum superconducting wire prepared by reacting and then winding and preparation method of Niobium-aluminum superconducting wire

Through the reaction and then winding process of niobium trialuminum superconducting wire, the equipment input and material requirements for winding first and then annealing heat treatment in the existing process are solved, and the uniform deformation and superconducting performance of niobium trialuminum superconducting wire are achieved. It is suitable for industrial applications.

CN119028657APending Publication Date: 2024-11-26SOUTHWESTERN INST OF PHYSICS
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411300359.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-18
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

The existing Niobium trialuminum (Nb3Al) superconducting wire preparation process requires winding and then annealing and heat treatment, which increases the difficulty of equipment investment and application, and puts forward high requirements for insulating materials and structural support materials, limiting their industrial applications.

Method used

Using the process of reaction first and then winding, Nb foil and Al foil are stacked and wound, and undergoing continuous emergency heat and heat treatment and annealing heat treatment to form niobium trialuminum (Nb3Al) ) Superconducting wires achieve uniform deformation of core wire and maintain superconducting current-carrying performance.

Benefits of technology

It reduces the requirements for heat treatment equipment in traditional processes, reduces the performance requirements of insulation and structural support materials, and is suitable for batch preparation and large-scale applications, and has commercial value.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119028657A_ABST
    Figure CN119028657A_ABST
Patent Text Reader

Abstract

The preparation method comprises the following steps: taking Nb foil and Al foil, stacking and winding the Nb foil and the Al foil on an Nb rod, then loading a porous Nb ingot, and integrally loading the porous Nb ingot into an oxygen-free copper sheath to obtain an Nb-Al multi-core composite sheath; performing room-temperature isostatic pressing, hot extrusion and multi-pass drawing processing on the Nb-Al multi-core composite sheath to obtain an Nb-Al multi-core composite wire; metal copper on the surface of the Nb-Al multi-core composite wire is removed, and an Nb-Al precursor wire is obtained; the Nb-Al precursor wire is subjected to continuous rapid heating and rapid cooling treatment, and a Nb (Al) ss wire is obtained; and bundling the Nb (Al) ss wire rod and an oxygen-free copper wire, putting the bundled Nb (Al) ss wire rod and the oxygen-free copper wire into an oxygen-free copper pipe, and carrying out multi-pass drawing to obtain the Nb-Al composite wire rod. The internal core wire of the superconducting wire rod is uniform in deformation, heat treatment reaction phase formation can be realized in a certain strain range, then a magnet system is formed by winding, the superconducting current-carrying performance is not influenced, and the requirements of the wire rod which is formed by winding and then reacting on heat treatment equipment, wire rod insulation and a magnet system structure supporting material are reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of superconducting material processing, in particular to a niobium-aluminum superconducting wire which is first reacted and then wound and a preparation method thereof. Background Art

[0002] Niobium trialuminum (Nb3Al) is currently the superconducting transition temperature (T c ), critical current density (J c ) and the upper critical field (H c2 ) and other low-temperature superconducting materials with the best comprehensive practical performance. Compared with Nb3Sn, it has a higher upper critical field and better high-field critical current density characteristics; more importantly, it has better stress-strain tolerance than Nb3Sn, and can be heat-treated into phases before winding into a magnet system within a certain stress-strain range. This operation avoids the stringent requirements for vacuum furnaces and magnet skeletons during the overall heat treatment of large magnet coils. Therefore, Nb3Al superconducting wire is considered to have an indispensable position in the application of superconducting magnets such as the next generation of magnetic confinement thermonuclear fusion reactors, nuclear magnetic resonance spectrometers (NMR) and high-energy particle accelerators (LHC).

[0003] Niobium trialuminum (Nb3Al) is an A15 structure and belongs to a brittle phase. At present, the niobium trialuminum (Nb3Al) superconducting wire obtained by the existing preparation process is strictly speaking only a Nb and Al composite. When preparing the magnet system, it is necessary to first wind it into a coil to complete all deformation processes, and then undergo a final phase annealing heat treatment (800℃ / 10 hours) reaction to obtain the niobium trialuminum (Nb3Al) superconducting phase. Therefore, the wire obtained by the current process is called "winding first and then reacting" niobium trialuminum (Nb3Al) wire. This process has increased the difficulty of applying niobium trialuminum (Nb3Al) superconducting wire to a certain extent. Take the coil for the next generation of magnetic confinement thermonuclear fusion reactor as an example: its single coil is 16m high, 9m wide, and weighs more than 360 tons. If the niobium trialuminum obtained by the existing process is used, it is necessary to anneal and heat treat such a large-sized coil after winding. The corresponding heat treatment furnace is also a considerable investment, and there are also unexpected risks in the heat treatment of the entire coil. “Wrapping first and reacting later” also puts forward new requirements for the insulation materials of the wire and the structural support materials of the magnet, requiring these materials to maintain their original performance after the final annealing heat treatment, or at least not to have a significant decline in the original performance. These difficulties have greatly restricted the industrial application of niobium trialuminum (Nb3Al) superconducting wires.

[0004] In view of this, this application is hereby filed. Summary of the invention

[0005] In order to solve the problems of the prior art, the present invention provides a niobium-aluminum superconducting wire that reacts first and then is wound, and a preparation method thereof. The obtained superconducting wire has uniform deformation of the core wire inside, and can be heat-treated and reacted into a phase within a certain strain range, and then wound into a magnet system, while not affecting the superconducting current-carrying performance. The requirements of the traditional "winding first and then reacting" wire on the final heat treatment equipment are reduced, and the requirements on the wire insulation and the magnet system structure support materials are reduced.

[0006] The present invention is achieved through the following technical solutions:

[0007] In a first aspect, the present invention provides a method for preparing a niobium-aluminum superconducting wire by first reacting and then winding, comprising the following steps:

[0008] (1) stacking Nb foil and Al foil and winding them on a Nb rod to obtain a Nb-Al wound rod; placing a plurality of Nb-Al wound rods into a porous Nb ingot, and then placing the entire ingot into an oxygen-free copper sheath to obtain a Nb-Al multi-core composite sheath;

[0009] (2) subjecting the Nb-Al multi-core composite sheath to room temperature isostatic pressing, hot extrusion and multiple drawing processes in sequence to obtain a Nb-Al multi-core composite wire;

[0010] (3) removing the metallic copper on the surface of the Nb-Al multi-core composite wire to obtain a Nb-Al precursor wire;

[0011] (4) subjecting the Nb-Al precursor wire to continuous rapid heating and cooling heat treatment to obtain Nb(Al) ss Wire;

[0012] (5) The Nb(Al) ss The wires and oxygen-free copper wires are bundled and loaded into oxygen-free copper tubes, and then drawn for multiple times to obtain Nb-Al composite wires;

[0013] (6) The Nb-Al composite wire is subjected to annealing heat treatment to obtain a niobium trialuminum (Nb3Al) superconducting wire.

[0014] In a specific embodiment, step (1) specifically comprises stacking Nb foil and Al foil together, winding them onto Nb rods, and then placing them in a three-roller pressing device for rolling and pressing until the foils do not rebound, placing a plurality of the above-mentioned winding rods into a porous Nb ingot, and then placing the Nb ingot with the winding rods into an oxygen-free copper sheath as a whole, and sealing and welding the two ends with copper covers to obtain a Nb-Al multi-core composite sheath;

[0015] The thickness of Nb foil and Al foil is in an atomic ratio of 3:1; the thickness of Nb foil is 0.05-0.1mm, the thickness of Al foil is 0.015-0.03mm, the size of Nb rod is Φ3-8mm, the cross-sectional area ratio of Nb rod in Nb-Al wound rod is 30-50%, and the rest is Nb-Al.

[0016] In a specific embodiment, the number of holes in the porous Nb ingot is 36, 48, 64, 84 or 108, which are arranged in a circular or hexagonal close-packed form; after the porous Nb ingot is assembled into a Nb-Al winding rod, the pure Nb part occupies 45-60% of the cross-sectional area, and the rest is Nb-Al.

[0017] In a specific embodiment, in step (2), the Nb-Al multi-core composite sheath is processed to Φ30-45 mm by hot extrusion, the extrusion ratio is 4-6, and the Nb-Al multi-core composite wire is processed to Φ1.02-1.527 mm.

[0018] In a specific embodiment, in step (3), a HNO3 solution with a concentration of 50-90% and a temperature of 20-80°C is used to etch away the metal, and the size of the Nb-Al precursor wire after etching away the metal is Φ0.92-1.31 mm.

[0019] In a specific embodiment, in step (4), the continuous rapid heating and cooling heat treatment line speed is 300-1000 mm / s, the heating voltage is 8.0-10.0 V, the heating current is 200-300 A, and the wire length fluctuation between the two heating electrodes during the heat treatment process is less than 2 mm.

[0020] In a specific embodiment, in step (5), the Nb(Al) ss The wire size is Φ0.86~1.27mm, cut to size, and Nb(Al) ss The wire and oxygen-free copper wire of the same size are bundled in a hexagonal close-packed manner, then loaded into an oxygen-free copper tube, and then subjected to multiple drawing processes to obtain Nb-Al composite wire; the close-packed bundled Nb(Al) ss The number of wires is 6 cores, 18 cores, and 30 cores. The final size of the Nb-Al composite wire after drawing is Φ0.82~1.0mm, and the internal component size of the Nb-Al composite wire is less than 10um.

[0021] In a specific embodiment, in step (6), the Nb-Al composite wire is wound onto a stainless steel wire wheel and subjected to vacuum annealing heat treatment. The annealing heat treatment temperature is 750-850°C and the holding time is 8-12h. The vacuum degree is better than 10 -2 After the heat treatment, the wire is heated from Pa to the furnace, cooled with the furnace, and taken out of the furnace when the furnace temperature is lower than 50°C. The wire strain before and after the heat treatment is less than 0.86%.

[0022] In a second aspect, the present invention provides a niobium (III) aluminum superconducting wire that is first reacted and then wound, which is prepared by the method for preparing a niobium (III) aluminum superconducting wire that is first reacted and then wound.

[0023] Compared with the prior art, the present invention has the following advantages and beneficial effects:

[0024] 1. The embodiment of the present invention provides a niobium-aluminum superconducting wire that is first reacted and then wound, and a preparation method thereof. The foil winding combined with a roller tightening device is used to achieve uniform compounding of Nb and Al. The wire is continuously subjected to rapid heating and cooling heat treatment combined with reassembly and drawing processing to obtain a composite wire with an internal component size of less than 10um. The composite wire can be heat-treated and reacted to form a phase within a certain strain range, and then wound into a magnet system, breaking the limitation of the intrinsic properties of the A15 structure superconductor on the application;

[0025] 2. The embodiment of the present invention provides a niobium-aluminum superconducting wire that reacts first and then winds and a preparation method thereof, which reduces the requirements of the traditional "winding first and then reacting" wire on the final heat treatment equipment, and reduces the requirements of the wire insulation and the magnet system structure support material;

[0026] 3. A niobium-aluminum superconducting wire that is first reacted and then wound and a preparation method thereof provided in an embodiment of the present invention, wherein the prepared composite wire is wound onto a test frame of different diameters after heat treatment, and still has good low-temperature current carrying capacity;

[0027] 4. The embodiment of the present invention provides a niobium-aluminum superconducting wire that is first reacted and then wound, and a preparation method thereof. The process is simple, suitable for batch preparation of superconducting wires, and is conducive to large-scale promotion and application, and has great commercial value. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] In order to more clearly illustrate the technical solutions of the exemplary embodiments of the present invention, the drawings required for use in the embodiments will be briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present invention and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other related drawings can be obtained based on these drawings without paying creative work.

[0029] Figure 1 This is a critical current density curve diagram of the superconducting wire prepared in Example 1 of the present invention under different background magnetic fields;

[0030] Figure 2 This is a critical current density curve diagram of the superconducting wire prepared in Example 2 of the present invention under different background magnetic fields;

[0031] Figure 3This is a critical current density curve diagram of the superconducting wire prepared in Example 3 of the present invention under different background magnetic fields. DETAILED DESCRIPTION

[0032] In order to make the objectives, technical solutions and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with embodiments and drawings. The exemplary embodiments of the present invention and their description are only used to explain the present invention and are not intended to limit the present invention.

[0033] In the following description, a large number of specific details are set forth in order to provide a thorough understanding of the present invention. However, it is apparent to one of ordinary skill in the art that these specific details need not be employed to practice the present invention. In other embodiments, in order to avoid confusing the present invention, well-known materials or methods are not specifically described.

[0034] Throughout the specification, references to "one embodiment," "an embodiment," "an example," or "an example" mean that a particular feature, structure, or characteristic described in conjunction with the embodiment or example is included in at least one embodiment of the present invention. Therefore, the phrases "one embodiment," "an embodiment," "an example," or "an example" appearing in various places throughout the specification do not necessarily all refer to the same embodiment or example. In addition, particular features, structures, or characteristics may be combined in one or more embodiments or examples in any suitable combination and / or sub-combination. In addition, it will be appreciated by those of ordinary skill in the art that the figures provided herein are for illustrative purposes and that the figures are not necessarily drawn to scale. The term "and / or" as used herein includes any and all combinations of one or more of the associated listed items.

[0035] In the description of the present invention, the directions or positional relationships indicated by terms such as “front”, “rear”, “left”, “right”, “up”, “down”, “vertical”, “horizontal”, “high”, “low”, “inside” and “outside” are based on the directions or positional relationships shown in the accompanying drawings and are only for the convenience of describing the present invention and simplifying the description. They do not indicate or imply that the device or element referred to must have a specific direction, be constructed and operated in a specific direction. Therefore, they should not be understood as limiting the scope of protection of the present invention.

[0036] At present, the niobium-aluminum (Nb3Al) superconducting wire obtained by the existing preparation process is strictly speaking only a Nb and Al composite. When preparing the magnet system, it is necessary to first wind it into a coil to complete all deformation processes, and then undergo a final phase annealing heat treatment (800℃ / 10 hours) reaction to obtain the niobium-aluminum (Nb3Al) superconducting phase. The wire obtained by the current process is called "winding first and then reacting" niobium-aluminum (Nb3Al) wire. This process has increased the difficulty of applying niobium-aluminum (Nb3Al) superconducting wire to a certain extent. The coil needs to be annealed and heat treated after winding. The heat treatment furnace is a considerable investment, and there are also unexpected risks in the heat treatment of the entire coil. "Wounding first and then reacting" also puts forward new requirements for the insulation material of the wire and the structural support material of the magnet, requiring these materials to maintain the original performance after the final annealing heat treatment, or at least the original performance cannot be significantly degraded. These difficulties have greatly restricted the industrial application of niobium-aluminum (Nb3Al) superconducting wire.

[0037] Therefore, the present invention provides a niobium-aluminum superconducting wire that reacts first and then winds, and a preparation method thereof. The obtained superconducting wire has uniform deformation of the core wire inside, and can be heat-treated to react into a phase within a certain strain range, and then wound into a magnet system. At the same time, it will not affect the superconducting current-carrying performance, and reduces the requirements of the traditional "winding first and then reacting" wire on the final heat treatment equipment, and reduces the requirements for the wire insulation and the magnet system structure support materials.

[0038] The present invention is achieved through the following technical solutions:

[0039] In a first aspect, the present invention provides a method for preparing a niobium-aluminum superconducting wire by first reacting and then winding, comprising the following steps:

[0040] (1) stacking Nb foil and Al foil and winding them on a Nb rod to obtain a Nb-Al wound rod; placing a plurality of Nb-Al wound rods into a porous Nb ingot, and then placing the entire ingot into an oxygen-free copper sheath to obtain a Nb-Al multi-core composite sheath;

[0041] (2) subjecting the Nb-Al multi-core composite sheath to room temperature isostatic pressing, hot extrusion and multiple drawing processes in sequence to obtain a Nb-Al multi-core composite wire;

[0042] (3) removing the metallic copper on the surface of the Nb-Al multi-core composite wire to obtain a Nb-Al precursor wire;

[0043] (4) subjecting the Nb-Al precursor wire to continuous rapid heating and cooling heat treatment to obtain Nb(Al) ss Wire;

[0044] (5) The Nb(Al) ssThe wires and oxygen-free copper wires are bundled and loaded into oxygen-free copper tubes, and then drawn for multiple times to obtain Nb-Al composite wires;

[0045] (6) The Nb-Al composite wire is subjected to annealing heat treatment to obtain a niobium trialuminum (Nb3Al) superconducting wire.

[0046] In a specific embodiment, step (1) specifically comprises stacking Nb foil and Al foil together, winding them onto Nb rods, and then placing them in a three-roller pressing device for rolling and pressing until the foils do not rebound, placing a plurality of the above-mentioned winding rods into a porous Nb ingot, and then placing the Nb ingot with the winding rods into an oxygen-free copper sheath as a whole, and sealing and welding the two ends with copper covers to obtain a Nb-Al multi-core composite sheath;

[0047] The thickness of Nb foil and Al foil is in an atomic ratio of 3:1; the thickness of Nb foil is 0.05-0.1mm, the thickness of Al foil is 0.015-0.03mm, the size of Nb rod is Φ3mm-Φ8mm, the cross-sectional area ratio of Nb rod in Nb-Al wound rod is 30-50%, and the rest is Nb-Al.

[0048] In a specific embodiment, the number of holes in the porous Nb ingot is 36, 48, 64, 84 or 108, which are arranged in a circular or hexagonal close-packed form; after the porous Nb ingot is assembled into a Nb-Al winding rod, the pure Nb part occupies 45-60% of the cross-sectional area, and the rest is Nb-Al.

[0049] In a specific embodiment, in step (2), the Nb-Al multi-core composite sheath is processed to Φ45 mm by hot extrusion, the extrusion ratio is 4-6, and the Nb-Al multi-core composite wire is processed to Φ1.527 mm.

[0050] In a specific embodiment, in step (3), HNO3 solution with a concentration of 50-90% and a temperature of 20-80°C is used to etch away copper, and the size of the Nb-Al precursor wire after etching away copper is Φ1.31 mm.

[0051] In a specific embodiment, in step (4), the continuous rapid heating and cooling heat treatment line speed is 300-1000 mm / s, the heating voltage is 8.0-10.0 V, the heating current is 200-300 A, and the wire length fluctuation between the two heating electrodes during the heat treatment process is less than 2 mm.

[0052] In a specific embodiment, in step (5), the obtained Nb(Al) ss After the surface of the wire is cleaned, the size is Φ1.27mm, cut to a fixed length, and Nb(Al) ssThe wire and oxygen-free copper wire of the same size are bundled in a hexagonal close-packed manner, then loaded into an oxygen-free copper tube, and then subjected to multiple drawing processes to obtain a Nb-Al composite wire; the close-packed bundled Nb(Al) ss The number of wires is 6 cores, 18 cores or 30 cores. The final size of the Nb-Al composite wire after drawing is Φ1.0mm, and the size of the internal component of the wire is less than 10um.

[0053] In a specific embodiment, in step (6), the Nb-Al composite wire is wound onto a stainless steel wire wheel and subjected to vacuum annealing heat treatment. The annealing heat treatment temperature is 750-850°C and the holding time is 8-12h. The vacuum degree is better than 10 -2 After the heat treatment, the wire is heated from Pa to the furnace, cooled with the furnace, and taken out of the furnace when the furnace temperature is lower than 50°C. The wire strain before and after the heat treatment is less than 0.86%.

[0054] In a second aspect, the present invention provides a niobium (III) aluminum superconducting wire that is first reacted and then wound, which is prepared by the method for preparing a niobium (III) aluminum superconducting wire that is first reacted and then wound.

[0055] Example 1

[0056] The embodiment of the present invention provides a method for preparing a niobium-aluminum superconducting wire by first reacting and then winding, and the steps are as follows:

[0057] Take Nb foil and Al foil and stack them together and wind them onto Nb rods, and then press them with a three-roller pressing device. Then, 64 of the above-mentioned winding rods are sequentially loaded into the small holes of the 64-hole Nb ingot, and then the whole is loaded into an oxygen-free copper sheath, and copper covers are added at both ends to seal and weld to obtain a Nb-Al multi-core composite sheath;

[0058] The Nb-Al multi-core composite sheath is subjected to room temperature isostatic pressing, hot extrusion and multiple drawing processes to obtain a Φ1.527 mm Nb-Al multi-core composite wire;

[0059] After the copper is removed from the Nb-Al multi-core composite wire, continuous rapid heating and cooling heat treatment is performed at a heat treatment speed of 300 mm / s to obtain Nb(Al) ss Wire; Nb(Al) ss The wire is cut to length after surface cleaning, 18 Nb (Al) ss The wire and an oxygen-free copper wire of the same size are closely packed and bundled into a Φ9 / Φ6.8mm oxygen-free copper tube, and drawn to Φ1.0mm to obtain a Nb-Al composite wire;

[0060] The Nb-Al composite wire was wound onto a Φ100 mm stainless steel wire wheel and annealed in a vacuum furnace at 800° C. for 10 hours to obtain a Φ1.0 mm niobium trialuminum (Nb3Al) superconducting wire.

[0061] The 1.0 mm niobium trialuminum (Nb3Al) superconducting wire obtained after heat treatment was rewound onto a 46 mm sample frame to test the low temperature current carrying capacity. Figure 1 As shown in the critical current density curves of the superconducting wire under different background magnetic fields, it can be seen that the Ф1.0 mm niobium trialuminum (Nb3Al) superconducting wire sample obtained in the embodiment of the present invention is subjected to heat treatment and then rewound to form a coil, and the room temperature and low temperature resistance ratio RRR value of the superconducting wire is 105.

[0062] Example 2

[0063] The embodiment of the present invention provides a method for preparing a niobium-aluminum superconducting wire by first reacting and then winding, and the steps are as follows:

[0064] Take Nb foil and Al foil and stack them together and wind them onto Nb rods, and then press them with a three-roller pressing device. Then, 84 of the wound rods are sequentially loaded into the small holes of the 84-hole Nb ingot, and then the whole is loaded into an oxygen-free copper sheath, and copper covers are added at both ends to seal and weld to obtain a Nb-Al multi-core composite sheath;

[0065] The Nb-Al multi-core composite sheath is subjected to room temperature isostatic pressing, hot extrusion and multiple drawing processes to obtain a Φ1.527 mm Nb-Al multi-core composite wire;

[0066] After the copper is removed from the Nb-Al multi-core composite wire, continuous rapid heating and cooling heat treatment is performed at a heat treatment speed of 300 mm / s to obtain Nb(Al) ss Wire; Nb(Al) ss The wire is cut to length after surface cleaning, 6 Nb(Al) ss The wire and an oxygen-free copper wire of the same size are closely packed and bundled into a Φ6.5 / Φ4.3mm oxygen-free copper tube, and drawn to Φ1.0mm to obtain a Nb-Al composite wire;

[0067] The Nb-Al composite wire was wound onto a Φ100 mm stainless steel wire wheel and annealed in a vacuum furnace at 800° C. for 10 hours to obtain a Φ1.0 mm niobium trialuminum (Nb3Al) superconducting wire.

[0068] The 1.0 mm niobium trialuminum (Nb3Al) superconducting wire obtained after heat treatment was rewound onto a 46 mm sample frame to test the low temperature current carrying capacity. Figure 2 As shown in the critical current density curves of the superconducting wire under different background magnetic fields, it can be seen that the Ф1.0 mm niobium trialuminum (Nb3Al) superconducting wire sample obtained in the embodiment of the present invention is heat-treated and then rewound to form a coil, and the room temperature and low temperature resistance ratio RRR value of the superconducting wire is 124.

[0069] Example 3

[0070] The embodiment of the present invention provides a method for preparing a niobium-aluminum superconducting wire by first reacting and then winding, and the steps are as follows:

[0071] Take Nb foil and Al foil and stack them together and wind them onto Nb rods, and then press them with a three-roller pressing device. Then, 108 of the above-mentioned winding rods are sequentially loaded into the small holes of the 108-hole Nb ingot, and then the whole is loaded into an oxygen-free copper sheath, and copper covers are added at both ends to seal and weld to obtain a Nb-Al multi-core composite sheath;

[0072] The Nb-Al multi-core composite sheath is subjected to room temperature isostatic pressing, hot extrusion and multiple drawing processes to obtain a Φ1.527 mm Nb-Al multi-core composite wire;

[0073] After the copper is removed from the Nb-Al multi-core composite wire, continuous rapid heating and cooling heat treatment is performed at a heat treatment speed of 300 mm / s to obtain Nb(Al) ss Wire; Nb(Al) ss The wire is cut to length after surface cleaning, 18 Nb (Al) ss The wire and an oxygen-free copper wire of the same size are closely packed and bundled into a Φ9 / Φ6.8mm oxygen-free copper tube, and drawn to Φ1.0mm to obtain a Nb-Al composite wire;

[0074] The Nb-Al composite wire was wound onto a Φ100 mm stainless steel wire wheel and annealed in a vacuum furnace at 800° C. for 10 hours to obtain a Φ1.0 mm niobium trialuminum (Nb3Al) superconducting wire.

[0075] The 1.0 mm niobium trialuminum (Nb3Al) superconducting wire obtained after heat treatment was rewound onto a 46 mm sample frame to test the low temperature current carrying capacity. Figure 3 As shown in the critical current density curves of the superconducting wire under different background magnetic fields, it can be seen that the Ф1.0 mm niobium trialuminum (Nb3Al) superconducting wire sample obtained in the embodiment of the present invention is heat-treated and then rewound to form a coil, and the room temperature and low temperature resistance ratio RRR of the superconducting wire is 108.

[0076] The specific implementation methods described above further illustrate the objectives, technical solutions and beneficial effects of the present invention in detail. It should be understood that the above description is only a specific implementation method of the present invention and is not intended to limit the scope of protection of the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the scope of protection of the present invention.

Claims

1. A method for preparing a niobium-aluminum superconducting wire by first reacting and then winding. It is characterized in that The steps include: (1) stacking Nb foil and Al foil and winding them on a Nb rod to obtain a Nb-Al wound rod; placing a plurality of Nb-Al wound rods into a porous Nb ingot, and then placing the entire ingot into a metal sheath to obtain a Nb-Al multi-core composite sheath; (2) subjecting the Nb-Al multi-core composite sheath to room temperature isostatic pressing, hot extrusion and multiple drawing processes in sequence to obtain a Nb-Al multi-core composite wire; (3) removing the metal on the surface of the Nb-Al multi-core composite wire to obtain a Nb-Al precursor wire; (4) subjecting the Nb-Al precursor wire to continuous rapid heating and cooling heat treatment to obtain Nb(Al) ss Wire; (5) The Nb(Al) ss The wires are bundled with metal wires, loaded into metal tubes, and drawn for multiple times to obtain Nb-Al composite wires.

2. The method for preparing a niobium-aluminum superconducting wire by first reacting and then winding according to claim 1, It is characterized in that The method further comprises: (6) subjecting the Nb-Al composite wire to annealing heat treatment, so as to obtain Nb-Al composite wire. 3 Al) superconducting wire.

3. The method for preparing a niobium-aluminum superconducting wire by first reacting and then winding according to claim 1, It is characterized in that In step (1), the thickness of the Nb foil is 0.05-0.1 mm, the thickness of the Al foil is 0.015-0.03 mm, the size of the Nb rod is Φ3-8 mm, and the cross-sectional area ratio of the Nb rod in the Nb-Al wound rod is 30-50%.

4. The method for preparing a niobium-aluminum superconducting wire by first reacting and then winding according to claim 3, It is characterized in that The number of holes in the porous Nb ingot is 36, 48, 64, 84 or 108; after the porous Nb ingot is assembled into a Nb-Al winding rod, the cross-sectional area ratio of the pure Nb part is 45-60%.

5. The method for preparing a niobium-aluminum superconducting wire by first reacting and then winding according to claim 1, It is characterized in that In step (2), the Nb-Al multi-core composite sheath is processed to Φ30-45 mm by hot extrusion, the extrusion ratio is 4-6, and the Nb-Al multi-core composite wire is processed to Φ1.02-1.527 mm.

6. The method for preparing a niobium-aluminum superconducting wire by first reacting and then winding according to claim 1, It is characterized in that In step (3), HNO with a concentration of 50-90% and a temperature of 20-80°C is used. 3 The solution is used to corrode the metal, and after the metal is corroded, the size of the Nb-Al precursor wire is Φ0.92-1.31 mm.

7. The method for preparing a niobium-aluminum superconducting wire by first reacting and then winding according to claim 1, It is characterized in that In step (4), the continuous rapid heating and cooling heat treatment line speed is 300-1000 mm / s, the heating voltage is 8.0-10.0 V, and the heating current is 200-300 A.

8. The method for preparing a niobium-aluminum superconducting wire by first reacting and then winding according to claim 1, It is characterized in that In step (5), the Nb(Al) ss The wire size is Φ0.86~1.27mm, and the Nb(Al) is densely packed. ss The number of wires is 6 cores, 18 cores, and 30 cores. The final size of the Nb-Al composite wire after drawing is Φ0.82~1.0mm, and the internal component size of the Nb-Al composite wire is less than 10um.

9. The method for preparing a niobium-aluminum superconducting wire by first reacting and then winding according to claim 1, It is characterized in that In step (6), the annealing heat treatment temperature is 750-850° C., and the holding time is 8-12 hours.

10. A niobium-aluminum superconducting wire that reacts first and then winds. It is characterized in that The invention is prepared by the preparation method according to any one of claims 1 to 9.