Corner-reinforced high-coercivity R-T-B rare earth permanent magnet and preparation method thereof

By applying the diffusion source on the surface of the NdFeB magnet and performing grain boundary diffusion and dispersion decomposition, the main phase grains of the anti-core-shell structure are formed, which solves the problem of missing edges and angles in the transportation and assembly process of NdFeB magnets. , improves the coercive force and edge strength of the magnet.

CN119028685APending Publication Date: 2024-11-26ZHEJIANG INNUOVO MAGNETICS
View PDF 0 Cites 2 Cited by

Patent Information

Application Number
CN202411061515.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-05
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

Neodymium iron boron magnets are prone to missing edges and angles during transportation and assembly, and traditional methods will lead to a reduction in residual magnetism when improving the mechanical properties of magnets, and existing edge and corner strengthening techniques are difficult to further improve the coercive force of the magnet.

Method used

By applying diffusion sources on the magnet surface, coating diffusion sources containing Zr, Ti, and Nb elements in the corner area, and coating diffusion sources with heavy rare earth elements in the non-corner area, grain boundary diffusion and dispersion decomposition treatment are performed to form an inverse nucleus with reverse nucleus The main phase grains of the shell structure to increase the coercive force of the magnet.

Benefits of technology

It significantly improves the edge-angle strength and coercive force of the magnet, reduces the angle drop rate of the edge-missing, and maintains magnetic properties, which has industrial application value.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119028685A_ABST
    Figure CN119028685A_ABST
Patent Text Reader

Abstract

The invention discloses a corner-strengthened high-coercivity R-T-B rare earth permanent magnet and a preparation method thereof, the method comprises the following steps: carrying out partition diffusion on a magnet diffusion source coating surface, coating a diffusion source containing Zr, Ti or Nb elements on a corner region of the magnet, coating a heavy rare earth element diffusion source on a non-corner region of the magnet, then heating in an environment containing H2, and carrying out heat treatment to obtain the corner-strengthened high-coercivity R-T-B rare earth permanent magnet. Main phase grains on the surface of the magnet coated diffusion source are disproportionated and decomposed, and are recrystallized in a slow cooling process after diffusion. Through disproportionation decomposition and recrystallization treatment, a layer of main phase crystal grains with an anti-core-shell structure is distributed on the outer side of main phase crystal grains with a core-shell structure in a non-corner region of the magnet, so that main phase crystal grains with a non-core-shell structure, main phase crystal grains with a core-shell structure and main phase crystal grains with an anti-core-shell structure are sequentially arranged in the non-corner region of the magnet from a core part to a diffusion surface of the magnet; the coercive force of the magnet is further improved, and the method has important significance in improving the magnetic performance of the R-T-B magnet and reducing the cost.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to an edge-reinforced high-coercivity RTB rare earth permanent magnet and a preparation method thereof, belonging to the field of rare earth magnets. Background Art

[0002] Grain boundary diffusion is a new technology developed in recent years. It can significantly improve the coercivity of RTB rare earth permanent magnets while ensuring that the magnets have high remanence. It is a common method for preparing high-performance RTB rare earth permanent magnets.

[0003] The grain boundary diffusion treatment first coats the magnet surface with a diffusion source layer containing heavy rare earth elements, and then heats it to a specified temperature and keeps it warm for a period of time. During the high temperature stage, the heavy rare earth elements in the diffusion source on the magnet surface will diffuse into the magnet along the grain boundary R-rich phase, forming a shell with a high anisotropy field on the surface of the main phase grains of the magnet. In addition, additional rare earth elements will infiltrate the magnet during the grain boundary diffusion process, increasing the total rare earth content of the magnet, and the grain boundary R-rich phase between the main phase grains will become more continuous, thereby achieving the de-exchange coupling effect between the main phase grains. Therefore, grain boundary diffusion improves the coercive force of the magnet by increasing the anisotropy field on the surface of the main phase grains and optimizing the distribution of the grain boundary R-rich phase.

[0004] Although RTB rare earth permanent magnets have high magnetic properties, they are relatively brittle due to the intrinsic properties of the material. During machining, machining stress will cause many micro cracks at the corners of the magnets. During the subsequent product transportation and assembly process, even a slight bump will cause the corners of the magnets to crack, resulting in missing edges and corners of the product.

[0005] Adding a certain amount of high melting point metal elements such as Zr, Ti and Nb to the magnet can strengthen the grain boundary R-rich phase of the magnet by solid solution or the formation of a second precipitated phase, thereby improving the mechanical properties of the magnet. However, as the content of non-magnetic elements increases, the remanence of the magnet will decrease; secondly, during the transportation and assembly process of NdFeB magnets, the corners are prone to defects due to collisions, while other parts of the magnet rarely produce collision defects. This means that by using a certain method to make certain elements such as Zr, Ti and Nb exist in the corner area of ​​the magnet without affecting other areas of the magnet, the qualified rate of NdFeB magnets can be improved without affecting the magnetic properties of the magnet. Patent CN116469635A discloses a corner-strengthened RTB rare earth permanent magnet, which makes certain elements such as Zr, Ti and Nb exist in the corner area of ​​the magnet by partitioning and coating the diffusion source, thereby improving the qualified rate. However, the coercive force of the magnet needs to be further improved. Summary of the invention

[0006] The purpose of the present invention is to further significantly improve the coercivity of the magnet under the premise of strengthening the corners of the magnet through process optimization, and to prepare a high coercivity RTB rare earth permanent magnet with corner strengthening.

[0007] The technical solution adopted by the present invention is as follows: A corner-strengthened high-coercivity RTB rare earth permanent magnet, the magnet comprising the following components in mass fraction: R: 28.5~34.0wt.%, R is composed of RL and RH, the content of RH is 0.1wt.%~10.0wt.% of the mass of the magnet, RH is at least one of Dy, Tb, Ho; the remainder of R is RL, RL represents one or more elements selected from Nd, Pr, La, Ce, Er, Gd, Sm, Tm, Lu, Y containing at least light rare earth elements; the light rare earth elements are one or more of La, Ce, Pr, Nd; B: 0.85~1.1wt.%, Ga: 0.1~1.0wt.%, M: 0.01-8.0 wt.%, M represents a plurality of elements selected from Al, Cu, Ga, Ni, Zn, Sn, Mn, Cr, Zr, Ti, and Nb, including at least X, where X is one or more of Zr, Ti, and Nb; Preferably, M includes at least M1 and X, wherein M1 is one or more of Al, Ga, and Cu; preferably Ga or Cu; M1 can be obtained entirely or partially through grain boundary diffusion; The balance is T and other unavoidable impurities, T is Fe or Fe and Co; The magnet has at least one surface A, and the light rare earth element content in the corner area of ​​the surface A is not lower than the average light rare earth content of the surface A; the light rare earth element is one or more of La, Ce, Pr, and Nd; and the corner area of ​​the surface A contains X, and X is one or more of Zr, Ti, and Nb.

[0008] The magnet has at least one surface A, the light rare earth element content of the corner area of ​​the surface A is not less than the average light rare earth content of the surface A; the light rare earth element is one or more of La, Ce, Pr, and Nd; and the corner area of ​​the surface A contains X, and X is one or more of Zr, Ti, and Nb; Within a depth range of 0.6 mm vertically from the surface A of the magnet, the corner body region does not contain anti-core-shell structure main phase grains, and the non-corner body region contains some anti-core-shell structure main phase grains. The anti-core-shell structure main phase grains have a core portion and a shell portion that wraps the core portion, and the RH mass concentration of the shell portion is lower than the mass concentration of the core portion.

[0009] Furthermore, from the center of the magnet to the surface A of the magnet, the non-corner body region is sequentially arranged with non-core-shell structure main phase grains, core-shell structure main phase grains and anti-core-shell structure main phase grains; the corner body region is sequentially arranged with non-core-shell structure main phase grains and core-shell structure main phase grains.

[0010] Preferably, the thickness of the magnet region containing the main phase grains of the inverse core-shell structure is 30-100 μm.

[0011] The inverse core-shell main phase grains are magnet main phase grains whose shell RH mass concentration C1 and core RH mass concentration C2 satisfy C2 / C1>1.1; the core-shell structure main phase grains are magnet main phase grains whose shell RH mass concentration C1 and core RH mass concentration C2 satisfy C1 / C2>1.1; the non-core-shell structure main phase grains are main phase grains whose interior RH concentration is evenly distributed, and there is no core-shell structure or inverse core-shell structure.

[0012] Furthermore, the surface A is a coating surface of the magnet coated with a diffusion source.

[0013] Furthermore, it is preferred that RH accounting for 0.05-2.5 wt.% of the mass of the magnet is obtained by grain boundary diffusion.

[0014] Furthermore, it is preferred that in the magnet, at least Ga accounting for 0.1 wt% of the mass of the magnet is not obtained by grain boundary diffusion, that is, it is added to the magnet matrix in the form of raw material during the smelting stage.

[0015] The X in the magnet can be obtained entirely or partially through grain boundary diffusion.

[0016] Preferably, in the magnet, more than 70% of RL is Nd; Preferably, in the magnet, X is Zr.

[0017] Furthermore, within a depth range of 0.6 mm from the surface A of the magnet, the X content in the corner body region is 0.05-1.2 wt.%.

[0018] The average X content of the magnet is 0.05-0.8 wt.%.

[0019] The corner area refers to the surface area within the width range of 0~Kmm from the edge line, K is the width of the corner area, and the range of K is 0.2~0.6. The non-corner area refers to the surface area outside the width range of Kmm from the edge line.

[0020] The corner body region is a body region enclosed by the corner area and a depth of 0.6 mm perpendicular to the surface A. The non-corner body region is a magnetic body region outside the corner body region.

[0021] The non-corner body region of the magnet does not contain X, or the X content in the non-corner body region is less than or equal to the X content in the corner body region of the magnet.

[0022] The edge-strengthened high coercivity RTB rare earth permanent magnet is preferably prepared according to the following method: (1) An H1 diffusion source coating area and an H2 diffusion source coating area are set on the diffusion surface of the RTB magnet substrate, and the diffusion sources are coated in different areas. The H1 diffusion source coating area is coated with the diffusion source H1, and the H2 diffusion source coating area is coated with the diffusion source H2; the H1 diffusion source coating area is the corner area of ​​the diffusion surface, and the H2 diffusion source coating area is the non-corner area of ​​the diffusion surface; The corner area refers to the surface area within the width range of 0~Kmm from the edge line, K is 0.2~0.6, and the non-corner area refers to the surface area outside the width range of Kmm from the edge line.

[0023] Schematic diagrams of the corner and non-corner areas of some common magnet shapes are shown below: Figure 1 shown.

[0024] The RTB magnet matrix contains more than 0.1wt% Ga; The diffusion source H1 includes the following components in mass fraction: R1: 50.0~80.0wt.%, R1 includes RL1 and RH1, RH1 is one or more of Dy, Tb, Ho, and accounts for 30.0~70.0wt.% of the mass ratio of H1, and the balance of R1 is RL1, RL1 represents one or more elements selected from Nd, Pr, La, Ce, Er, Gd, Sm, Tm, Lu, Y containing at least light rare earth elements; the light rare earth elements are one or more of La, Ce, Pr, Nd; preferably RL1 is Nd and Pr; X1: 10-30wt.%, X1 is one or more of Zr, Ti, and Nb; preferably Zr; M1: 5.0-40.0wt.%, M1 is one or more of Al, Ga, and Cu; preferably Ga or Cu; The diffusion source H2 is one or more mixtures of pure metals, alloys or compounds containing heavy rare earth elements, and the heavy rare earth element is at least one of Dy, Tb and Ho. Preferably, the content of heavy rare earth elements in H2 is greater than 70%.

[0025] Furthermore, the content of heavy rare earth elements in the diffusion source H1 is lower than that in H2.

[0026] Preferably, H1 is composed of the following components: R1: 65-75%, X1: 15-25%, M1: 10-15%, more preferably R1: 70%, X1: 20%, M1: 10%.

[0027] The coating thickness of the diffusion source H1 and the coating thickness of the diffusion source H2 may be the same or different. Preferably, the coating thickness of the diffusion source H1 and the coating thickness of the diffusion source H2 are the same.

[0028] The coating amount of diffusion source H1 is generally 0.5~2.0% of the mass of the magnet; the coating amount of diffusion source H2 is generally 0.5~2.0% of the mass of the magnet.

[0029] (2) Place the magnet coated with diffusion sources in hydrogen or a mixture of hydrogen and nitrogen at 400-600°C for 10-30 minutes.

[0030] When the magnet is heated in hydrogen or a mixture of hydrogen and nitrogen, the 2:14:1 phase main phase grains in the surface layer of the magnet undergo disproportionate decomposition. The thickness of the disproportionate decomposition area can be controlled by controlling the heating temperature and heating time.

[0031] (3) The magnet of step (2) is subjected to diffusion treatment at a diffusion temperature of 800° C. to 1000° C. for a holding time of 6 to 30 hours, and then subjected to tempering treatment after cooling to obtain the RTB rare earth permanent magnet.

[0032] The present invention also provides a method for preparing an edge-reinforced high-coercivity RTB rare earth permanent magnet, the method comprising the following steps: (1) An H1 diffusion source coating area and an H2 diffusion source coating area are set on the diffusion surface of the RTB magnet substrate, and the diffusion sources are coated in different areas. The H1 diffusion source coating area is coated with the diffusion source H1, and the H2 diffusion source coating area is coated with the diffusion source H2; the H1 diffusion source coating area is the corner area of ​​the diffusion surface, and the H2 diffusion source coating area is the non-corner area of ​​the diffusion surface; The corner area refers to the surface area within the range of 0~Kmm width from the edge line, K is the width of the corner area, and the range of K is 0.2~0.6. The non-corner area refers to the surface area outside the range of Kmm width from the edge line; The RTB magnet matrix contains more than 0.1wt% Ga; The diffusion source H1 includes the following components in mass fraction: R1: 50.0~80.0wt.%, R1 includes RL1 and RH1, RH1 is one or more of Dy, Tb, Ho, and accounts for 30.0~70.0wt.% of the mass ratio of H1, and the balance of R1 is RL1, RL1 represents one or more elements selected from Nd, Pr, La, Ce, Er, Gd, Sm, Tm, Lu, Y containing at least light rare earth elements; the light rare earth elements are one or more of La, Ce, Pr, Nd; X1: 10-30wt.%, X1 is one or more of Zr, Ti, and Nb; M1: 5.0~40.0wt.%, M1 is one or more of Al, Ga, and Cu; The diffusion source H2 is one or more mixtures of pure metals, alloys or compounds containing heavy rare earth elements, and the heavy rare earth element is at least one of Dy, Tb and Ho; And the content of heavy rare earth elements in the diffusion source H1 is lower than that in H2; (2) placing the magnet coated with diffusion sources in a hydrogen or hydrogen and nitrogen mixture at 400-600°C for 10-30 minutes; (3) The magnet coated with the diffusion source in step (2) is subjected to diffusion treatment at a diffusion temperature of 800° C. to 1000° C. for a holding time of 6 to 30 hours, and then subjected to tempering treatment after cooling to obtain the RTB rare earth permanent magnet.

[0033] In the step (1), the diffusion surface refers to the surface of the magnet coated with the diffusion source, which can generally be a magnet surface perpendicular to the magnet orientation direction, parallel to the magnet orientation direction, or at any angle to the magnet orientation direction.

[0034] The surface A is the diffusion surface.

[0035] Preferably, the diffusion surfaces are two surfaces perpendicular to the orientation direction of the magnet.

[0036] In the step (1), the partition coating diffusion source can be achieved by the following method: Use shielding sheet 1 to cover the corner area of ​​the magnet, expose the non-corner area as the H2 diffusion source coating area, and coat the diffusion source H2, then use shielding sheet 2 to cover the non-corner area of ​​the magnet, expose the corner area of ​​the magnet, and coat the diffusion source H1 as the H1 diffusion source coating area; or first use shielding sheet 2 to cover the non-corner area of ​​the magnet, expose the corner area of ​​the magnet, and coat the diffusion source H1 as the H1 diffusion source coating area, and coat the diffusion source H1, then use shielding sheet 1 to cover the corner area of ​​the magnet, expose the non-corner area, and coat the diffusion source H2 as the H2 diffusion source coating area. Exchanging the coating order of diffusion sources H1 and H2 will not affect the final effect.

[0037] The shielding sheet 1 is composed of a shielding area 1 and a hollow area 1, wherein the shielding area 1 corresponds to the corner area of ​​the magnet, and the hollow area 1 corresponds to the non-corner area of ​​the magnet; The shielding sheet 2 consists of a shielding area 2 and a hollow area 2. The shielding area 2 corresponds to the non-corner area of ​​the magnet, and the hollow area corresponds to the corner area of ​​the magnet.

[0038] The shielding sheet 1 or the shielding sheet 2 can be made of polymer plastic material or metal material such as stainless steel.

[0039] The diffusion source may be coated by PVD, spraying or printing.

[0040] When the diffusion source is coated by PVD, the diffusion source H1 is obtained by melting a large ingot; when the diffusion source is coated by spraying or printing, the diffusion source H1 is obtained by melting SC sheets, hydrogen crushing and air flow grinding to obtain a powdered diffusion source.

[0041] When the diffusion source is coated by printing, the printed coating needs to be dried between two coatings.

[0042] Printing and coating the diffusion source has the advantage of simple operation and is very suitable for mass production of products. Therefore, in the present invention, screen printing is preferably used to coat the diffusion source: Furthermore, the partition coating of the diffusion source is preferably carried out by screen printing, and the partition coating of the diffusion source specifically includes the following steps: (a) A hollow area with holes and a shielding area without holes are set on the screen, and the positions of the hollow area and the shielding area of ​​the printing screen are changed according to the product size and the size of the corner area. At least printing screen 1 and printing screen 2 should be included, wherein the hollow area of ​​printing screen 1 corresponds to the non-corner area of ​​the magnet, and the shielding area corresponds to the corner area of ​​the magnet; the hollow area of ​​printing screen 2 corresponds to the corner area of ​​the magnet, and the shielding area corresponds to the non-corner area of ​​the magnet; printing screen 1 and printing screen 2 can include multiple hollow areas or shielding areas, and print multiple magnetic sheets at the same time; (b) Align the shielding area of ​​printing screen 1 with the corner area of ​​the magnet, align the hollow area with the non-corner area, as the H2 diffusion source coating area, print the diffusion source H2, and dry it. Then align the shielding area of ​​printing screen 2 with the non-corner area of ​​the magnet, align the hollow area with the corner area of ​​the magnet, as the H1 diffusion source coating area, print the diffusion source H1, and dry it; or use the opposite order to perform zone coating.

[0043] The RTB magnet matrix of the present invention is obtained by processing a sintered bulk NdFeB magnet into a desired shape and size, cleaning the magnet after surface treatment and drying the magnet.

[0044] The surface treatment of the magnet is to remove oil stains and rust spots on the surface of the magnet by grinding, pickling or sandblasting.

[0045] In the step (2), the volume ratio of hydrogen in the mixed gas of hydrogen and nitrogen is not less than 30 vol.%.

[0046] In the step (2), when the magnet is heated in hydrogen or a mixture of hydrogen and nitrogen, the 2:14:1 phase main phase grains in the surface layer of the magnet undergo disproportionate decomposition, and the thickness of the disproportionate decomposition area can be controlled by controlling the heating temperature and heating time.

[0047] In the step (3), the diffusion treatment is generally carried out in a vacuum diffusion furnace.

[0048] In the step (3), the cooling rate is no more than 500° C. / h.

[0049] In the tempering treatment, the tempering temperature is 400° C. to 600° C. (preferably 480° C. to 420° C.), and the tempering time is 2 h to 10 h (preferably 3 h to 5 h).

[0050] In the present invention, the scattered source coating method can be PVD, spraying or printing.

[0051] NdFeB magnets are very brittle, so they are prone to chipping and falling off due to collisions during transportation and assembly. In addition, machining during the preparation of NdFeB products will cause microcracks at the corners of the magnets, making the corners of the magnets more likely to fall off due to impacts. The chipping and falling off rate of the product can be reduced by improving the mechanical properties of NdFeB magnets. The traditional method is to add a certain amount of elements such as Zr, Ti and Nb to the raw materials of the magnets. These elements strengthen the grain boundary R-rich phase of the magnet by solid solution or the formation of second-phase precipitates, thereby improving the mechanical properties of NdFeB magnets. However, as the content of non-magnetic elements increases, the remanence of the magnet will gradually decrease. At the same time, the defects of NdFeB magnets are mainly concentrated in the corner areas. Therefore, it is only necessary to improve the mechanical properties of the corner areas of the magnets to significantly reduce the chipping and falling off rate of the magnets during transportation and assembly.

[0052] Patent CN116469635A discloses a corner-strengthened RTB rare earth permanent magnet and a preparation method thereof. By analyzing the area where the magnet is prone to mechanical property defects, the magnet diffusion source coating surface is divided into a corner area and a non-corner area. The corner area of ​​the magnet is coated with a diffusion source containing Zr, Ti, and Nb elements, while the non-corner area of ​​the magnet is coated with a heavy rare earth element diffusion source that does not contain the above elements. During the grain boundary diffusion process, Zr, Ti, and Nb elements diffuse into the grain boundary R-rich phase of the magnet, and only enrich Zr, Ti, and Nb in the corner area of ​​the magnet, and strengthen the grain boundary R-rich phase in the corner area of ​​the magnet by solid solution or the formation of second phase precipitates, thereby improving the strength and other mechanical properties of the magnet corner. In addition, the diffusion source in the corner area of ​​the magnet contains a certain amount of light rare earth elements, which can repair the microcracks caused by machining during the grain boundary diffusion process, eliminate the deterioration of the mechanical properties of the magnet corner by machining, and further enhance the ability of the magnet corner to resist impact. It is of great significance to reduce the rate of product edge and corner missing.

[0053] The diffusion source H1 also contains 30.0~70.0wt.% RH. After the grain boundary diffusion of RH, a shell layer rich in heavy rare earth elements RH will be formed on the surface of the main phase grains of the magnet. Since the shell layer has a high anisotropy field, it can significantly improve the coercive force of the NdFeB magnet. The 5~40wt.% M1 in the diffusion source H1 can reduce the melting point of the diffusion source, and at the same time, it can reduce the melting point of the R-rich phase at the grain boundary of the magnet during grain boundary diffusion, increase the RH diffusion depth, and strengthen the RL's ability to repair microcracks.

[0054] Based on the prior art, the invention can further improve the coercivity of the magnet under the condition of strengthening the magnet corners by optimizing the process, and prepare the high coercivity RTB rare earth permanent magnet with corner strengthening.

[0055] The present invention first coats diffusion sources on the surface of a magnet in different areas, and then places the magnet coated with diffusion sources in different areas in hydrogen or a mixture of hydrogen and nitrogen, and keeps the temperature at 400-600°C for 10-30 minutes. The main purpose of this process is to heat in an environment containing H2 to disproportionately decompose the main phase grains on the surface of the magnet coated with diffusion sources. During the furnace cooling process after the grain boundary diffusion treatment, the main phase grains decomposed in the non-corner body area of ​​the magnet will recrystallize. The RH elements that are not consumed in the grain boundary phase during the grain boundary diffusion treatment will also participate in the recrystallization of the main phase to form new 2:14:1 main phase grains. At the beginning of crystallization, the RH element concentration in the surrounding environment is high, so the RH concentration in the core of the main phase particles is high. As the new crystallized grains grow, the RH element is gradually consumed, so the RH concentration at the edge of the main phase particles gradually decreases. Therefore, the main phase grains finally formed have a high heavy rare earth RH concentration in the center and a low heavy rare earth element RH concentration at the edge, forming a main phase grain with an RH element reverse core-shell structure.

[0056] During the furnace cooling process after the grain boundary diffusion treatment, the main phase grains decomposed in the corner region of the magnet will also recrystallize, but the crystallization process is quite different from that in the non-corner region. Since a high concentration of X element diffuses from the outside into the grain boundary phase of the corner region of the magnet during the grain boundary diffusion process, the X element reacts with the B element in the main phase particles decomposed by disproportionation to form a second phase B compound, resulting in the corner region of the magnet being in a B-poor environment during the subsequent cooling and solidification process. Since there is a certain amount of Ga in the magnet, the low B environment will promote the formation of a high-Ga, low-B phase (6:13:1 phase). Studies have shown that the heavy rare earth element RH is more easily distributed in the 6:13:1 phase because the RH element has a higher affinity with the 6:13:1 phase. At the beginning of the recrystallization of the main phase grains in the corner region, the concentration of RH elements involved in the formation of the core of the main phase particles is low. As the grain boundary process proceeds, the RH element concentration in the rare earth phase around the main phase particles continues to be enriched. As the main phase grains grow further, the amount of RH elements in the rare earth phase at the grain boundary that participate in the formation of the main phase particles increases under the action of the element concentration gradient. The main phase particles in the corner area of ​​the magnet eventually grow into main phase grains with a core-shell structure, that is, the RH concentration of heavy rare earth elements is high at the edge of the main phase grains, while the RH concentration of heavy rare earth elements in the core is low.

[0057] The coercivity of the main phase grains at the locations where defects are easily generated on the magnet surface is relatively low. Traditional grain boundary diffusion is to transform all the main phase grains within a certain depth range from the magnet surface into main phase grains with a core-shell structure enriched with RH elements on the surface, such as patent document CN116469635A. However, the present invention has found that the coercivity of the magnet can be further improved by distributing another layer of main phase grains with an RH anti-shell layer on the outside of the magnet core-shell structure main phase grains. The main reasons are as follows: (1) The anisotropy field of the core of the anti-core-shell main phase grains is improved, and the anisotropy field changes at the core-shell interface, increasing the pinning force, so the coercivity of the magnet containing the anti-core-shell main phase grains is improved. (2) The anti-core-shell main phase grains have more RH in the core and low remanence. After the anti-magnetization, the influence on the magnetization reversal of the adjacent main phase grains is also small, and the transfer of the reverse magnetic domain on the magnet surface is suppressed, so the coercivity of the magnet can be improved. Therefore, compared with the traditional magnet grain boundary diffusion method, the present invention makes the magnet have non-core-shell structure main phase grains, core-shell structure main phase grains and reverse core-shell structure main phase grains arranged in sequence from the center of the magnet to the surface A of the magnet, which can further improve the coercive force of the magnet.

[0058] The present invention finds that the internal stress of the main phase grains with the inverse core-shell structure of the RH element is greater, resulting in large brittleness of the magnet. If the main phase grains with the inverse core-shell structure of the RH element are also generated in the corner body region of the magnet, the brittleness of the corners of the magnet will increase. Therefore, in the present invention, it is necessary to control the magnet matrix to have a certain Ga element, form a certain 6:13:1 phase in the corner body region of the magnet, and suppress the generation of the main phase grains with the inverse core-shell structure of the RH element in the corner body region.

[0059] The beneficial effects of the present invention are embodied in that the magnet diffusion source coating surface is divided into a corner area and a non-corner area. The corner area of ​​the magnet is coated with a diffusion source containing Zr, Ti or Nb elements, while the non-corner area of ​​the magnet is coated with a diffusion source of heavy rare earth elements that does not contain the above elements. In the grain boundary diffusion process, Zr, Ti, and Nb elements diffuse into the grain boundary R-rich phase of the magnet, and strengthen the grain boundary R-rich phase of the magnet by solid solution or the formation of second phase precipitates, thereby improving the strength of the magnet corners. The main phase grains of the magnet within a certain depth range from the diffusion surface are decomposed by disproportionate decomposition and recrystallization treatment and recrystallized during the slow cooling process after diffusion. Then, several grain layers of main phase grains with RH element reverse shell structure are generated outside the core-shell structure main phase grains in the non-corner area of ​​the magnet, and non-core-shell structure main phase grains, core-shell structure main phase grains and reverse core-shell structure main phase grains are arranged in sequence from the core to the magnet diffusion surface in the non-corner area of ​​the magnet, thereby improving the coercive force of the magnet. The corner area of ​​the magnet is arranged with non-core-shell structure main phase grains and core-shell structure main phase grains in sequence from the core to the magnet diffusion surface, reducing the brittleness of the corner area. The magnet of the present invention not only improves the magnetic properties of the RTB magnet, but also has good corner strength, reduces production costs, and has great industrial application value. BRIEF DESCRIPTION OF THE DRAWINGS

[0060] Figure 1 Schematic diagram of the corner and non-corner areas of magnets of common shapes.

[0061] Figure 2 Schematic diagram of magnet selection printing in Experiment No. 2 and Experiment No. 6.

[0062] Figure 3 Cross-sectional view of the corner area of ​​the magnet in Experiment No. 2.

[0063] Figure 4 Microstructure diagram of non-corner area after magnet diffusion in Experiment No. 3 and Experiment No. 4.

[0064] Figure 5 Microstructure diagram of the corner area of ​​the magnets of Experiment No. 5 and Experiment No. 6. DETAILED DESCRIPTION

[0065] The sintered RTB magnet is prepared by melt-spinning SC sheets, hydrogen crushing, air flow grinding, orientation molding, isostatic pressing, vacuum sintering and aging. The bulk NdFeB magnet is processed into the required shape and size. After surface treatment, the magnet is cleaned and dried to obtain the RTB magnet matrix.

[0066] An H1 diffusion source coating area and an H2 diffusion source coating area are set on the diffusion surface of the RTB magnet substrate, and the diffusion sources are coated in different areas. The H1 diffusion source coating area coats the diffusion source H1, and the H2 diffusion source coating area coats the diffusion source H2; the H1 diffusion source coating area is the corner area of ​​the diffusion surface, and the H2 diffusion source coating area is the non-corner area of ​​the diffusion surface.

[0067] The corner area refers to the surface area within the width range of 0~Kmm from the edge line, K is 0.2~0.6, and the non-corner area refers to the surface area outside the width range of Kmm from the edge line.

[0068] Schematic diagrams of the corner and non-corner areas of some common magnet shapes are shown below: Figure 1 shown.

[0069] In the present invention, the diffusion source H1 is prepared by smelting according to the actual composition. When the diffusion source is coated by PVD, a large ingot can be directly prepared by smelting. When the diffusion source is coated by coating or printing, it is necessary to prepare a powdered diffusion source by melting SC sheets, hydrogen crushing and air flow milling.

[0070] The diffusion source H2 can directly adopt a commercial pure metal, alloy or compound ingot or powder containing at least one of the heavy rare earth elements Dy, Tb and Ho.

[0071] The magnet coated with diffusion sources in different areas is placed in hydrogen or a mixture of hydrogen and nitrogen, and kept at 400-600°C for 10-30 minutes. Then, a grain boundary diffusion treatment is performed, the diffusion temperature is 800-1000°C, and the holding time is 6-30 hours. After the treatment, the magnet is cooled to room temperature with a cooling rate of no more than 500°C / h. Then, the magnet is heated to 400-600°C and kept for 2-10 hours to obtain the magnet.

[0072] The surface of the magnet after secondary aging is sandblasted to expose the fresh surface of the magnet. ICP is used to measure the magnet composition, and SEM and EPMA are used to analyze the magnet microstructure and micro-region composition. NIM equipment is used to measure the magnetic properties of the magnet. Each group of experiments tests 11 samples and calculates the average value of the magnetic performance index. 200 products are selected for drop test, the drop height is 1 meter, the drop number is 1 time, and the corners of the magnet have a size greater than the surface area greater than 0.3mm 2 Products in defective areas are considered unqualified products, and the qualified rate of products is calculated.

[0073] Embodiment 1: The sintered RTB magnet is prepared by melt-spinning SC sheets, hydrogen crushing, air flow milling, orientation molding, isostatic pressing, vacuum sintering and aging.

[0074] The sintered and aged magnets were machined into magnet sheets with a length × width × height of 10 mm × 10 mm × 5 mm, where the height direction is the magnet orientation direction. The magnet surface was cleaned of oil and rust by pickling, then cleaned with clean water and dried.

[0075] The powder of diffusion source H1 is prepared by melt-spinning SC sheet, hydrogen crushing and air flow grinding. The powder particle size SMD is 1.5μm. The composition of the heavy rare earth element powder of diffusion source H1 is as follows: R1: 70wt.%, R1 includes R1L and RH1, RH1 is Tb and accounts for 60% of the mass ratio of H1, the balance of R1 is RL1, RL1 is Pr and Nd, the mass ratio of Pr and Nd is 25:75, Zr: 20wt.%, Ga: 10wt.%, The heavy rare earth element powder of the diffusion source H2 is commercial terbium hydride powder (Tb content 98.2wt.%), and the powder particle size SMD1.5μm.

[0076] The screen printing coating was prepared according to the following ratio: the mass ratio of heavy rare earth diffusion source powder, pineol, polyvinyl butyral and aluminum oxide was 70:26:2:2, and the screen printing coating was obtained after mixing evenly.

[0077] Diffusion sources are printed on the two surfaces of the magnet perpendicular to the orientation direction, and the thickness of the diffusion source layer is 15μm. In Experiment No.1, diffusion source H2 is printed on both surfaces of the magnet. In Experiment No.2, diffusion sources are coated in different areas, with diffusion source H1 coated on the corners of the magnet and diffusion source H2 coated on the non-corner areas. The width of the corner area is 0.4mm. Experiment No.2 realizes the partition coating of diffusion sources by designing two printing screens of different sizes. The schematic diagram of the printing screen of the magnet in Experiment No.2 is shown in the figure. Figure 2 shown. Figure 2 The printing screen can print 3 magnetic sheets of the same size at the same time.

[0078] use Figure 2 The shielding area of ​​the left printing screen is aligned with the corner area of ​​the magnet, and the hollow area is aligned with the non-corner area, which is used as the H2 diffusion source coating area. The diffusion source H2 is printed, dried, and then Figure 2 The shielding area of ​​the printing screen on the right is aligned with the non-corner area of ​​the magnet, and the hollow area is aligned with the corner area of ​​the magnet, which serves as the H1 diffusion source coating area and prints the diffusion source H1.

[0079] After printing on one side of the magnet, it is dried in a drying oven at 50°C, and then printed on the second side and dried again.

[0080] The magnet is placed in hydrogen and heated to 500°C for 20 minutes to allow the magnet surface to undergo disproportionate decomposition.

[0081] The magnet was placed in a vacuum diffusion furnace and heated to 950°C for 15 hours, and then cooled to room temperature at a rate of no more than 500°C / h. It was then heated to 520°C and kept for 4 hours to obtain the magnet.

[0082] The surface of the magnet after secondary aging is sandblasted to expose the fresh surface of the magnet. ICP is used to measure the magnet composition, and SEM and EPMA are used to analyze the magnet microstructure and micro-region composition. NIM equipment is used to measure the magnetic properties of the magnet. Each group of experiments tests 11 samples and calculates the average value of the magnetic performance index. 200 products are selected for drop test, the drop height is 1 meter, the drop number is 1 time, and the corners of the magnet have a size greater than the surface area greater than 0.3mm 2 Products in defective areas are considered unqualified products, and the qualified rate of products is calculated.

[0083] The magnet matrix composition of Experiment No. 1 and Experiment No. 2 is the same. The magnet matrix and magnet composition after grain boundary diffusion are shown in Table 1: Table 1 No. Nd Pr Co Cu Ga B Tb Fe Zr Matrix 27.6 0.60 0.97 0.1 0.2 0.96 / Bal / 1 27.7 0.61 0.97 0.1 0.2 0.96 0.21 Bal / 2 27.7 0.60 0.97 0.1 0.25 0.96 0.20 Bal 0.1 The magnetic properties and qualified rate of the magnets are shown in Table 2: Table 2 Experiment No. Br (kGs) Hcj (kOe) Pass rate (%) 1 14.49 23.1 80% 2 14.49 23.2 96% From the data in Table 1 and Table 2, it can be seen that the Tb content of the magnets of Experiment No. 1 and Experiment No. 2 is basically the same after grain boundary diffusion, but since the magnet of Experiment No. 2 adopts the method of partitioned grain boundary diffusion, that is, the diffusion source of the coating area of ​​the corners of the magnet contains a certain amount of Zr, the magnet contains 0.1wt.% Zr after grain boundary diffusion. At the same time, it can be seen from the magnetic properties of the magnets in Table 2 that the magnetic properties of Experiment No. 1 and Experiment No. 2 are basically the same after grain boundary diffusion, but the qualified rate of the magnet of Experiment No. 2 is significantly higher than that of Experiment No. 1, indicating that the partitioned grain boundary diffusion method provided by the present invention can effectively improve the mechanical properties of the corners of the NdFeB magnet, thereby reducing the edge and corner loss rate of the product.

[0084] like Figure 3As shown, the corner area of ​​the magnet was cut by precision wire cutting and its composition was tested. The results showed that the average Zr content at the corners of the magnet was 0.4wt.%, which was significantly higher than the average Zr content of the magnet. This shows that after the Zr diffusion source was coated on the surface of the corner area of ​​the magnet and grain boundary diffusion was carried out, the Zr element would be enriched at the corners of the magnet. With the help of PEMA point scanning analysis, it was found that the Zr element was mainly distributed in the grain boundary R-rich phase of the magnet. The Zr element can strengthen the grain boundary R-rich phase of the magnet by solid solution or the formation of second phase precipitates, thereby improving the mechanical properties of the corners of the magnet.

[0085] EPMA surface scanning was used to analyze the average light rare earth element content of the surface corner area of ​​the magnet surface A and the overall average light rare earth element content of the surface A, and it was found that the light rare earth element content of the corner area of ​​the magnet surface A was not lower than the average light rare earth content of the surface A. In the corner area diffusion source H1 of the present invention, part of the light rare earth element RL was used to replace RH. After grain boundary diffusion, RL was mainly concentrated in the grain boundary phase of the magnet, repairing the microcracks at the corners of the magnet caused by machining, thereby enhancing the mechanical properties of the corners of the magnet. In addition, due to the high diffusion rate of RL, it will not be enriched only in the corner area of ​​the magnet, so the light rare earth element content of the corner area of ​​the magnet surface A is not lower than the average light rare earth content of the surface A. In addition, it can be seen from the data in Table 2 that the magnetic properties of the magnet of Experiment No. 2 are not reduced compared with Experiment No. 1, so the use of part of the light rare earth element RL to replace RH in the diffusion source H1 of the present invention does not lead to a reduction in magnetic properties.

[0086] The present invention realizes the partitioned grain boundary diffusion of the NdFeB magnet by using the partitioned coating diffusion source method, by coating the diffusion source containing Zr, Ti, and Nb elements in the corner area of ​​the magnet, and coating the diffusion source without the above elements in the non-corner area of ​​the magnet. During the grain boundary diffusion process, the Zr, Ti, and Nb elements diffuse into the grain boundary R-rich phase of the magnet, and strengthen the grain boundary R-rich phase of the magnet by solid solution or generation of second phase precipitates, thereby improving the strength of the magnet corner. The present invention improves the mechanical properties of the magnet corner area by partitioned grain boundary diffusion without affecting the non-corner area of ​​the magnet.

[0087] Embodiment 2: The sintered RTB magnet is prepared by melt-spinning SC sheets, hydrogen crushing, air flow milling, orientation molding, isostatic pressing, vacuum sintering and aging.

[0088] The sintered and aged magnets were machined into magnet sheets with a length × width × height of 10 mm × 10 mm × 5 mm, where the height direction is the magnet orientation direction. The magnet surface was cleaned of oil and rust by pickling, then cleaned with clean water and dried.

[0089] The powder of diffusion source H1 is prepared by melt-spinning SC sheet, hydrogen crushing and air flow grinding. The powder particle size SMD is 1.5μm. The composition of the heavy rare earth element powder of diffusion source H1 is as follows: R1: 70wt.%, R1 contains RL1 and RH1, RH1 is Tb and accounts for 60% of the mass ratio of H1, the remainder of R1 is RL1, RL1 is Nd, Ti: 20wt.%, Ga: 10wt.%, The heavy rare earth element powder of the diffusion source H2 is commercial terbium hydride powder (Tb content 98.2wt.%), and the powder particle size SMD1.5μm.

[0090] The screen printing coating was prepared according to the following ratio: the mass ratio of heavy rare earth diffusion source powder, pineol, polyvinyl butyral and aluminum oxide was 70:26:2:2, and the screen printing coating was obtained after mixing evenly.

[0091] Diffusion sources are printed on the two surfaces of the magnet perpendicular to the orientation direction, and the thickness of the diffusion source layer is 15μm. Experiment No. 3 and Experiment No. 4 magnets are both coated with diffusion sources in different areas. Diffusion source H1 is coated on the corner area of ​​the magnet, and diffusion source H2 is coated on the non-corner area. The width of the corner area is 0.4mm. The diffusion source is coated in different areas by designing two printing screens of different sizes. The schematic diagram of the printing screen is shown in the figure. Figure 2 shown. Figure 2 The printing screen can print 3 magnetic sheets of the same size at the same time.

[0092] use Figure 2 The shielding area of ​​the left printing screen is aligned with the corner area of ​​the magnet, and the hollow area is aligned with the non-corner area, which is used as the H2 diffusion source coating area. The diffusion source H2 is printed, dried, and then Figure 2 The shielding area of ​​the printing screen on the right is aligned with the non-corner area of ​​the magnet, and the hollow area is aligned with the corner area of ​​the magnet, which serves as the H1 diffusion source coating area and prints the diffusion source H1.

[0093] After printing on one side of the magnet, it is dried in a drying oven at 50°C, and then printed on the second side and dried again.

[0094] In Experiment No. 4, the magnet was subjected to a disproportionate decomposition process before diffusion, that is, the magnet coated with the diffusion source was placed in hydrogen and heated to 500° C. for 20 minutes to disproportionately decompose the magnet surface. In Experiment No. 3, the magnet was not subjected to the disproportionate decomposition process.

[0095] The magnet was placed in a vacuum diffusion furnace and heated to 950°C for 15 hours, and then cooled to room temperature at a rate of no more than 500°C / h. It was then heated to 520°C and kept for 4 hours to obtain the magnet.

[0096] The surface of the magnet after secondary aging is sandblasted to expose the fresh surface of the magnet. ICP is used to measure the magnet composition, and SEM and EPMA are used to analyze the magnet microstructure and micro-region composition. NIM equipment is used to measure the magnetic properties of the magnet. Each group of experiments tests 11 samples and calculates the average value of the magnetic performance index. 200 products are selected for drop test, the drop height is 1 meter, the drop number is 1 time, and the corners of the magnet have a size greater than the surface area greater than 0.3mm 2 Products in defective areas are considered unqualified products, and the qualified rate of products is calculated.

[0097] The magnet matrix composition of Experiment No. 3 and Experiment No. 4 is the same. The magnet matrix and magnet composition after grain boundary diffusion are shown in Table 3: Table 3 No. Nd Co Cu Ga Tb B Fe Ti Matrix 28.5 1.5 0.15 0.10 / 0.93 Bal 0.1 3 28.5 1.5 0.15 0.15 0.22 0.93 Bal 0.16 4 28.5 1.5 0.15 0.15 0.22 0.93 Bal 0.16 The magnetic properties and qualified rate of the magnets are shown in Table 4: Table 4 Experiment No. Br (kGs) Hcj (kOe) Pass rate (%) 3 14.46 22.0 97.8% 4 14.46 23.5 98.0% From the data in Table 3 and Table 4, we can see that the qualified rates of the products in Experiment No. 3 and Experiment No. 4 are both high, indicating that the qualified rate of the magnets will not be affected by the disproportionate decomposition treatment before diffusion. By comparing the coercive forces of the magnets in Experiment No. 3 and Experiment No. 4, we can see that the coercive force of the magnets in Experiment No. 4 is significantly higher than that of the magnets in Experiment No. 3. Figure 4 It can be seen that in the non-corner area within a certain depth range from the magnet surface A of the No.3 magnet, there is only a core-shell structure main phase grain layer. In the non-corner area within a certain depth range from the magnet surface A of the experiment No.4 magnet, there is a layer of anti-core-shell structure main phase grain area within a certain depth range from the magnet surface A, in which the RH element concentration in the core of the main phase grain is higher than that in the edge of the main phase. Below the anti-core-shell structure main phase grain area is the core-shell structure main phase grain area, in which the RH element concentration in the edge of the magnet main phase grain is higher than that in the center of the main phase grain.

[0098] The present invention first coats diffusion sources on the surface of a magnet in different areas, and then places the magnet coated with diffusion sources in different areas in hydrogen or a mixture of hydrogen and nitrogen, and keeps the temperature at 400-600°C for 10-30 minutes. The main purpose of this process is to heat in an environment containing H2 to disproportionately decompose the main phase grains on the surface of the magnet coated with diffusion sources. During the furnace cooling process after the grain boundary diffusion treatment, the main phase grains decomposed in the non-corner area of ​​the magnet will recrystallize. The RH elements that are not consumed in the grain boundary phase during the grain boundary diffusion treatment will also participate in the recrystallization of the main phase to form new 2:14:1 main phase grains. At the beginning of crystallization, the RH element concentration in the surrounding environment is high, so the RH concentration in the core of the main phase particles is high. As the new crystallized grains grow, the RH element is gradually consumed, so the RH concentration at the edge of the main phase particles gradually decreases. Finally, the main phase grains with a high heavy rare earth RH concentration in the center and a low heavy rare earth RH concentration at the edge are formed, and the RH element reverse core-shell structure is formed.

[0099] The anisotropy field of the core of the main phase grains of the inverse core-shell structure is high, and the anisotropy field changes at the core-shell interface, and the pinning force increases, so the coercive force of the magnet containing the inverse core-shell main phase grains is improved. Secondly, the main phase grains of the inverse core-shell structure have more RH in the core and low remanence. The influence of the magnetization reversal of the adjacent main phase particles after the reverse magnetization is also small, and the transfer of the reverse magnetic domain on the surface of the magnet is suppressed, which can improve the coercive force of the magnet. Therefore, the method of the present invention can significantly reduce the edge and corner missing rate of the magnet during transportation and assembly, and improve the coercive force of the magnet.

[0100] Embodiment three: The sintered RTB magnet is prepared by melt-spinning SC sheets, hydrogen crushing, air flow milling, orientation molding, isostatic pressing, vacuum sintering and aging.

[0101] The sintered and aged magnets were machined into magnet sheets with a length × width × height of 10 mm × 10 mm × 5 mm, where the height direction is the magnet orientation direction. The magnet surface was cleaned of oil and rust by pickling, then cleaned with clean water and dried.

[0102] The powder of diffusion source H1 is prepared by melt-spinning SC sheet, hydrogen crushing and air flow grinding. The powder particle size SMD is 1.5μm. The composition of the heavy rare earth element powder of diffusion source H1 is as follows: R1: 70wt.%, R1 includes RL1 and RH1, RH1 is Tb and accounts for 60% of the mass ratio of H1, the remainder of R1 is RL1, and RL1 is Nd.

[0103] Nb: 20wt.%, Ga: 10wt.%, The heavy rare earth element powder of the diffusion source H2 is commercial terbium hydride powder (Tb content 98.2wt.%), and the powder particle size SMD1.5μm.

[0104] The screen printing coating was prepared according to the following ratio: the mass ratio of heavy rare earth diffusion source powder, pineol, polyvinyl butyral and aluminum oxide was 70:26:2:2, and the screen printing coating was obtained after mixing evenly.

[0105] Diffusion sources are printed on the two surfaces of the magnet perpendicular to the orientation direction, and the thickness of the diffusion source layer is 15μm. Experiment No. 5 and Experiment No. 6 magnets are both coated with diffusion sources in different areas. Diffusion source H1 is coated on the corner area of ​​the magnet, and diffusion source H2 is coated on the non-corner area. The width of the corner area is 0.4mm. The diffusion source is coated in different areas by designing two printing screens of different sizes. The schematic diagram of the printing screen is shown in the figure. Figure 2 shown. Figure 2 The printing screen can print 3 magnetic sheets of the same size at the same time.

[0106] use Figure 2 The shielding area of ​​the left printing screen is aligned with the corner area of ​​the magnet, and the hollow area is aligned with the non-corner area, which is used as the H2 diffusion source coating area. The diffusion source H2 is printed, dried, and then Figure 2 The shielding area of ​​the printing screen on the right is aligned with the non-corner area of ​​the magnet, and the hollow area is aligned with the corner area of ​​the magnet, which serves as the H1 diffusion source coating area and prints the diffusion source H1.

[0107] After printing on one side of the magnet, it is dried in a drying oven at 50°C, and then printed on the second side and dried again.

[0108] The magnets of Experiment No. 5 and Experiment No. 6 were subjected to a disproportionate decomposition process before diffusion, that is, the magnets coated with diffusion sources were placed in hydrogen and heated to 500° C. and kept warm for 20 minutes to allow the magnet surface to undergo disproportionate decomposition.

[0109] The magnet is placed in a vacuum diffusion furnace and heated to 950°C for 15 hours. After the heating, it is cooled to room temperature at a rate not higher than 500°C / h, and then heated to 520°C for 4 hours to obtain the magnet.

[0110] The surface of the magnet after secondary aging is sandblasted to expose the fresh surface of the magnet. ICP is used to measure the magnet composition, and SEM and EPMA are used to analyze the magnet microstructure and micro-region composition. NIM equipment is used to measure the magnetic properties of the magnet. Each group of experiments tests 11 samples and calculates the average value of the magnetic performance index. 200 products are selected for drop test, the drop height is 1 meter, the drop number is 1 time, and the corners of the magnet have a size greater than the surface area greater than 0.3mm 2 Products in defective areas are considered unqualified products, and the qualified rate of products is calculated.

[0111] The magnet matrix compositions of Experiment No. 5 and Experiment No. 6 are different. The magnet matrix and magnet compositions after grain boundary diffusion are shown in Table 5: Table 5 No. Nd Co Cu Ga Tb B Fe Ti Nb No.5 Matrix 28.6 1.5 0.15 0 / 0.96 Bal 0.1 0 No.6 Matrix 28.6 1.5 0.15 0.10 / 0.96 Bal 0.1 0 5 28.6 1.5 0.15 0.02 0.22 0.96 Bal 0.1 0.11 6 28.6 1.5 0.15 0.12 0.22 0.96 Bal 0.1 0.11 The magnetic properties and qualified rate of the magnets are shown in Table 6: Table 6 Experiment No. Br (kGs) Hcj (kOe) Pass rate (%) 5 14.41 24.2 87.1% 6 14.41 24.4 99.3% It can be seen from the data in Table 5 and Table 6 that the magnetic properties of the magnets of Experiment No. 5 and Experiment No. 6 are basically the same after diffusion, while the edge and corner qualified rate of Experiment No. 5 is much lower than that of Experiment No. 6. Figure 5The microstructures of the corner regions of the magnets of Experiment No. 5 and Experiment No. 6 are shown respectively. It can be seen that the main phase grains of the RH inverse core-shell structure are distributed near the surface A of the corner region of the magnet of Experiment No. 5, while the main phase grains of the RH inverse core-shell structure do not exist near the surface A of the corner region of the magnet of Experiment No. 6. This is because the magnet matrix of Experiment No. 6 contains a certain Ga element, while the magnet matrix of Experiment No. 5 does not contain Ga element. During the furnace cooling process after the grain boundary diffusion treatment of the magnets of Experiment No. 5 and No. 6, the main phase grains decomposed in the corner region of the magnet will recrystallize. Since a high concentration of X element diffuses from the outside into the grain boundary phase of the corner region of the magnet during the grain boundary diffusion process, the X element will react with the B element in the main phase particles of the disproportionate decomposition to form a second phase B compound, resulting in the corner region of the magnet being in a low B environment during the subsequent cooling and solidification process. Since there is a certain Ga element in the magnet of Experiment No. 6, the low B environment will promote the formation of a high Ga and low B phase (6:13:1 phase). Studies have shown that the RH element has a higher affinity with the 6:13:1 phase, so the heavy rare earth element RH is more easily distributed in the 6:13:1 phase. Therefore, during the recrystallization process of the main phase grains in the corner area of ​​the magnet of Experiment No. 6, the concentration of RH elements participating in the formation of the core of the main phase particles is low. As the grain boundary process proceeds, the concentration of RH elements in the rare earth phase around the main phase particles continues to be enriched. As the main phase grains grow further, the amount of RH elements participating in the formation of the main phase particles increases under the action of the element concentration gradient. Under this action, the main phase particles in the corner area of ​​the magnet grow into main phase grains with a core-shell structure, that is, the concentration of heavy rare earth elements RH is high at the edge of the main phase grains, while the concentration of heavy rare earth elements RH is low in the center. However, the matrix of the magnet of Experiment No. 5 does not contain Ga, so the 6:13:1 phase will not be formed. Therefore, main phase grains with RH inverse core-shell structure will be formed in the corner area of ​​the magnet of Experiment No. 5. Due to the greater stress in the main phase grains with RH inverse shell structure, the magnet is brittle. When the main phase grains with the RH element inverse core-shell structure are generated in the corner region of the magnet, the brittleness of the corner of the magnet will increase. Therefore, in the present invention, it is necessary to control the magnet matrix to have a certain amount of Ga element (more than 0.1wt%) to inhibit the generation of the main phase grains with the RH element inverse core-shell structure in the corner region.

[0112] Embodiment 4: The sintered RTB magnet is prepared by melt-spinning SC sheets, hydrogen crushing, air flow milling, orientation molding, isostatic pressing, vacuum sintering and aging.

[0113] The sintered and aged magnets were machined into magnet sheets with a length × width × height of 10 mm × 10 mm × 5 mm, where the height direction is the magnet orientation direction. The magnet surface was cleaned of oil and rust by pickling, then cleaned with clean water and dried.

[0114] The powder of the diffusion source H1 was prepared by melt-spinning SC sheets, hydrogen crushing, and air flow grinding. The powder particle size SMD was 1.5 μm. The heavy rare earth element powder composition of the diffusion source H1 of Experiment No. 7 and Experiment No. 8 was as follows: R1: 75wt.%, R1 contains RL1 and RH1, RH1 is Tb and accounts for 60% of the mass ratio of H1, the balance of R1 is RL1, RL1 is Pr and Nd, the mass ratio of Pr and Nd is 25:75, Ti: 15wt.%, Cu: 15wt.%, The diffusion source H2 containing heavy rare earth element powder is commercial terbium hydride powder, and the powder particle size SMD is 1.5 μm.

[0115] The screen printing coating was prepared according to the following ratio: the mass ratio of heavy rare earth diffusion source powder, pineol, polyvinyl butyral and aluminum oxide was 70:26:2:2, and the screen printing coating was obtained after mixing evenly.

[0116] Diffusion sources are printed on two surfaces of the magnet perpendicular to the orientation direction, and the thickness of the diffusion source layer is 20 μm.

[0117] The diffusion source is coated in different areas. The corner area of ​​the magnet is coated with diffusion source H1, and the non-corner area is coated with diffusion source H2. The width of the corner area is 0.4mm. The diffusion source is coated by printing. After printing on one side of the magnet, it is dried in a drying tunnel at 50°C, and then the second side is printed and then dried again.

[0118] The magnets of Experiment No.7 and Experiment No.8 were subjected to a disproportionate decomposition process before diffusion. The magnets of Experiment No.7 were placed in a mixed gas of 80 vol.% and 20 vol.% N2 and H2, respectively, while the magnets of Experiment No.8 were placed in a mixed gas of 70 vol.% and 30 vol.% N2 and H2, respectively. They were then heated at 500°C for 20 minutes.

[0119] The magnet is placed in a vacuum diffusion furnace and heated to 950°C for 15 hours. After the heating, it is cooled to room temperature at a rate not higher than 500°C / h, and then heated to 520°C for 4 hours to obtain the magnet.

[0120] The surface of the magnet after secondary aging is sandblasted to expose the fresh surface of the magnet. ICP is used to measure the magnet composition, and SEM and EPMA are used to analyze the magnet microstructure and micro-region composition. NIM equipment is used to measure the magnetic properties of the magnet. Each group of experiments tests 11 samples and calculates the average value of the magnetic performance index. 200 products are selected for drop test, the drop height is 1 meter, the drop number is 1 time, and the corners of the magnet have a size greater than the surface area greater than 0.3mm 2Products in defective areas are considered unqualified products, and the qualified rate of products is calculated.

[0121] The magnet matrix composition of Experiment No. 7 and Experiment No. 8 is the same. The magnet matrix and magnet composition after grain boundary diffusion are shown in Table 7: Table 7 No. Nd Pr Co Cu Ga Tb Fe Zr Ti B Matrix 27.6 0.8 2.5 0.3 0.2 / Bal 0.1 / 1.01 7 27.8 0.8 2.5 0.36 0.2 0.22 Bal 0.1 0.08 1.01 8 27.8 0.8 2.5 0.36 0.2 0.22 Bal 0.1 0.08 1.01 The magnetic properties and qualified rate of the magnets are shown in Table 8: Table 8 Experiment No. Br (kGs) Hcj (kOe) Pass rate (%) 7 14.48 22.9 97% 8 14.48 24.2 97% It can be seen from the experimental results in Tables 7 and 8 that the use of different disproportionate decomposition atmospheres will not affect the strengthening effect of the corners of the magnets after diffusion and the qualified rate of the magnets, but will affect the coercive force of the magnets after diffusion. The coercive force of the magnets in Experiment No. 8 is significantly higher than that of the magnets in Experiment No. 7. By analyzing the microstructure of the magnets in Experiment No. 7 after diffusion, it is found that the thickness of the anti-core-shell main phase grain region in the non-corner area of ​​the magnet is significantly reduced. The thickness of the anti-core-shell structure main phase grain region of the magnet in Experiment No. 8 is 60μm, while the thickness of the anti-core-shell structure main phase grain region of the magnet in Experiment No. 7 is 15μm. The enhancement effect of the anti-core-shell structure main phase grains on the coercive force of the magnet is reduced, resulting in a reduction in the coercive force of the magnet in Experiment No. 7.

[0122] The disproportionate decomposition of the main phase grains of the magnet requires the participation of hydrogen. When the proportion of H2 in the mixed atmosphere is relatively small, the thickness of the main phase of the disproportionate decomposition of the magnet surface is reduced. Therefore, the thickness of the main phase grain area of ​​the anti-core-shell structure finally generated in the non-corner area of ​​the magnet is reduced. Therefore, in order to ensure the coercive force increment of the magnet in the present invention, when a mixed gas of hydrogen and nitrogen is used as the atmosphere for the disproportionate decomposition of the magnet, the proportion of hydrogen is not less than 30 vol.%.

[0123] Embodiment five: The sintered RTB magnet is prepared by melt-spinning SC sheets, hydrogen crushing, air flow milling, orientation molding, isostatic pressing, vacuum sintering and aging.

[0124] The sintered and aged magnets were machined into magnet sheets with a length × width × height of 10 mm × 10 mm × 5 mm, where the height direction is the magnet orientation direction. The magnet surface was cleaned of oil and rust by pickling, then cleaned with clean water and dried.

[0125] The powder of diffusion source H1 is prepared by melt-spinning SC sheet, hydrogen crushing and air flow grinding. The powder particle size SMD is 1.5μm. The composition of the heavy rare earth element powder of diffusion source H1 is as follows: R1: 70wt.%, R includes RL1 and RH1, RH1 is Tb and accounts for 60% of the mass ratio of H1, the remainder of R1 is RL1, RL1 is Nd, Zr: 20wt.%, Ga: 10wt.%, The heavy rare earth element powder of the diffusion source H2 is commercial terbium hydride powder (Tb content 98.2wt.%), and the powder particle size SMD1.5μm.

[0126] The screen printing coating was prepared according to the following ratio: the mass ratio of heavy rare earth diffusion source powder, pineol, polyvinyl butyral and aluminum oxide was 70:26:2:2, and the screen printing coating was obtained after mixing evenly.

[0127] Diffusion sources are printed on the two surfaces of the magnet perpendicular to the orientation direction, and the thickness of the diffusion source layer is 15μm. Experiment No. 9 to Experiment No. 13 magnets all use zoned coating of diffusion sources, with diffusion source H1 coated on the corner area of ​​the magnet and diffusion source H2 coated on the non-corner area. The width of the corner area is 0.4mm. The zoned coating of the diffusion source is achieved by designing two printing screens of different sizes. The schematic diagram of the printing screen is shown in the figure. Figure 2 shown. Figure 2 The printing screen can print 3 magnetic sheets of the same size at the same time.

[0128] use Figure 2 The shielding area of ​​the left printing screen is aligned with the corner area of ​​the magnet, and the hollow area is aligned with the non-corner area, which is used as the H2 diffusion source coating area. The diffusion source H2 is printed, dried, and then Figure 2 The shielding area of ​​the printing screen on the right is aligned with the non-corner area of ​​the magnet, and the hollow area is aligned with the corner area of ​​the magnet, which serves as the H1 diffusion source coating area and prints the diffusion source H1.

[0129] After printing on one side of the magnet, it is dried in a drying oven at 50°C, and then printed on the second side and dried again.

[0130] In experiments No. 9 to No. 13, the magnets were placed in hydrogen and subjected to the disproportionation decomposition steps shown in Table 10.

[0131] The magnet was placed in a vacuum diffusion furnace and heated to 950°C for 15 hours, and then cooled to room temperature at a rate of no more than 500°C / h, and then heated to 520°C for 4 hours to obtain the magnet.

[0132] The surface of the magnet after secondary aging is sandblasted to expose the fresh surface of the magnet. ICP is used to measure the magnet composition, and SEM and EPMA are used to analyze the magnet microstructure and micro-region composition. NIM equipment is used to measure the magnetic properties of the magnet. Each group of experiments tests 11 samples and calculates the average value of the magnetic performance index. 200 products are selected for drop test, the drop height is 1 meter, the drop number is 1 time, and the corners of the magnet have a size greater than the surface area greater than 0.3mm 2 Products in defective areas are considered unqualified products, and the qualified rate of products is calculated.

[0133] The disproportionate decomposition of the magnets of Experiment No.9~No.13 is shown in Table 9: Table 9 Experiment No. Decomposition temperature (℃) Decomposition time (min) 9 500 20 10 600 15 11 400 30 12 600 45 13 800 10 The magnet matrix compositions of Experiment No. 9 to Experiment No. 13 are the same. The magnet matrix and magnet compositions after grain boundary diffusion are shown in Table 10. It can be seen that different disproportionate decomposition processes will not affect the composition of the magnet after diffusion.

[0134] Table 10 No. Nd Co Cu Ga Tb B Fe Zr Matrix 28.7 1.5 0.15 0.10 / 0.93 Bal 0.1 9 28.7 1.5 0.15 0.15 0.22 0.93 Bal 0.16 10 28.7 1.5 0.15 0.15 0.22 0.93 Bal 0.16 11 28.7 1.5 0.15 0.15 0.22 0.93 Bal 0.16 12 28.7 1.5 0.15 0.15 0.22 0.93 Bal 0.16 13 28.7 1.5 0.15 0.15 0.22 0.93 Bal 0.16 The magnetic properties and qualified rate of the magnets are shown in Table 11: Table 11 Experiment No. Br (kGs) Hcj (kOe) Pass rate (%) 9 14.46 23.5 98.0% 10 14.47 23.6 98.5% 11 14.47 23.4 98.5% 12 14.38 23.6 98.3% 13 14.35 23.6 98.1% From the data in Table 11, we can see that the qualified rates of the products of Experiment No.9~No.13 are all high, indicating that different disproportionate decomposition treatments will not affect the qualified rate of the magnets. However, by comparing the magnetic properties of magnets in different experimental groups, we can see that the coercive forces of the magnets in each experimental group are basically the same, but the remanence of the magnets in Experiment No.9~No.11 is much higher than that in Experiment No.12 and Experiment No.13.

[0135] By analyzing the microstructure of the magnets after diffusion in different experimental groups, the size of the main phase grain area of ​​the anti-shell structure was statistically analyzed. The thickness of the main phase grain area of ​​the anti-shell structure of the magnets in Experiment No. 9 to Experiment No. 13 was 62μm, 50μm, 45μm, 150μm and 200μm, respectively. The main phase grains of the anti-core-shell structure have an enhancing effect on the coercive force of the magnet, but the present invention finds that when the thickness exceeds 100μm, the promoting effect on the coercive force is no longer significant. On the contrary, the increase in the thickness of the anti-core-shell main phase grain area will significantly reduce the remanence of the magnet. Therefore, in the present invention, it is necessary to control the thickness of the anti-shell main phase grain area, and therefore it is also necessary to control the process of the disproportionation decomposition process. In the present invention, the preferred disproportionation decomposition temperature is 400~600℃, and the holding time is 10-30min.

[0136] Embodiment 6 The sintered RTB magnet is prepared by melt-spinning SC sheets, hydrogen crushing, air flow milling, orientation molding, isostatic pressing, vacuum sintering and aging.

[0137] The sintered and aged magnets were machined into magnet sheets with a length × width × height of 10 mm × 10 mm × 5 mm, where the height direction is the magnet orientation direction. The magnet surface was cleaned of oil and rust by pickling, then cleaned with clean water and dried.

[0138] The powder of the diffusion source H1 was prepared by melting SC sheet, hydrogen crushing and air flow grinding. The powder particle size SMD was 1.5 μm. The heavy rare earth element powder composition of the diffusion source H1 of Experiment No. 14 and Experiment No. 15 was as follows: R: 75wt.%, R includes RL and RH, RH is Tb and accounts for 60% of the mass ratio of H1, the balance of R is RL, RL is Pr and Nd, the mass ratio of Pr and Nd is 25:75, Ti: 15wt.%, Cu: 15wt.%, The diffusion source H2 containing heavy rare earth element powder is commercial terbium hydride powder, and the powder particle size SMD is 1.5 μm.

[0139] The screen printing coating was prepared according to the following ratio: the mass ratio of heavy rare earth diffusion source powder, pineol, polyvinyl butyral and aluminum oxide was 70:26:2:2, and the screen printing coating was obtained after mixing evenly.

[0140] Diffusion sources are printed on two surfaces of the magnet perpendicular to the orientation direction, and the thickness of the diffusion source layer is 20 μm.

[0141] The diffusion source is coated in different areas. The corner area of ​​the magnet is coated with diffusion source H1, and the non-corner area is coated with diffusion source H2. The width of the corner area is 0.4mm. The diffusion source is coated by printing. After printing on one side of the magnet, it is dried in a drying tunnel at 50°C, and then the second side is printed and then dried again.

[0142] The magnets of Experiment No. 14 and Experiment No. 15 were placed in hydrogen and subjected to a disproportionation decomposition process at a heating temperature of 500° C. for 20 minutes.

[0143] The magnet was placed in a vacuum diffusion furnace and heated to 950°C for 15 hours, then cooled to room temperature. The cooling rate of experiment No. 14 was 500°C / h, and experiment No. 15 adopted conventional air cooling with a cooling rate of 820°C / h.

[0144] After cooling, the mixture was heated to 520° C. and kept at this temperature for 4 hours to obtain the magnet.

[0145] The surface of the magnet after secondary aging is sandblasted to expose the fresh surface of the magnet. ICP is used to measure the magnet composition, and SEM and EPMA are used to analyze the magnet microstructure and micro-region composition. NIM equipment is used to measure the magnetic properties of the magnet. Each group of experiments tests 11 samples and calculates the average value of the magnetic performance index. 200 products are selected for drop test, the drop height is 1 meter, the drop number is 1 time, and the corners of the magnet have a size greater than the surface area greater than 0.3mm 2 Products in defective areas are considered unqualified products, and the qualified rate of products is calculated.

[0146] The magnet matrix composition of Experiment No. 14 and Experiment No. 15 is the same. The magnet matrix and magnet composition after grain boundary diffusion are shown in Table 12: Table 12 No. Nd Pr Co Cu Ga Tb Fe Zr Ti B Matrix 27.6 0.8 2.5 0.3 0.2 / Bal 0.1 / 1.01 14 27.8 0.8 2.5 0.35 0.2 0.22 Bal 0.1 0.08 1.01 15 27.8 0.8 2.5 0.35 0.2 0.22 Bal 0.1 0.08 1.01 The magnetic properties and qualified rate of the magnets are shown in Table 13: Table 13 Experiment No. Br (kGs) Hcj (kOe) Pass rate (%) 14 14.48 24.2 97% 15 14.43 23.9 97% As shown in Table 13, the Br and Hcj of the magnet in Experiment No. 15 using conventional air cooling are slightly lower than those in Experiment No. 14. This is because the cooling rate of air cooling is relatively fast, which is not conducive to the recrystallization of the decomposed main phase on the surface of the magnet. The crystallization of the main phase on the surface of the magnet is incomplete, resulting in the Br of the magnet being slightly lower than that of Experiment No. 14. In addition, due to the incomplete crystallization of the main phase on the surface, the amount of the main phase grains formed in the anti-shell layer is reduced, resulting in a decrease in the coercive force of the magnet. Therefore, in the present invention, it is preferred to use slow cooling, that is, the cooling rate is not greater than 500°C / h.

Claims

1. A high coercivity RTB rare earth permanent magnet with corner reinforcement, characterized in that The magnet contains the following components in mass fractions: R: 28.5~34.0wt.%, R is composed of RL and RH, the content of RH is 0.1wt.%~10.0wt.% of the mass of the magnet, RH is at least one of Dy, Tb, Ho; the remainder of R is RL, RL represents one or more elements selected from Nd, Pr, La, Ce, Er, Gd, Sm, Tm, Lu, Y containing at least light rare earth elements; the light rare earth elements are one or more of La, Ce, Pr, Nd; B: 0.85~1.1wt.%, Ga: 0.1~1.0wt.%, M: 0.01-8.0 wt.%, M represents a plurality of elements selected from Al, Cu, Ga, Ni, Zn, Sn, Mn, Cr, Zr, Ti, and Nb, including at least X, where X is one or more of Zr, Ti, and Nb; The balance is T and other unavoidable impurities, T is Fe or Fe and Co; The magnet has at least one surface A, the light rare earth element content of the corner area of ​​the surface A is not less than the average light rare earth content of the surface A; the light rare earth element is one or more of La, Ce, Pr, and Nd; and the corner area of ​​the surface A contains X, and X is one or more of Zr, Ti, and Nb; Within a depth range of 0.6 mm vertically from the surface A of the magnet, the corner body region does not contain anti-core-shell structure main phase grains, and the non-corner body region contains some anti-core-shell structure main phase grains. The anti-core-shell structure main phase grains have a core portion and a shell portion encapsulating the core portion, and the RH mass concentration of the shell portion is lower than the RH mass concentration of the core portion.

2. The high coercivity RTB rare earth permanent magnet with corner reinforcement as claimed in claim 1, characterized in that From the center of the magnet to the magnet surface A, the non-corner body region is sequentially arranged with non-core-shell structure main phase grains, core-shell structure main phase grains and anti-core-shell structure main phase grains; the corner body region is sequentially arranged with non-core-shell structure main phase grains and core-shell structure main phase grains.

3. The edge-strengthened high coercivity RTB rare earth permanent magnet according to claim 2, characterized in that: The thickness of the magnet region containing the main phase grains of the inverse core-shell structure is 30~100μm.

4. The high coercive force RTB rare earth permanent magnet with corner reinforcement as claimed in claim 2, characterized in that The inverse core-shell structure main phase grains are magnet main phase grains whose shell RH mass concentration C1 and core RH mass concentration C2 satisfy C2 / C1>1.1; the core-shell structure main phase grains are magnet main phase grains whose shell RH mass concentration C1 and core RH mass concentration C2 satisfy C1 / C2>1.1; the non-core-shell structure main phase grains are main phase grains with uniform RH concentration distribution inside, and no core-shell structure or inverse core-shell structure exists.

5. The edge-strengthened high coercivity RTB rare earth permanent magnet according to claim 1, characterized in that Within the depth range of 0.6 mm vertically from the surface A of the magnet, the X content in the corner area is 0.05-1.2 wt.%; the average X content of the magnet is 0.05-0.8 wt.%.

6. The edge-strengthened high coercivity RTB rare earth permanent magnet according to claim 1, characterized in that The corner area refers to the surface area within the range of 0~Kmm width from the edge of the magnet, K is the width of the corner area, and the range of K is 0.2~0.

6. The non-corner area refers to the surface area outside the range of Kmm width from the edge; The corner body region is the body region enclosed by the corner area and a depth of 0.6 mm vertically away from the surface A; the non-corner body region is the magnet region outside the corner body region; the non-corner body region of the magnet does not contain X, or the X content in the non-corner body region is lower than the X content in the corner body region of the magnet;.

7. The edge-strengthened high coercivity RTB rare earth permanent magnet according to any one of claims 1 to 6, characterized in that The edge-strengthened high coercivity RTB rare earth permanent magnet is prepared according to the following method: (1) An H1 diffusion source coating area and an H2 diffusion source coating area are set on the diffusion surface of the RTB magnet substrate, and the diffusion sources are coated in different areas. The H1 diffusion source coating area is coated with the diffusion source H1, and the H2 diffusion source coating area is coated with the diffusion source H2; the H1 diffusion source coating area is the corner area of ​​the diffusion surface, and the H2 diffusion source coating area is the non-corner area of ​​the diffusion surface; The RTB magnet matrix contains more than 0.1wt% Ga; The diffusion source H1 includes the following components by mass fraction: R1: 50.0~80.0wt.%, R1 includes RL1 and RH1, RH1 is one or more of Dy, Tb, Ho, and accounts for 30.0~70.0wt.% of the mass ratio of H1, and the balance of R1 is RL1, RL1 represents one or more elements selected from Nd, Pr, La, Ce, Er, Gd, Sm, Tm, Lu, Y containing at least light rare earth elements; the light rare earth elements are one or more of La, Ce, Pr, Nd; X1: 10-30wt.%, X1 is one or more of Zr, Ti, and Nb; M1: 5.0~40.0wt.%, M1 is one or more of Al, Ga, and Cu; The diffusion source H2 is one or more mixtures of pure metals, alloys or compounds containing heavy rare earth elements, and the heavy rare earth element is at least one of Dy, Tb and Ho; And the content of heavy rare earth elements in the diffusion source H1 is lower than that in H2; (2) placing the magnet coated with diffusion sources in a hydrogen or hydrogen and nitrogen mixture at 400-600°C for 10-30 minutes; (3) The magnet of step (2) is subjected to diffusion treatment at a diffusion temperature of 800° C. to 1000° C. for a holding time of 6 to 30 hours, and then subjected to tempering treatment after cooling to obtain the RTB rare earth permanent magnet.

8. A method for preparing an edge-strengthened high coercivity RTB rare earth permanent magnet as claimed in any one of claims 1 to 6, characterized in that The method comprises the following steps: (1) An H1 diffusion source coating area and an H2 diffusion source coating area are set on the diffusion surface of the RTB magnet substrate, and the diffusion sources are coated in different areas. The H1 diffusion source coating area is coated with the diffusion source H1, and the H2 diffusion source coating area is coated with the diffusion source H2; the H1 diffusion source coating area is the corner area of ​​the diffusion surface, and the H2 diffusion source coating area is the non-corner area of ​​the diffusion surface; The corner area refers to the surface area within the range of 0~Kmm width from the edge line, K is the width of the corner area, and the range of K is 0.2~0.

6. The non-corner area refers to the surface area outside the range of Kmm width from the edge line; The RTB magnet matrix contains more than 0.1wt% Ga; The diffusion source H1 includes the following components by mass fraction: R1: 50.0~80.0wt.%, R1 includes RL1 and RH1, RH1 is one or more of Dy, Tb, Ho, and accounts for 30.0~70.0wt.% of the mass ratio of H1, and the balance of R1 is RL1, RL1 represents one or more elements selected from Nd, Pr, La, Ce, Er, Gd, Sm, Tm, Lu, Y containing at least light rare earth elements; the light rare earth elements are one or more of La, Ce, Pr, Nd; X1: 10-30wt.%, X1 is one or more of Zr, Ti, and Nb; M1: 5.0~40.0wt.%, M1 is one or more of Al, Ga, and Cu; The diffusion source H2 is one or more mixtures of pure metals, alloys or compounds containing heavy rare earth elements, and the heavy rare earth element is at least one of Dy, Tb and Ho; And the content of heavy rare earth elements in the diffusion source H1 is lower than that in H2; (2) placing the magnet coated with diffusion sources in a hydrogen or hydrogen and nitrogen mixture at 400-600°C for 10-30 minutes; (3) The magnet coated with the diffusion source in step (2) is subjected to diffusion treatment at a diffusion temperature of 800° C. to 1000° C. for a holding time of 6 to 30 hours, and then subjected to tempering treatment after cooling to obtain the RTB rare earth permanent magnet.

9. The method according to claim 8, characterized in that In the step (2), when a mixed gas of hydrogen and nitrogen is used, the volume ratio of hydrogen is not less than 30 vol.%.

10. The method according to claim 8, characterized in that In the step (3), the cooling rate is no more than 500° C. / h.

Citation Information

Cited By

  • Method for testing coercive force of sintered neodymium-iron-boron selective diffusion magnet and application

    CN122631748A

  • Method for testing coercivity of sintered neodymium-iron-boron selected area diffusion magnet and application

    CN122631748B