Epitaxial growth method for reducing background doping of semiconductor material

By performing high-temperature degassing operations on the substrate support and source furnace, combining the substrate pretreatment and oxide layer removal, the cleaning process is optimized, and the background doping problem of semiconductor materials is solved and the material purity and performance are improved.

CN119028813APending Publication Date: 2024-11-26INST OF SEMICONDUCTORS - CHINESE ACAD OF SCI
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411191385.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-28
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

During the epitaxial growth of semiconductor materials, background doping problems lead to the impact of material purity and performance, and the prior art is difficult to effectively reduce background doping, especially when preparing extremely high purity materials, impurities are still a key issue.

Method used

By performing high-temperature degassing operation on the substrate stent in the growth chamber, replacing the high-temperature resistant sheet, adjusting the vacuum degree of the growth chamber, and performing high-temperature degassing operation on the source furnace, combining the pretreatment of the substrate and the removal of the oxide layer, optimize cleaning Process to reduce impurities entering.

Benefits of technology

It effectively reduces undesired impurities entering the epitaxial layer, improves the purity and performance of semiconductor materials, and significantly improves device efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119028813A_ABST
    Figure CN119028813A_ABST
Patent Text Reader

Abstract

The invention provides an epitaxial growth method for reducing background doping of a semiconductor material, which is applied to the technical field of semiconductor manufacturing and comprises the following steps: putting a pretreated substrate support into a growth cavity, and performing high-temperature degassing operation on the substrate support based on the growth cavity; wherein a high-temperature-resistant sheet is arranged on the substrate support; replacing the high-temperature-resistant sheet on the substrate support with a substrate; adjusting the vacuum degree of the growth cavity to enable the growth cavity to meet the target state; carrying out high-temperature degassing operation on the source furnace; executing a second operation on the substrate to obtain a target substrate; wherein the second operation is used for removing an oxide layer on the surface of the substrate; and growing an epitaxial layer on the target substrate. According to the epitaxial growth method for reducing the background doping of the semiconductor material, the operation condition of the source furnace is optimized, and a novel cleaning process is introduced, so that unexpected impurities entering the epitaxial layer are effectively reduced, and the purity and the performance of the semiconductor material are improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present disclosure relates to the field of semiconductor manufacturing technology, and more specifically, to an epitaxial growth method for reducing background doping of semiconductor materials. Background Art

[0002] Molecular beam epitaxy (MBE) is a high-precision thin film growth technology that is widely used in the manufacture of high-quality semiconductor materials. However, during the epitaxial growth process, background doping problems may affect the purity and performance of the epitaxial layer, thereby affecting the performance of the final device. In addition to selecting suitable growth conditions and performing appropriate heat treatment on the substrate, it is also very important to reduce the impurities brought by the equipment itself. Impurities in the equipment itself include impurities in the source material and crucible, and uncontrolled volatilization of impurities in the equipment's internal components at high temperatures.

[0003] At present, in order to reduce background doping, methods such as high-purity source materials and enhanced source furnace cleaning are usually used. However, in the preparation process of certain semiconductor materials that require extremely high purity, background doping is still a key issue. How to further reduce the background concentration of epitaxial materials can effectively reduce the dark current of some semiconductor materials and improve their device efficiency, which is an urgent problem to be solved. Summary of the invention

[0004] 1. Technical issues to be resolved

[0005] The present disclosure provides an epitaxial growth method for reducing background doping of semiconductor materials, which is used to at least partially solve one of the above-mentioned technical problems.

[0006] (II) Technical solution

[0007] The present invention provides an epitaxial growth method for reducing background doping of semiconductor materials, the method comprising: placing a pre-treated substrate holder into a growth chamber, and performing a high-temperature degassing operation on the substrate holder based on the growth chamber; wherein a high-temperature resistant thin sheet is mounted on the substrate holder; replacing the high-temperature resistant thin sheet on the substrate holder with a substrate; adjusting the vacuum degree of the growth chamber so that the growth chamber meets a target state; performing a high-temperature degassing operation on a source furnace; performing a second operation on the substrate to obtain a target substrate; wherein the second operation is used to remove an oxide layer on the surface of the substrate; and growing an epitaxial layer on the target substrate.

[0008] According to an embodiment of the present disclosure, a high-temperature degassing operation is performed on a substrate holder based on a growth chamber, including: placing the substrate holder on a growth chamber heater, and performing a high-temperature degassing operation on the substrate holder based on the growth chamber heater; monitoring the degassing of the substrate holder, and stopping heating when the degassing condition meets preset conditions; wherein the temperature of the high-temperature degassing operation is 50~150℃ higher than the maximum growth temperature.

[0009] According to an embodiment of the present disclosure, when a high-temperature degassing operation is performed on a substrate holder, a high-temperature resistant sheet is shielded at a through hole of a growth chamber.

[0010] According to an embodiment of the present disclosure, replacing the high temperature resistant thin sheet on the substrate holder with the substrate includes: taking out the substrate holder after cooling down and replacing the high temperature resistant thin sheet on the substrate holder with the substrate under a specified environment; performing low temperature baking and medium temperature baking operations on the replaced substrate and substrate holder to obtain a pre-treated substrate.

[0011] According to an embodiment of the present disclosure, the vacuum degree of the growth chamber is adjusted so that the growth chamber meets the target state, including: performing a vacuum operation on the growth chamber based on a titanium sublimation pump to obtain a growth chamber that meets the target state; wherein the target state is that the vacuum degree of the growth chamber is lower than 5E-9 Torr in a non-growth state.

[0012] According to an embodiment of the present disclosure, a high-temperature degassing operation is performed on a source furnace, including: performing a high-temperature degassing operation on the source furnace based on a specified temperature; wherein the specified temperature is determined based on a maximum operating temperature; and when a first condition is met, the degassing operation is terminated; wherein the first condition includes that the degassing time meets a preset time length or the vacuum degree change meets a preset condition.

[0013] According to an embodiment of the present disclosure, the method also includes pre-processing the substrate holder: performing a low-temperature degassing operation and a medium-temperature degassing operation on the substrate holder in sequence; wherein the low-temperature degassing operation is performed in the injection chamber, and the medium-temperature degassing operation is performed in the pretreatment chamber, the temperature of the low-temperature degassing is 150~200°C, and the temperature of the medium-temperature degassing is 400~500°C.

[0014] According to an embodiment of the present disclosure, a second operation is performed on a substrate to obtain a target substrate, including: placing a pretreated substrate into a growth chamber in a target state; preliminarily removing an oxide layer of the substrate based on a first temperature and a first gas pressure; after preliminarily removing the oxide layer of the substrate, secondarily removing the oxide layer of the substrate based on a second temperature and a second gas pressure to obtain the target substrate; wherein the first temperature is greater than the second temperature, and the first gas pressure is greater than the second gas pressure.

[0015] According to an embodiment of the present disclosure, the material of the high temperature resistant sheet is molybdenum or silicon.

[0016] According to an embodiment of the present disclosure, a baffle is arranged between the substrate and the source furnace, and the baffle is opened and closed during the epitaxial growth process and the degassing process; when the baffle is opened, the baffle is heated by a baffle heating device; wherein the temperature of the baffle heating device is lower than the temperature of the source furnace mouth, and a heat shielding device is arranged between the heating device and the source furnace mouth.

[0017] (III) Beneficial effects

[0018] The epitaxial growth method for reducing background doping of semiconductor materials provided by the present invention includes at least the following beneficial effects:

[0019] By optimizing the operating conditions of the source furnace and introducing a new cleaning process, the entry of unwanted impurities into the epitaxial layer can be effectively reduced, thereby improving the purity and performance of semiconductor materials. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] The above and other objects, features and advantages of the present disclosure will become more apparent through the following description of the embodiments of the present disclosure with reference to the accompanying drawings, in which:

[0021] Figure 1 A flow chart of an epitaxial growth method for reducing background doping of semiconductor materials according to an embodiment of the present invention is schematically shown;

[0022] Figure 2 A schematic diagram showing a principle diagram of an epitaxial growth method for reducing background doping of semiconductor materials according to another embodiment of the present invention;

[0023] Figure 3 The principle diagram of an epitaxial growth method for reducing background doping of semiconductor materials according to another embodiment of the present invention is schematically shown. DETAILED DESCRIPTION

[0024] In order to make the purpose, technical scheme and advantages of the present invention more clearly understood, the present invention is further described in detail below in combination with specific embodiments and with reference to the accompanying drawings. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0025] The terms used herein are only for describing specific embodiments and are not intended to limit the present invention. The terms "comprise", "include", etc. used herein indicate the existence of the features, steps, operations and / or components, but do not exclude the existence or addition of one or more other features, steps, operations or components.

[0026] In the present invention, unless otherwise clearly specified and limited, the terms "installed", "connected", "connected", "fixed" and the like should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection, an electrical connection, or can communicate with each other; it can be a direct connection, or an indirect connection through an intermediate medium, it can be the internal connection of two elements or the interaction relationship between two elements. For ordinary technicians in this field, the specific meanings of the above terms in the present invention can be understood according to specific circumstances.

[0027] In the description of the present invention, it should be understood that the terms "longitudinal", "length", "circumferential", "front", "rear", "left", "right", "top", "bottom", "inside", "outside", etc., indicating the orientation or positional relationship are based on the orientation or positional relationship shown in the accompanying drawings, and are only for the convenience of describing the present invention and simplifying the description, rather than indicating or implying that the subsystem or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as a limitation on the present invention.

[0028] Throughout the drawings, the same elements are represented by the same or similar reference numerals. Conventional structures or configurations will be omitted when they may cause confusion in the understanding of the present invention. The shapes, sizes, and positional relationships of the components in the drawings do not reflect the actual size, proportion, and actual positional relationship. In addition, in the claims, any reference symbol between brackets shall not be construed as a limitation to the claims.

[0029] Similarly, in order to simplify the present invention and help understand one or more of the various disclosed aspects, in the above description of exemplary embodiments of the present invention, the various features of the present invention are sometimes grouped together into a single embodiment, figure, or description thereof. The description with reference to the terms "one embodiment", "some embodiments", "example", "specific example", or "some examples" etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described may be combined in any one or more embodiments or examples in a suitable manner.

[0030] In addition, the terms "first" and "second" are used for descriptive purposes only and should not be understood as indicating or implying relative importance or implicitly indicating the number of the indicated technical features. Therefore, the features defined as "first" and "second" may explicitly or implicitly include one or more of the features. In the description of the present invention, the meaning of "plurality" is at least two, such as two, three, etc., unless otherwise clearly and specifically defined.

[0031] Figure 1 The flowchart of the epitaxial growth method for reducing background doping of semiconductor materials according to an embodiment of the present invention is schematically shown.

[0032] like Figure 1 As shown, an epitaxial growth method for reducing background doping of semiconductor materials provided by an embodiment of the present disclosure includes operations S110 to S160.

[0033] In operation S110, the pre-treated substrate holder is placed in a growth chamber, and a high-temperature degassing operation is performed on the substrate holder based on the growth chamber; wherein a high-temperature resistant sheet is mounted on the substrate holder.

[0034] In some embodiments, pre-treating the substrate holder includes: sequentially performing a low-temperature degassing operation and a medium-temperature degassing operation on the substrate holder; wherein the low-temperature degassing operation is performed at 150-200°C, and the medium-temperature degassing operation is performed at 400-500°C. By performing the low-temperature degassing and the medium-temperature degassing, the impurity content brought into the growth chamber by the substrate holder can be effectively reduced, which is beneficial to maintaining the vacuum degree of the growth chamber. After the low-temperature degassing and the medium-temperature degassing operations are completed, the substrate holder after cooling is introduced into the growth chamber, and a high-temperature degassing operation is performed on the substrate holder in the growth chamber.

[0035] Specifically, when the substrate holder is not in use, it is kept in a low temperature state for a long time or even exposed to the atmosphere, which is easy to absorb impurities. When the growth temperature rises to a higher growth temperature, the substrate holder may release impurities, resulting in the occurrence of background doping. Therefore, before performing a high-temperature degassing operation on the substrate holder, a high-temperature resistant shielding sheet can be used to shield the through hole of the growth chamber. The high-temperature resistant shielding sheet can be a molybdenum sheet. For a material system with a growth temperature of 600~700℃ or lower, the high-temperature resistant shielding sheet can also be a silicon sheet.

[0036] In some embodiments, a high-temperature degassing operation is performed on a substrate holder based on a growth chamber, including: placing the substrate holder on a growth chamber heater, controlling the growth chamber heater to perform high-temperature degassing on the substrate holder based on a specified temperature; monitoring the degassing of the substrate holder, and stopping heating when the degassing condition meets a preset condition. The preset conditions include that the degassing time meets 20min~2h and / or the change in the vacuum gauge reading (i.e., the pressure or vacuum degree in the growth chamber) meets the preset conditions. The specific degassing time can be selected according to actual conditions, and the present disclosure is not limited here, or the heating can be stopped when the vacuum gauge reading changes from a rapid decrease to a slow decrease. The specified temperature of the high-temperature degassing operation is 50~150℃ higher than the maximum growth temperature.

[0037] After the heating is stopped, the cooled substrate holder is transferred to the sample loading chamber. If the substrate holder does not need to be grown immediately, the substrate holder after high temperature degassing is stored in the vacuum chamber and then transferred to the sample loading chamber to be filled before loading.

[0038] In operation S120, the high temperature resistant sheet on the substrate holder is replaced with a substrate.

[0039] In some embodiments, after operation S110 is completed, the high temperature resistant sheet is quickly replaced with the substrate in a sample injection room or a dry and clean glove box, and the substrate is pre-treated.

[0040] To save time and improve efficiency, operation S120 may be performed simultaneously with operation S130.

[0041] In the specific implementation process, the substrate is pretreated including: after the replacement is completed, conventional vacuuming and low-temperature baking degassing operations are performed in the sample chamber. The temperature of the low-temperature baking is 150~200℃, and the time is 0.5~3h. After the low-temperature baking is completed, the substrate holder and the substrate are transferred to the pretreatment chamber, and the medium-temperature baking degassing operation is performed in the pretreatment chamber. The temperature of the medium-temperature baking degassing must be higher than the low-temperature baking temperature by more than 50℃, and the temperature of the medium-temperature baking degassing must be lower than the decomposition temperature of the substrate without atmosphere protection. The time of the medium-temperature baking is 0.5~2h.

[0042] After the medium temperature baking is completed, the substrate holder and the substrate are transferred into the growth chamber to perform subsequent operations S150 to S160 in the growth chamber.

[0043] In operation S130, the vacuum degree of the growth chamber is adjusted so that the growth chamber meets a target state.

[0044] In some embodiments, before growth and during growth intervals, a titanium sublimation pump is used to evacuate the growth chamber to obtain a growth chamber that meets the target state. The target state means that the vacuum degree of the growth chamber can be lower than 5E-9 Torr in the non-growth state. E-9 means 10 -9 Torr is the unit of vacuum degree. Preferably, when the vacuum degree of the growth chamber is lower than 2E-9 Torr, the effect is better.

[0045] Specifically, adjusting the vacuum degree of the growth chamber before growth and during growth intervals helps the growth chamber to be in a good ultra-high vacuum state.

[0046] In operation S140, a high-temperature degassing operation is performed on the source furnace.

[0047] In some embodiments, the temperature of the source furnace required for growth can be increased to perform a high-temperature degassing operation. The high-temperature degassing operation can remove impurities adsorbed on the source material, crucible, and baffle, thereby effectively reducing the possibility of the source material, crucible, and baffle releasing impurities during the epitaxial process.

[0048] Specifically, the source furnace is degassed based on the specified temperature, wherein the specified temperature is determined based on the maximum use temperature and is usually 5-30°C higher than the maximum use temperature. When the degassing time meets the preset time, or the vacuum degree change meets the preset conditions (i.e., the vacuum degree decreases significantly slower under the same baffle switch conditions), the degassing is terminated. After the degassing is completed, the source furnace is cooled down to the temperature used for this growth, and is ready for growth.

[0049] During the degassing process, the baffle will be opened and closed periodically, such as opening for 1 to 5 minutes and then closing for 1 to 5 minutes, so as to degas the baffle and the source furnace more effectively.

[0050] If there are multiple source furnaces, these source furnaces can be degassed at the same time. If the source furnace is a dual-temperature zone source furnace, both temperature zones of the dual-temperature zone source furnace must be higher than the maximum operating temperature, and the temperature of the high temperature zone must always be higher than the temperature of the low temperature zone. If the source furnace is a gas source furnace, only the source furnace mouth needs to be degassed.

[0051] In operation S150, a second operation is performed on the substrate to obtain a target substrate.

[0052] In some embodiments, after operation S140 is completed, the substrate is introduced into the growth chamber and a second operation is performed to obtain a target substrate, wherein the second operation is used to remove the oxide layer on the surface of the substrate.

[0053] If the oxide layer on the substrate surface cannot be fully removed, oxygen impurities will be introduced at the interface, diffused to the epitaxial layer in the subsequent growth and become impurities, resulting in an increase in background concentration. Therefore, it is necessary to use high temperature to fully remove the oxide layer on the substrate surface. However, if the high temperature causes the substrate surface to decompose, therefore, the present disclosure proposes to use a higher pressure protective gas to prevent the substrate surface from decomposing while fully removing the oxide layer on the substrate surface.

[0054] In the specific implementation process, the second operation can be divided into a first stage and a second stage. The first stage refers to: preliminarily removing the substrate oxide layer based on the first temperature and the first gas pressure. The second node refers to, after the preliminary removal of the substrate oxide layer, the substrate oxide layer is secondary removed based on the second temperature and the second gas pressure to obtain the target substrate. Among them, the first temperature is greater than the second temperature, the first gas pressure is greater than the second gas pressure, the second temperature is the conventional oxide layer removal temperature, and the second gas pressure is the conventional protective gas pressure. Among them, the conventional oxide layer removal temperature and conventional protective gas pressure corresponding to different substrates are different, and those skilled in the art can choose according to actual conditions, and the present disclosure is not limited here.

[0055] Specifically, the first stage is performed 2 minutes before the second operation, the first temperature is 10-20°C higher than the conventional oxide layer removal temperature, the first gas pressure is 20-50% higher than the conventional protective gas pressure, and the oxide layer is initially removed based on the first temperature and the first gas pressure. When the temperature drops to the conventional oxide layer removal temperature and the protective gas pressure drops to the conventional protective gas pressure, the oxide layer removal of the second stage is performed, wherein the oxide layer is removed using a protective gas at the conventional oxide layer removal temperature (i.e., the second temperature) and the conventional pressure (i.e., the second gas pressure), and the duration is 3-10 minutes.

[0056] By sequentially performing the oxide layer removal in the first stage and the second stage, the substrate surface can be thoroughly cleaned while protecting the substrate surface from being decomposed and damaged.

[0057] In operation S160 , an epitaxial layer is grown on a target substrate.

[0058] In some embodiments, an epitaxial layer is grown on the surface of a target substrate. During the growth of the epitaxial layer, a baffle of the source furnace may have a corresponding on / off state to accurately control the epitaxial growth. When the baffle of the source furnace is opened, a heating device located below the baffle heats the baffle.

[0059] In the embodiment of the present disclosure, a baffle heating device is provided below the source furnace baffle to heat the baffle when the baffle is opened to prevent the temperature of the baffle from dropping rapidly.

[0060] When the baffle is open, the temperature of the baffle drops rapidly, which makes it easy to absorb impurities. When the baffle is closed, the source furnace port will quickly heat the baffle, and the impurities adsorbed on the baffle may be released, affecting the cleanliness of the source furnace area and causing the problem of increased background doping.

[0061] To improve this situation, the present disclosure proposes to set a heating device at the baffle opening position to maintain the baffle temperature when the baffle is open, to prevent the baffle from absorbing impurities due to too low a temperature when in the open state, and to prevent the baffle state change from affecting the cleanliness of the source furnace area.

[0062] Specifically, the temperature of the baffle heating device can be slightly lower than the temperature of the source furnace port to prevent the impurities there from evaporating and depositing at the source furnace port. The temperature of the baffle heating device changes with the temperature of the source furnace. For example, when a high-temperature degassing operation is performed based on the source furnace before growth, the temperature of the baffle heating device should also be increased accordingly to heat the baffle in the open state and improve the degassing efficiency of the baffle.

[0063] Preferably, the temperature of the baffle heating device should be 20-80° C. lower than the temperature of the source furnace port. When the source furnace is degassing, the difference between the degassing temperature of the baffle heating device and the use temperature is equal to the difference between the degassing temperature of the source furnace port and the use temperature.

[0064] In addition, a heat shielding device may be provided between the baffle heating device and the source furnace port to avoid thermal interference of the baffle heating device on the source furnace port, thereby avoiding influence on the beam uniformity.

[0065] The technical solution of the present disclosure is described in detail below in conjunction with specific embodiments.

[0066] Figure 2 The principle diagram of an epitaxial growth method for reducing background doping of semiconductor materials according to another embodiment of the present invention is schematically shown.

[0067] In this embodiment, the number of substrates is 1.

[0068] A high temperature resistant sheet is placed on the substrate holder, wherein the high temperature resistant sheet is a silicon (Si) sheet. A low temperature degassing operation is performed on the substrate holder in the sample loading chamber, for example, a low temperature baking degassing at 190°C for 1 hour is performed in the sample loading chamber. After the low temperature degassing operation is completed, the cooled substrate holder is transferred to the pretreatment chamber, and a medium temperature removal operation is performed on the substrate holder in the pretreatment chamber, for example, a medium temperature baking degassing at 400-450°C for 45 minutes is performed in the pretreatment chamber.

[0069] After the substrate holder cools down, it is transferred into the growth chamber, and a high-temperature degassing operation is performed on the substrate holder based on the growth chamber: the substrate holder is heated by the growth chamber heater to a state exceeding the expected maximum operating temperature of 70~80°C, and the baking is continued for 20 minutes.

[0070] After cooling down, the substrate holder is transferred to the injection chamber, and the substrate is installed on the substrate holder: the injection chamber is inflated, and a dry and clean glove box is connected to the open position of the injection chamber, and the high-temperature resistant thin sheet on the substrate holder is quickly replaced with the substrate in the glove box. In this embodiment, the high-temperature resistant thin sheet is a Si wafer, and the substrate is a GaAs substrate. After the replacement is completed, the substrate holder is placed back into the injection chamber, and a low-temperature baking and degassing operation is performed after vacuuming, wherein the baking temperature is 190°C and the baking time is 1h. After the low-temperature baking and degassing operation is completed, the substrate holder is sent to the pretreatment chamber for a warm baking and degassing operation, wherein the baking temperature is 400-450°C and the baking time is 45min.

[0071] While installing the substrate, the vacuum degree of the growth chamber is adjusted to increase the vacuum degree of the growth chamber to 1.5E-9 Torr. While increasing the vacuum degree of the growth chamber, the source furnace required for growth can be heated up to prepare for subsequent high-temperature degassing operations.

[0072] After the vacuum degree of the growth chamber is adjusted, the source furnace is subjected to high-temperature degassing: the heated source furnace is the source furnace required for this growth, such as gallium (Ga), aluminum (Al), indium (In), arsenic (As), silicon (Si), beryllium (Be), etc. After the vacuum degree of the growth chamber reaches the target value, the source furnace is subjected to high-temperature degassing. Among them, the high-temperature degassing temperature of the source furnace needs to be 15°C higher than the maximum operating temperature of this time, and the entire degassing process lasts for 15 minutes. During the degassing process, the baffle is periodically opened and closed (open the baffle for 3~5 minutes, close the baffle for 1~2 minutes). When the baffle is open, the open baffle is heated based on the baffle heating device. During the heating process, the temperature of the baffle heating device is always 20~60°C lower than the temperature of the source furnace mouth, for example, it can be 40°C.

[0073] After the high-temperature degassing operation of the source furnace is completed, close the dampers of all source furnaces and cool the source furnaces to the growth temperature.

[0074] The substrate holder that has completed the medium-temperature degassing in the pretreatment chamber is transferred into the growth chamber, and the substrate oxide layer is removed in the growth chamber: the substrate temperature is raised to a temperature 15°C higher than the conventional deoxidation temperature, and the As pressure (arsenic vapor pressure) is ensured to be 130% of the pressure value during conventional deoxidation, and the oxide layer is removed in this state for 2 minutes. Then the substrate temperature is cooled down to the conventional deoxidation temperature, and the As pressure is reduced to the pressure during conventional deoxidation, and the oxide layer is removed for 8 minutes to obtain the target substrate.

[0075] An epitaxial layer is grown on the target substrate. During the growth of the epitaxial layer, when the baffle of the corresponding source furnace is opened, the baffle is heated by a baffle heater located below the baffle, wherein the temperature of the baffle heater is 40° C. lower than the temperature of the source furnace port.

[0076] Figure 3 The principle diagram of an epitaxial growth method for reducing background doping of semiconductor materials according to another embodiment of the present invention is schematically shown.

[0077] In this embodiment, the number of substrates is 2.

[0078] A high temperature resistant sheet is placed on each substrate holder respectively, wherein the high temperature resistant sheet is a molybdenum sheet. Substrate holder A and substrate holder B are pretreated: low temperature baking and degassing operation is performed on substrate holder A and substrate holder B in the injection chamber, for example, low temperature baking and degassing at 180°C for 2 hours is performed in the injection chamber. After the low temperature degassing operation is completed, the cooled substrate holder A and substrate holder B are transferred into the pretreatment chamber, and medium temperature baking and degassing operation is performed on substrate holder A and substrate holder B in the pretreatment chamber, for example, medium temperature baking and degassing at 460~490°C for 1.5 hours is performed in the pretreatment chamber. The pretreatment of substrate holder A and substrate holder B can be performed simultaneously or separately (for example, substrate holder A is pretreated first, and then substrate holder B is pretreated).

[0079] After the substrate holder cools down, substrate holder A and substrate holder B are introduced into the growth chamber in sequence, and a high-temperature degassing operation is performed on the substrate holders based on the growth chamber.

[0080] Specifically, if the pretreatment of substrate holder A and substrate holder B is carried out simultaneously, substrate holder A is introduced into the growth chamber to perform a high-temperature degassing operation, and substrate holder B is stored in a vacuum chamber (such as a sampling chamber after cooling, or a substrate holder bracket set inside the equipment). After the high-temperature degassing of substrate holder A is completed, substrate holder B is introduced into the growth chamber to perform a high-temperature degassing operation.

[0081] If the pretreatment of substrate holder A and substrate holder B is performed separately, substrate holder B can be pretreated before or after the high-temperature degassing of substrate holder A is completed.

[0082] The substrate holder is heated by the growth chamber heater to a temperature 100-120°C higher than the expected maximum use temperature and the baking is continued for 30 minutes. After cooling down, the substrate holder A is transferred to the sample injection chamber, while the substrate holder B is kept in a vacuum state.

[0083] Install the substrate on the substrate holder A in the injection chamber: Inflate the injection chamber, open the injection chamber and connect it to a dry and clean glove box, and quickly replace the molybdenum sheet on the substrate holder with an indium phosphide (InP) substrate in the glove box. After the replacement is completed, put the substrate holder back into the injection chamber, evacuate the vacuum and perform a low-temperature baking and degassing operation, where the baking temperature is 180°C and the baking time is 40 minutes. After the low-temperature baking and degassing operation is completed, send the substrate holder into the pretreatment chamber for a warm baking and degassing operation, where the baking temperature is 300°C and the baking time is 1 hour.

[0084] While the substrate is being installed, the vacuum of the growth chamber is adjusted based on a titanium sublimation pump to increase the vacuum of the growth chamber to 1.5E-9 Torr. While increasing the vacuum of the growth chamber, the temperature of the source furnace for the desired growth can be increased to prepare for subsequent high-temperature degassing operations.

[0085] The source furnace that is heated is the source furnace required for this growth, for example, gallium (Ga), aluminum (Al), indium (In), arsenic (As), silicon (Si), beryllium (Be), etc. After the vacuum degree of the growth chamber reaches the target value, the source furnace is subjected to high-temperature degassing operation. Among them, the high-temperature degassing temperature of the source furnace needs to be 10°C higher than the maximum operating temperature of this time, and the baffle heating device needs to be heated to 30°C lower than the temperature of the source furnace mouth. The entire degassing process lasts for 10 minutes. During the degassing process, the baffle is periodically opened and closed (open the baffle for 2~3 minutes, close the baffle for 1 minute). When the baffle is open, the open baffle is heated based on the baffle heating device. During the heating process, the temperature of the baffle heating device is always 15~50°C lower than the temperature of the source furnace mouth.

[0086] After the high-temperature degassing operation of the source furnace is completed, close the dampers of all source furnaces and cool the source furnaces to the growth temperature.

[0087] After the medium-temperature degassing in the pretreatment chamber, the substrate holder A is introduced into the growth chamber, and the substrate temperature is raised to a temperature 10°C higher than the conventional deoxidation temperature, while ensuring that the As pressure (arsenic vapor pressure) is 140% of the pressure value during the conventional deoxidation. The deoxidation is carried out for 2 minutes under this state. Then the substrate temperature is cooled down to the conventional deoxidation temperature, and the As pressure is reduced to the pressure during the conventional deoxidation, and the deoxidation is continued for 8 minutes to obtain the target substrate A.

[0088] An epitaxial layer is grown on the target substrate A. During the growth of the epitaxial layer, when the baffle of the corresponding source furnace is opened, the baffle is heated by a baffle heater located below the baffle, wherein the temperature of the baffle heater is 30° C. lower than the temperature of the source furnace port.

[0089] Before the epitaxial layer growth on substrate holder A is completed, the substrate is installed on substrate holder B based on the same process as substrate holder A, and after the substrate installation is completed, low-temperature baking degassing and medium-temperature baking degassing operations are performed on substrate holder B.

[0090] After the substrate holder A is grown and transferred out of the growth chamber, all source furnace baffles in the growth chamber are closed, and the vacuum degree of the growth chamber is adjusted to below 1.5E-9 Torr using the titanium sublimation pump again.

[0091] After the substrate holder B is baked and degassed at medium temperature and the vacuum degree of the growth chamber is adjusted, the substrate holder B is introduced into the growth chamber and the oxide layer is removed to obtain the target substrate B. The specific process of removing the oxide layer is similar to that of removing the oxide layer of the substrate holder A, and will not be described in detail here.

[0092] An epitaxial layer is grown on the target substrate B. The specific growth process is similar to the process of growing the epitaxial layer on the target substrate A, and will not be described in detail here.

[0093] The embodiments of the present invention are described above. However, these embodiments are only for the purpose of illustration, and are not intended to limit the scope of the present invention. Although each embodiment is described above, it does not mean that the measures in each embodiment cannot be used in combination advantageously. Without departing from the scope of the present invention, those skilled in the art may make various substitutions and modifications, which should all be included in the protection scope of the present invention.

Claims

1. An epitaxial growth method for reducing background doping of semiconductor materials, characterized in that: The method comprises: placing the pre-treated substrate holder into a growth chamber, and performing a high-temperature degassing operation on the substrate holder based on the growth chamber; wherein a high-temperature resistant sheet is mounted on the substrate holder; Replacing the high temperature resistant sheet on the substrate holder with a substrate; Adjusting the vacuum degree of the growth chamber so that the growth chamber meets the target state; Perform high-temperature degassing operation on the source furnace; Performing a second operation on the substrate to obtain a target substrate; wherein the second operation is used to remove an oxide layer on the surface of the substrate; An epitaxial layer is grown on the target substrate.

2. The epitaxial growth method according to claim 1, characterized in that: The step of performing a high-temperature degassing operation on the substrate holder based on the growth chamber comprises: placing the substrate holder on a growth chamber heater, and performing a high-temperature degassing operation on the substrate holder based on the growth chamber heater; Monitoring the degassing of the substrate holder, and stopping heating when the degassing meets a preset condition; Wherein, the temperature of the high-temperature degassing operation is 50-150° C. higher than the maximum growth temperature.

3. The epitaxial growth method according to claim 2, characterized in that: When a high-temperature degassing operation is performed on the substrate holder, a high-temperature resistant sheet is shielded at the through hole of the growth chamber.

4. The epitaxial growth method according to claim 1, characterized in that: The step of replacing the high temperature resistant sheet on the substrate holder with a substrate comprises: After the temperature drops, take out the substrate holder and replace the high temperature resistant sheet on the substrate holder with a substrate under a specified environment; The replaced substrate and substrate holder are subjected to low-temperature baking and high-temperature baking operations to obtain a pre-processed substrate.

5. The epitaxial growth method according to claim 1, characterized in that: The step of adjusting the vacuum degree of the growth chamber so that the growth chamber meets a target state includes: Performing a vacuum operation on the growth chamber based on a titanium sublimation pump to obtain a growth chamber that meets a target state; The target state is that the vacuum degree of the growth chamber is lower than 5E-9 Torr in a non-growth state.

6. The epitaxial growth method according to claim 1, characterized in that: The high-temperature degassing operation on the source furnace comprises: performing a high-temperature degassing operation on the source furnace based on a specified temperature; wherein the specified temperature is determined based on a maximum use temperature; When a first condition is met, the degassing operation is terminated; wherein the first condition includes that the degassing time meets a preset time or the vacuum degree change meets a preset condition.

7. The epitaxial growth method according to claim 1, characterized in that: The method further comprises pre-processing the substrate holder: performing a low-temperature degassing operation and a medium-temperature degassing operation on the substrate holder in sequence; Among them, the low-temperature degassing operation is performed in the injection chamber, and the medium-temperature degassing operation is performed in the pretreatment chamber. The temperature of the low-temperature degassing is 150~200℃, and the temperature of the medium-temperature degassing is 400~500℃.

8. The epitaxial growth method according to claim 1, characterized in that: The performing a second operation on the substrate to obtain a target substrate includes: placing the pre-treated substrate into a growth chamber in a target state; Preliminarily removing the substrate oxide layer based on the first temperature and the first gas pressure; After initially removing the substrate oxide layer, secondarily removing the substrate oxide layer based on a second temperature and a second gas pressure to obtain a target substrate; The first temperature is greater than the second temperature, and the first air pressure is greater than the second air pressure.

9. The epitaxial growth method according to claim 3, characterized in that: The material of the high temperature resistant sheet is molybdenum or silicon.

10. The epitaxial growth method according to claim 1, characterized in that: A baffle is provided between the substrate and the source furnace, and the baffle is opened and closed during the epitaxial growth process and the degassing process; When the baffle is opened, heating the baffle based on the baffle heating device; Wherein, the temperature of the baffle heating device is lower than the temperature of the source furnace mouth, and a heat shielding device is arranged between the heating device and the source furnace mouth.