Preparation method of rod coating printing wafer level FET (Field Effect Transistor)
By employing a rod-coating method for fabricating wafer-level FETs, and utilizing electrochemical-assisted liquid-phase stripping and rod coating, the Fermi pinning effect and solution waste problems of two-dimensional semiconductor FETs are solved. This improves the electrical performance of the FETs and reduces the operational difficulty, providing feasibility for industrial production.
Patent Information
- Application Number
- CN202411151064.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-21
- Publication Date
- 2024-11-26
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
In existing technologies, two-dimensional semiconductor FETs suffer from the Fermi pinning effect, which leads to low performance. At the same time, liquid-phase electrochemical-assisted stripping methods result in significant solution waste during spin coating.
A rod-coating wafer-level FET fabrication method was adopted, in which a two-dimensional semiconductor solution was prepared by electrochemical-assisted liquid phase exfoliation, and then the two-dimensional semiconductor was coated on SiO2/Si wafer by rod coating. Subsequently, calcination, photolithography, etching and MXene nanosheets were prepared to form a highly conductive electrode to achieve quasi-ohmic contact.
This reduces operational complexity, improves the electrical performance of FET transistors, achieves cost savings while enhancing FET performance, and provides feasibility for industrial production.
Smart Images

Figure CN119028827A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a method for preparing a wafer-level FET. Background Art
[0002] Silicon-based transistor technology is approaching its limit at nodes below 10nm. Further expansion of field effect transistors (FETs) requires new channel materials. Two-dimensional semiconductors have the advantages of atomic layer thickness and high carrier mobility and are widely studied. However, the high contact resistance caused by the Fermi level pinning effect introduced by the non-ideal interface of traditional metal physical vapor deposition makes two-dimensional semiconductor FETs show low performance. Two-dimensional MXene has good conductivity and can form van der Waals contact with two-dimensional semiconductors, thereby eliminating the Fermi pinning effect. In addition, the commonly used methods for synthesizing two-dimensional semiconductor materials are MOCVD (high temperature and high pressure are required, and the transfer process causes damage and doping), mechanical stripping (cannot effectively control the channel thickness and cannot be prepared on a large area), and liquid-phase electrochemical assisted stripping. Among them, liquid-phase electrochemical assisted synthesis of two-dimensional semiconductor materials has good substrate compatibility. Usually, the two-dimensional semiconductor stripped by liquid-phase electrochemical assisted stripping is assembled into a thin film by spin coating. Most of the solution is thrown out during the spin coating process, which causes a lot of waste. Summary of the invention
[0003] The present invention aims to solve the technical problems that the Fermi pinning effect causes low performance of two-dimensional semiconductor FET and a large amount of solution is wasted in the spin coating method, and provides a method for preparing wafer-level FET by rod coating printing.
[0004] The preparation method of the rod-coated printed wafer-level FET of the present invention is carried out according to the following steps:
[0005] First, prepare the two-dimensional semiconductor by electrochemically assisted liquid phase exfoliation, and then disperse it in DMF to obtain a two-dimensional semiconductor solution;
[0006] 2. Perform hydrophilic treatment on SiO2 / Si wafer;
[0007] 3. Using a rod coating method, the two-dimensional semiconductor solution of step 1 is evenly coated on the SiO2 / Si wafer hydrophilized in step 2;
[0008] 4. calcining the product of step 3 to remove organic matter on the surface of the two-dimensional semiconductor;
[0009] 5. using a photolithography machine to pattern a two-dimensional semiconductor channel on the product of step 4;
[0010] 6. Etching a two-dimensional semiconductor channel;
[0011] 7. Soak the two-dimensional semiconductor channel in acetone to remove the photoresist on the surface;
[0012] 8. Prepare highly conductive MXene nanosheets by liquid phase exfoliation, wash them multiple times to make them electrically neutral, and then disperse the MXene nanosheets in deionized water to obtain a MXene nanosheet solution;
[0013] 9. Photolithography patterning the shape of the electrode on the product after removing the photoresist in step 7;
[0014] 10. uniformly coating the MXene nanosheet solution obtained in step 8 on the electrode surface patterned in step 9;
[0015] 11. Soak the product of step 10 in acetone to remove the photoresist and obtain FET.
[0016] The present invention adopts a rod coating method, uses a two-dimensional semiconductor with electrochemical assisted liquid phase exfoliation as an n-type channel material, and uses a highly conductive MXene as an electrode to reduce the Schottky barrier between the electrode material and the channel material, thereby achieving quasi-ohmic contact and presenting better transistor characteristics.
[0017] The present invention uses a rod coating method to prepare a FET channel, which achieves savings (spin coating a 1cm×1cm MoSe2 film requires approximately 100μL of MoSe2 solution, while the present invention uses a rod coating method, 12μL of MoSe2 solution can coat a 1cm×4cm film) and reduces the difficulty of operation, can improve the electrical performance of FET transistors, and provides feasibility for industrial production. BRIEF DESCRIPTION OF THE DRAWINGS
[0018] Figure 1 An optical micrograph of a FET with a MoSe2 channel MXene electrode prepared in the first embodiment;
[0019] Figure 2 This is the Id-Vg characteristic curve of the FET with MoSe2 channel MXene electrode in the final product of experiment one. DETAILED DESCRIPTION
[0020] Specific implementation method 1: This implementation method is a method for preparing a wafer-level FET by rod coating printing, which is specifically carried out according to the following steps:
[0021] First, prepare the two-dimensional semiconductor by electrochemically assisted liquid phase exfoliation, and then disperse it in DMF to obtain a two-dimensional semiconductor solution;
[0022] 2. Perform hydrophilic treatment on SiO2 / Si wafer;
[0023] 3. Using a rod coating method, the two-dimensional semiconductor solution of step 1 is evenly coated on the SiO2 / Si wafer hydrophilized in step 2;
[0024] 4. calcining the product of step 3 to remove organic matter on the surface of the two-dimensional semiconductor;
[0025] 5. using a photolithography machine to pattern a two-dimensional semiconductor channel on the product of step 4;
[0026] 6. Etching a two-dimensional semiconductor channel;
[0027] 7. Soak the two-dimensional semiconductor channel in acetone to remove the photoresist on the surface;
[0028] 8. Prepare highly conductive MXene nanosheets by liquid phase exfoliation, wash them multiple times to make them electrically neutral, and then disperse the MXene nanosheets in deionized water to obtain a MXene nanosheet solution;
[0029] 9. Photolithography patterning the shape of the electrode on the product after removing the photoresist in step 7;
[0030] 10. uniformly coating the MXene nanosheet solution obtained in step 8 on the electrode surface patterned in step 9;
[0031] 11. Soak the product of step 10 in acetone to remove the photoresist and obtain FET. The structural diagram is shown in Figure 1 As shown, the two symmetrical No. 1 are MXene electrodes and No. 2 is the MoSe2 channel.
[0032] Specific implementation method 2: This implementation method is different from specific implementation method 1 in that: the material of the two-dimensional semiconductor described in step 1 is MoSe2, In2Se3 or MoS2; the method for limiting the concentration of the two-dimensional semiconductor solution described in step 1 is: take 10 μL of the two-dimensional semiconductor solution and dissolve it in 5 mL of DMF, and test its absorbance at 475 nm to be 0.5. Others are the same as specific implementation method 1.
[0033] Specific embodiment three: This embodiment is different from specific embodiment one or two in that: the method for preparing a two-dimensional semiconductor by electrochemically assisted liquid phase exfoliation in step one is: weigh 0.15g of tetraheptyl ammonium bromide and 0.6g of polyvinyl pyrrolidone and dissolve them in DMF, use a carbon rod as the positive electrode and a two-dimensional semiconductor raw material as the negative electrode, apply a 5V to 10V voltage to intercalate for 1h; weigh 0.4g of PVP and dissolve it in 20mL of DMF, add the intercalated two-dimensional semiconductor and ultrasonicate for 5min, then centrifuge at 3000rpm for 5min, then take the upper layer solution and centrifuge at 10000rpm for 10min, and the obtained solid part is the two-dimensional semiconductor. The rest is the same as specific embodiment one or two.
[0034] Specific embodiment 4: This embodiment is different from specific embodiments 1 to 3 in that: the method for hydrophilizing the SiO2 / Si wafer in step 2 is: immersing the SiO2 / Si wafer in piranha solution for 30 minutes to obtain a hydrophilized surface; or using plasma to hydrophilize the SiO2 / Si surface for 5 minutes at a power of 100 W. Others are the same as specific embodiments 1 to 3.
[0035] Specific embodiment 5: This embodiment is different from specific embodiment 4 in that the rod coating in step 3 is completed by using a Meyer rod. The rest is the same as specific embodiment 4.
[0036] Specific embodiment 6: This embodiment is different from specific embodiment 1 in that the calcination temperature in step 4 is 300°C and the time is 1h to 2h, and the SiO2 / Si sheet is carried during calcination. The rest is the same as specific embodiment 1.
[0037] Specific implementation example 7: This implementation example is different from specific implementation example 1 in that the photolithography step in step 5 includes spin coating of photoresist, exposure and development. The rest is the same as specific implementation example 1.
[0038] Specific embodiment 8: This embodiment differs from specific embodiment 1 in that the etching in step 6 is performed by using an ICP dry etcher and CF4 or SF6 gas. The rest is the same as specific embodiment 1.
[0039] Specific embodiment 9: This embodiment is different from specific embodiment 1 in that: in step 8, highly conductive MXene nanosheets are prepared by liquid phase exfoliation, washed multiple times to make them electrically neutral, and then the MXene nanosheets are dispersed in deionized water to obtain a MXene nanosheet solution. The specific process is:
[0040] Weigh 1.6g of lithium fluoride and add it to 20mL of 36% hydrochloric acid, stir in a water bath at 40℃ for 15min, slowly add 1g of MXene powder, react for 10h, centrifuge at 8000rpm for 5min, add 50mL of deionized water, shake at 140rpm for 1d with a shaker, centrifuge at 3000rpm for 5min, take the upper layer solution and centrifuge at 10000rpm for 10min, wash the precipitate several times to make it electrically neutral, and test the electrical neutrality with pH test paper; then disperse the precipitate in deionized water to obtain a MXene nanosheet solution with a concentration of 3-5mg / mL. The rest is the same as the first embodiment.
[0041] Specific embodiment 10: This embodiment is different from specific embodiment 1 in that the photolithography step in step 9 includes spin coating of photoresist, exposure and development. The rest is the same as specific embodiment 1.
[0042] The present invention is verified by the following tests:
[0043] Experiment 1: For the preparation of logic gate devices, two methods, local back gate and top gate, are used. At the same time, in order to reduce the resistance of the device, it is ensured that there is van der Waals contact between the channel material and the electrode. Experiment 1 first introduces the local back gate method.
[0044] 1) Weigh 1.6 g of lithium fluoride and add it to 20 mL of 36% hydrochloric acid, stir in a water bath at 40 ° C for 15 min, slowly add 1 g of MXene powder, react for 10 h, centrifuge at 8000 rpm for 5 min, then add 50 mL of deionized water, shake at 140 rpm for 1 day with a shaker, centrifuge at 3000 rpm for 5 min, take the upper layer solution and centrifuge at 10000 rpm for 10 min, wash the precipitate several times to make it electrically neutral, and test the electrical neutrality with pH test paper; then disperse the precipitate in deionized water to obtain a MXene nanosheet solution with a concentration of 3 mg / mL;
[0045] 2) The surface of the SiO2 / Si wafer with a thickness of 285 nm was hydrophilized by plasma treatment at a power of 100 W for 5 min;
[0046] 3) Spin-coating photoresist on SiO2 / Si after hydrophilization treatment in step 2, exposing and developing to obtain an electrode pattern (gate electrode);
[0047] 4) Coating the SiO2 / Si surface patterned in step 3 with 50 nm thick MXene (obtained in step 1) by rod coating (Meyer rod);
[0048] 5) Soak in acetone for 3 min to remove the photoresist on the surface of the MXene electrode;
[0049] 6) Depositing a 30 nm dielectric layer of Al2O3 on the surface of MXene by ALD;
[0050] 7) Prepare MoSe2 two-dimensional semiconductor solution by electrochemical assisted liquid phase exfoliation, the specific process is: weigh 0.15g of tetraheptylammonium bromide (THAB) and 0.6g of polyvinylpyrrolidone (PVP) and dissolve them in DMF, use carbon rod as positive electrode and MoSe2 as negative electrode, apply 10V voltage for intercalation for 1h; weigh 0.4g of PVP and dissolve it in 20mL of DMF, add the intercalated MoSe2 and ultrasonicate for 5min, then centrifuge at 3000rpm for 5min, then take the upper layer solution and centrifuge at 10000rpm for 10min, the solid part is MoSe2, then disperse it in DMF to obtain MoSe2 solution; take 10μL of MoSe2 solution and dissolve it in 5mL of DMF, test its absorbance at 475nm to be 0.5;
[0051] 8) rod coating MoSe2 two-dimensional semiconductor on SiO2-MXene-Al2O3 surface by rod coating (Meyer rod);
[0052] 9) Calcination to remove organic matter on the surface of the two-dimensional semiconductor, the calcination temperature is 300℃, the time is 1h;
[0053] 10) Photolithography to pattern the channel;
[0054] 11) Etching the MoSe2 channel shape using an ICP dry etcher and CF4 gas;
[0055] 12) Soak in acetone for 3 minutes to remove the photoresist on the surface of the channel material;
[0056] 13) Photolithography of transistor electrode patterns (channel electrodes) and Inverter, NOR, and NAND logic patterns;
[0057] 14) rod coating the MXene electrode by rod coating;
[0058] 15) Soak in acetone to remove the photoresist;
[0059] 16) Calcine the device at 300°C for 1 h in an inert atmosphere to remove water and acetone residues from photolithography.
[0060] Figure 2 This is the Id-Vg characteristic curve (SD = 0.1V) of the FET with MoSe2 channel and MXene electrode in the final product of Experiment 1. The black curve in the figure is the test result, corresponding to the ordinate on the left; the blue curve is the log of the ordinate value on the left, corresponding to the curve on the right. The Id-Vg curve of the FET with 30nm thick Al2O3 as the dielectric layer, MoSe2 as the channel material, and MXene as the electrode has no inflection point. It can be seen that the transistor achieves quasi-ohmic contact and has a mobility of 20cm 2 ·V -1 ·s -1 , the on / off ratio is 10 7 .
[0061] Test 2:
[0062] 1) For local back-gate logic gates, the gate electrode can be obtained by evaporation or sputtering of metal electrodes in addition to MXene. First, the pattern of the back-gate electrode is obtained according to steps 2 and 3 of experiment 1;
[0063] 2) Magnetron sputtering TiPd electrode;
[0064] 3) Soak in acetone for 3 minutes to remove the photoresist on the surface of the TiPd electrode;
[0065] 4) Depositing a 15 nm thick HfO2 dielectric layer or a 30 nm thick Al2O3 dielectric layer on the surface of the TiPd electrode by ALD;
[0066] 5) Preparation of MoSe2 two-dimensional semiconductor solution by electrochemically assisted liquid phase exfoliation;
[0067] 6) Rod coating MoSe2 on the SiO2-TiPd-HfO2 surface;
[0068] 7) The MoSe2 channel was obtained according to steps 9, 10 and 11 of Experiment 1;
[0069] 8) Preparation of logic gate top electrode follows steps 12 to 16 of Experiment 1.
[0070] Test 3:
[0071] 1) For channel materials, it is not limited to MoSe2. Electrochemically assisted liquid phase stripping is also applicable to In2Se3 and MoS2. In2Se3 is prepared by electrochemically assisted stripping;
[0072] 2) The gate electrode (TiPd electrode) and the gate dielectric (HfO2 or Al2O3) were prepared according to steps 1 to 4 in Experiment 2;
[0073] 3) Rod coating of In2Se3 by rod coating;
[0074] 4) In2Se3 film was annealed at 350℃ to remove organic matter;
[0075] 5) Photolithographic patterning of the channel;
[0076] 6) In2Se3 is etched with Ar gas to obtain a patterned channel;
[0077] 7) Soak in acetone to remove the photoresist;
[0078] 8) Photolithography patterning of top electrode patterns of Inverter, NAND and other logic gates;
[0079] 9) Rod coating MXene to obtain a logic gate circuit;
[0080] 10) Remove the photoresist by soaking in acetone.
[0081] Experiment 4: The preparation method for the top-gate logic device is as follows:
[0082] 1) Prepare highly conductive MXene nanosheets by liquid phase exfoliation and wash them multiple times to make them close to electrical neutrality;
[0083] 2) Preparation of MoSe2 solution by electrochemically assisted liquid phase exfoliation;
[0084] 3) Treat SiO2 / Si wafer with piranha solution for hydrophilization;
[0085] 4) Rod coating of MoSe2 on piranha treated SiO2 / Si wafers;
[0086] 5) Calcination to remove organic matter between MoSe2 material layers;
[0087] 6) Photolithography patterning channels;
[0088] 7) Etching the MoSe2 channel shape;
[0089] 8) Soaking the patterned MoSe2 channel in acetone to remove the photoresist on its surface;
[0090] 9) Photolithography patterning of channel electrodes;
[0091] 10) Rod-coated MXene channel electrode;
[0092] 11) Remove the photoresist by immersion in acetone;
[0093] 12) ALD deposition of a 15 nm thick HfO2 dielectric layer or a 30 nm thick Al2O3 dielectric layer;
[0094] 13) Photolithography patterning of gate electrodes of logic gates such as NAND and NOR;
[0095] 14) Evaporation of TiPd electrode;
[0096] 15) Soak in acetone for 3 minutes to remove the photoresist around the electrode.
Claims
1. A method for preparing a rod-coated printed wafer-level FET, characterized in that The preparation method of the rod coating printed wafer-level FET is carried out according to the following steps: First, prepare the two-dimensional semiconductor by electrochemically assisted liquid phase exfoliation, and then disperse it in DMF to obtain a two-dimensional semiconductor solution; 2. Perform hydrophilic treatment on SiO2 / Si wafer; 3. Using a rod coating method, the two-dimensional semiconductor solution of step 1 is evenly coated on the SiO2 / Si wafer hydrophilized in step 2; 4. calcining the product of step 3 to remove organic matter on the surface of the two-dimensional semiconductor; 5. using a photolithography machine to pattern a two-dimensional semiconductor channel on the product of step 4; 6. Etching a two-dimensional semiconductor channel; 7. Soak the two-dimensional semiconductor channel in acetone to remove the photoresist on the surface; 8. Prepare highly conductive MXene nanosheets by liquid phase exfoliation, wash them multiple times to make them electrically neutral, and then disperse the MXene nanosheets in deionized water to obtain a MXene nanosheet solution; 9. Photolithography patterning the shape of the electrode on the product after removing the photoresist in step 7; 10. uniformly coating the MXene nanosheet solution obtained in step 8 on the electrode surface patterned in step 9; 11. Soak the product of step 10 in acetone to remove the photoresist and obtain FET. The structural diagram is shown in Figure 1. The two symmetrical No. 1 are MXene electrodes, and No. 2 is the MoSe2 channel.
2. The method for preparing a rod-coated printed wafer-level FET according to claim 1, characterized in that The material of the two-dimensional semiconductor described in step one is MoSe2, In2Se3 or MoS2; the method for limiting the concentration of the two-dimensional semiconductor solution described in step one is: take 10 μL of the two-dimensional semiconductor solution and dissolve it in 5 mL of DMF, and test its absorbance at 475 nm to be 0.
5.
3. The method for preparing a rod-coated printed wafer-level FET according to claim 1, characterized in that The method for preparing a two-dimensional semiconductor by electrochemically assisted liquid phase exfoliation in step one is as follows: weigh 0.15 g of tetraheptylammonium bromide and 0.6 g of polyvinylpyrrolidone and dissolve them in DMF, use a carbon rod as the positive electrode and a two-dimensional semiconductor raw material as the negative electrode, and apply a voltage of 5V to 10V for intercalation for 1 hour; weigh 0.4 g of PVP and dissolve it in 20 mL of DMF, add the intercalated two-dimensional semiconductor and ultrasonicate for 5 minutes, then centrifuge at 3000 rpm for 5 minutes, and then take the upper layer solution and centrifuge it at 10000 rpm for 10 minutes. The solid part obtained is the two-dimensional semiconductor.
4. The method for preparing a rod-coated printed wafer-level FET according to claim 1, characterized in that In step 2, the method for hydrophilizing the SiO2 / Si wafer is as follows: immersing the SiO2 / Si wafer in a piranha solution for 30 minutes to obtain a hydrophilized surface; or using plasma to hydrophilize the SiO2 / Si surface for 5 minutes at a power of 100W.
5. The method for preparing a rod-coated printed wafer-level FET according to claim 1, characterized in that The stick coating method in step three is done with a Meyer stick.
6. The method for preparing a rod-coated printed wafer-level FET according to claim 1, characterized in that In step 4, the calcination temperature is 300°C and the time is 1h to 2h, and the SiO2 / Si sheet is carried along during calcination.
7. The method for preparing a rod-coated printed wafer-level FET according to claim 1, characterized in that The photolithography step in step five includes spin coating of photoresist, exposure and development.
8. The method for preparing a rod-coated printed wafer-level FET according to claim 1, characterized in that In step six, etching is performed using an ICP dry etcher, using CF4 or SF6 gas.
9. The method for preparing a rod-coated printed wafer-level FET according to claim 1, characterized in that In step eight, highly conductive MXene nanosheets are prepared by liquid phase exfoliation, washed multiple times to make them electrically neutral, and then the MXene nanosheets are dispersed in deionized water to obtain a MXene nanosheet solution. The specific process is as follows: Weigh 1.6 g of lithium fluoride and add it to 20 mL of 36% hydrochloric acid, stir in a water bath at 40°C for 15 min, slowly add 1 g of MXene powder, react for 10 h, centrifuge at 8000 rpm for 5 min, add 50 mL of deionized water, shake at 140 rpm for 1 d with a shaker, centrifuge at 3000 rpm for 5 min, take the upper solution and centrifuge at 10000 rpm for 10 min, wash the precipitate several times to make it electrically neutral, and test the electrical neutrality with pH test paper; then disperse the precipitate in deionized water to obtain a MXene nanosheet solution with a concentration of 3 to 5 mg / mL.
10. The method for preparing a rod-coated printed wafer-level FET according to claim 1, characterized in that The photolithography step in step nine includes spin coating of photoresist, exposure and development.