Light conversion glass, preparation method and photovoltaic module

By doping rare earth elements into the encapsulated glass of photovoltaic cells, the conversion of ultraviolet rays into visible light is achieved, and the damage to photovoltaic cells is solved, which extends the service life and improves the performance and efficiency of photovoltaic modules.

CN119029075APending Publication Date: 2024-11-26TRINA SOLAR CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411124009.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-16
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

The encapsulated glass of existing photovoltaic cells has a high UV transmittance and cannot effectively resist the damage of UV to crystalline silicon or amorphous silicon components, resulting in battery power attenuation and aging.

Method used

Light conversion glass doped with rare earth elements is used to convert ultraviolet rays into visible light, which is used to protect photovoltaic cells and improve their photoelectric conversion efficiency.

Benefits of technology

It effectively extends the service life of photovoltaic cells, improves the overall performance and initial power of photovoltaic modules, and reduces power attenuation.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119029075A_ABST
    Figure CN119029075A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of photovoltaic materials, and particularly provides light conversion glass, a preparation method and a photovoltaic module, the light conversion glass comprises matrix glass doped with a light conversion material, and the light conversion material comprises rare earth elements and is used for converting ultraviolet light into visible light. The light conversion glass can convert ultraviolet rays into visible light, and can reduce power attenuation when being used in photovoltaic cells.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of photovoltaic materials, and specifically provides a light conversion glass, a preparation method and a photovoltaic module. Background Art

[0002] With the continuous growth of global energy demand, the exploitation and utilization of traditional fossil energy has faced serious challenges. Not only are the resources limited, but also they have a great pressure on the environment. Therefore, the development and utilization of new energy has become the focus of world attention. As a clean and renewable energy form, solar energy is of great significance in alleviating energy pressure, reducing environmental pollution and promoting sustainable development.

[0003] Photovoltaic cells, as a device that directly uses sunlight to generate electricity, have been widely used. Photovoltaic cells use solar energy to generate electricity, and do not produce any pollutants in the process. They are a clean and environmentally friendly form of energy. Vigorously developing photovoltaic cells will help reduce greenhouse gas emissions from the combustion of fossil fuels, alleviate the pressure of global warming, protect the ecological environment, and achieve sustainable development. The basis of the working principle of photovoltaic cells is the photovoltaic effect of the semiconductor PN junction. The so-called photovoltaic effect is an effect that when an object is exposed to light, the charge distribution state in the object changes, generating electromotive force and current. When sunlight or other light irradiates the PN junction of a semiconductor, a voltage will appear on both sides of the PN junction, which is called photovoltaic voltage.

[0004] In solar power generation systems, glass is often used as a packaging material for battery components to prevent crystalline silicon or amorphous silicon components from aging under ultraviolet radiation, thereby shortening their service life. However, the ultraviolet transmittance of the packaging glass in the prior art is relatively high, and it cannot effectively prevent ultraviolet damage to crystalline silicon or amorphous silicon components.

[0005] In photovoltaic cells, the TCO film layer and amorphous or microcrystalline silicon film layer in HJT cells absorb ultraviolet light, which makes it more likely to cause photoaging of the cells and make the current of the cells lower than that of ordinary cells, which can easily cause power attenuation of the components.

[0006] Therefore, a UV cut-off film is needed to protect photovoltaic cells. The UV cut-off film in the prior art usually increases the utilization rate of UVA and reduces the damage of the UVB band to photovoltaic cells and light conversion powder by adding UV absorbers and light conversion powder to the film. However, components prepared using the existing UV cut-off film will result in low initial power of the components. Summary of the invention

[0007] In order to overcome the above defects, the present invention provides a light conversion glass, a preparation method and a photovoltaic module. The light conversion glass of the present invention can convert ultraviolet rays into visible light and can reduce power attenuation when used in photovoltaic cells.

[0008] In a first aspect, the present invention provides a light-converting glass, comprising:

[0009] A matrix glass doped with a light conversion material, wherein the light conversion material includes a rare earth element and is used to convert ultraviolet light into visible light.

[0010] Furthermore, the light conversion material includes a trivalent or divalent rare earth element.

[0011] Furthermore, the rare earth element includes one or more of yttrium, europium, cerium, samarium, thulium, neodymium, holmium, praseodymium, lanthanum, gadolinium, terbium, dysprosium, erbium, ytterbium, and lutetium.

[0012] Furthermore, the light conversion material includes oxides, fluorides or silicates of trivalent or divalent rare earth elements.

[0013] Furthermore, the photoconversion material includes one or more of cerium trioxide, thulium trioxide, samarium trioxide, yttrium fluoride, bismuth trioxide, europium trioxide, lanthanum trioxide and cerium silicate.

[0014] Furthermore, the mass fraction of the light conversion material in the matrix glass is 0.01%-10%.

[0015] Furthermore, the matrix glass includes Na2O-CaO-SiO2 glass.

[0016] Furthermore, the thickness of the matrix glass is 1 mm-12 mm.

[0017] Furthermore, the glass further comprises:

[0018] The anti-reflection film is arranged on the substrate glass.

[0019] In a second aspect, the present invention provides a method for preparing a light-converting glass, comprising:

[0020] forming a mixture of a matrix glass and a light conversion material;

[0021] Melt-forming based on the mixture;

[0022] The formed mixture is annealed.

[0023] In a third aspect, the present invention provides a photovoltaic module, comprising:

[0024] The light conversion glass according to the first aspect; and

[0025] Photovoltaic cells;

[0026] Furthermore, the photovoltaic cell is a HJT cell.

[0027] The above one or more technical solutions of the present invention have at least one or more of the following beneficial effects:

[0028] The present invention adds a light conversion material to the matrix glass, and the light conversion material can be well dispersed in the matrix glass to improve the light conversion performance of the glass. The light conversion glass and the photovoltaic cell form a photovoltaic module, and the light conversion glass converts ultraviolet light into visible light, thereby protecting the photovoltaic cell and extending its service life. At the same time, the light conversion glass can also improve the photoelectric conversion efficiency of the photovoltaic cell, further improving the overall performance of the photovoltaic module. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] The disclosure of the present invention will become more easily understood with reference to the accompanying drawings. It will be readily understood by those skilled in the art that these drawings are only for illustrative purposes and are not intended to limit the scope of protection of the present invention. In addition, similar numbers in the drawings represent similar components, wherein:

[0030] Figure 1 is a schematic flow chart of a method for preparing light-converting glass according to the present invention;

[0031] Figure 2 is a schematic diagram of the structure of a photovoltaic module according to the present invention;

[0032] Figure 3 is a schematic diagram of the light conversion effect of the light conversion glass sample according to Example 1 of the present invention;

[0033] Figure 4 is a schematic diagram of the light conversion effect of the light conversion glass sample according to Example 2 of the present invention;

[0034] Figure 5 is a schematic diagram of the light conversion effect of the light conversion glass sample according to Example 3 of the present invention;

[0035] Figure 6 is a schematic diagram of the light conversion effect of the light conversion glass sample according to Example 4 of the present invention;

[0036] Figure 7 Schematic diagram of the light conversion effect of the light conversion glass sample according to Example 5 of the present invention. DETAILED DESCRIPTION

[0037] Some embodiments of the present invention are described below with reference to the accompanying drawings. It should be understood by those skilled in the art that these embodiments are only used to explain the technical principles of the present invention and are not intended to limit the protection scope of the present invention.

[0038] The present invention provides a light conversion glass, comprising:

[0039] A matrix glass doped with a light conversion material, wherein the light conversion material includes a rare earth element and is used to convert ultraviolet light into visible light.

[0040] The present invention introduces a light conversion material into the matrix glass, which can effectively change the wavelength of light incident on the glass, thereby solving the problem of damage to photovoltaic cells caused by ultraviolet rays and making the most of incident light, thereby reducing energy loss.

[0041] The light conversion glass of the present invention can be applied to photovoltaic cells (solar cells).

[0042] In photovoltaic cells, ultraviolet damage is mainly reflected in two aspects: first, ultraviolet can cause the performance of photovoltaic cells to decline, and second, ultraviolet can accelerate the aging of battery components. The present invention modifies the matrix glass to enable it to have the function of light conversion.

[0043] The present invention adopts a light conversion material to convert ultraviolet rays into visible light. In this way, the damage of ultraviolet rays to photovoltaic cells is effectively alleviated. At the same time, the energy conversion efficiency of photovoltaic cells under light conditions is improved.

[0044] In one embodiment, the light conversion material includes a trivalent or divalent rare earth element.

[0045] In order to realize light conversion in the present invention, the valence state of the rare earth element doped in the matrix glass is positive trivalent or positive divalent.

[0046] In one embodiment, the rare earth element includes one or more of yttrium, europium, cerium, samarium, thulium, neodymium, holmium, praseodymium, lanthanum, gadolinium, terbium, dysprosium, erbium, ytterbium, and lutetium.

[0047] In one embodiment, the light conversion material includes oxides, fluorides or silicates of trivalent or divalent rare earth elements.

[0048] In the present invention, the rare earth element exists in the matrix glass in the form of +3 or +2 valence oxide, fluoride or silicate.

[0049] In one embodiment, the light conversion material includes cerium trioxide and thulium trioxide.

[0050] One or more of samarium trioxide, yttrium fluoride, bismuth trioxide, europium trioxide, lanthanum trioxide and cerium silicate.

[0051] In one embodiment, the mass fraction of the light conversion material in the matrix glass is 0.01%-10%.

[0052] Under this doping amount, the light conversion glass of the present invention effectively converts ultraviolet light in incident light into visible light.

[0053] In one embodiment, the matrix glass includes Na2O-CaO-SiO2 glass.

[0054] In one embodiment, the thickness of the matrix glass is 1 mm-12 mm.

[0055] When glass is used in the field of photovoltaic cell technology, especially the application of photovoltaic cells in the field of construction, the matrix glass needs to have sufficient strength to cope with bad weather such as wind, rain, etc. If the thickness of the matrix glass is too low, its strength is insufficient and it may break in bad weather, thus affecting the normal use of photovoltaic cells. Therefore, in this case, the thickness of the matrix glass must meet certain standards to ensure that it has sufficient strength in the application of the construction field.

[0056] However, on the other hand, too high glass thickness will also bring some problems. First, the cost of glass that is too thick will increase accordingly during the manufacturing process. This is because glass that is too thick requires more raw materials and the manufacturing process is more complicated, which will lead to higher costs. Secondly, glass that is too thick will also lead to quality redundancy.

[0057] In one embodiment, the thickness of the matrix glass is 1 mm-6 mm.

[0058] In one embodiment, the glass further comprises:

[0059] The anti-reflection film is arranged on the substrate glass. The anti-reflection film is plated on the surface of the substrate glass to enhance the light transmittance.

[0060] When the light conversion glass of the present invention is used for photovoltaic cells, the anti-reflection film (anti-reflection film) mainly plays the following roles:

[0061] (1) Reduce reflectivity and increase light absorption: Anti-reflection film reduces the reflection of light on the surface of photovoltaic cells, allowing more light to be absorbed by the cells.

[0062] (2) Enhanced light transmission: Anti-reflection film can enhance the light transmission ability, making it easier for light to pass through the surface of the photovoltaic cell and reach the photovoltaic devices inside the cell.

[0063] (3) Improve the conversion efficiency of photovoltaic cells: Since the anti-reflection film reduces reflection and enhances light transmission, photovoltaic cells can absorb more sunlight and convert it into electrical energy.

[0064] (4) Protecting photovoltaic cells: Anti-reflection film also has good anti-oxidation and corrosion resistance, which can protect the surface of photovoltaic cells in various harsh environments, extend their service life and reduce maintenance costs.

[0065] Reference Figure 1 The present invention also provides a method for preparing light-converting glass, comprising:

[0066] S10, forming a mixture of a matrix glass and a light conversion material;

[0067] S20, performing melt forming based on the mixture;

[0068] S30, annealing is performed based on the formed mixture.

[0069] In forming the mixture of the matrix glass and the light conversion material, the light conversion material may be added after the matrix glass is melted and then mixed evenly in a molten state, or the matrix glass and the light conversion material may be mixed, melted, and then mixed evenly.

[0070] The S20, melt-forming based on the mixture comprises:

[0071] Melt at 1470℃ for 35min.

[0072] The S30, annealing based on the formed mixture, comprises:

[0073] Anneal at 500 °C for 4 h.

[0074] Reference Figure 2 The present invention also provides a photovoltaic module, comprising:

[0075] The light conversion glass; and

[0076] Photovoltaic cells.

[0077] In one embodiment, the photovoltaic cell generally includes front glass, front packaging film, welded cell layer, rear packaging film, back plate or rear glass during packaging.

[0078] The cell layer includes photovoltaic cells for converting light energy into electrical energy.

[0079] The main purpose of encapsulation is to protect photovoltaic cells from damage by the external environment, while improving the efficiency and stability of photovoltaic modules.

[0080] The light conversion glass of the present invention is used as the front glass during the packaging of photovoltaic cells.

[0081] The front glass mainly protects the cells and increases light transmittance, allowing more sunlight to shine on the photovoltaic cells. The front encapsulation film is used to tightly bond the photovoltaic cells to the front glass to form a sealed whole, preventing impurities such as moisture and dust from entering the cell layer.

[0082] The present invention adds rare earth elements to inorganic glass. Compared with the prior art, it has significant advancement. First, rare earth elements have better compatibility with glass and can be better dispersed in glass, thereby improving the light conversion performance of glass. Secondly, glass has a higher temperature tolerance, which is conducive to process control and avoids the decomposition and combustion problems of the adhesive film in a high temperature environment. The application of photoconversion glass in the field of photovoltaic cells is of great significance. Photovoltaic cells, as a renewable energy source, are affected by ultraviolet rays, which will cause performance degradation or even damage. By using photoconversion glass, ultraviolet rays are converted into visible light, thereby protecting photovoltaic cells and extending their service life. At the same time, photoconversion glass can also improve the photoelectric conversion efficiency of photovoltaic cells and further improve the overall performance of the system.

[0083] The following examples 1-6 illustrate the process of preparing light conversion glass by adding different light conversion materials to matrix glass, as well as the corresponding light conversion effect and electrochemical performance of a photovoltaic module composed of the prepared glass and photovoltaic cells.

[0084] Example 1

[0085] The matrix glass adopts Na2O-CaO-SiO2, and the matrix glass ingredients include SiO2, Na2CO3, CaCO3, Al2O3 and MgO. The mass fraction ratios of SiO2, Na2CO3, CaCO3, Al2O3 and MgO are 70%, 13%, 11%, 3% and 3% respectively.

[0086] The matrix glass is doped with cerium oxide, wherein the mass fraction of cerium oxide in the matrix glass is 0.19%.

[0087] The Na2O-CaO-SiO2 matrix glass and cerium oxide are mixed according to the above ratio to form a uniform mixture.

[0088] The mixed material is melted at 1470° C. for 35 minutes to achieve melt forming;

[0089] The melt-formed mixture was annealed at 500° C. for 4 hours to obtain the light-converting glass sample of Example 1.

[0090] Comparative Example 1

[0091] The only difference between Comparative Example 1 and Example 1 is that cerium trioxide is not doped into the matrix glass in Comparative Example 1. Finally, a glass sample of Comparative Example 1 is obtained.

[0092] The products of Example 1 and Comparative Example 1 were tested respectively.

[0093] The results showed that the reference Figure 3The light conversion glass sample of Example 1 can well convert 320nm ultraviolet light into 400-460nm blue-violet light.

[0094] Comparative Example 1 and Example 1 were respectively applied in photovoltaic modules, and the average power of the photovoltaic modules was increased from 701.5 W (glass sample of Comparative Example 1) to 703.3 W (light-conversion glass sample of Example 1). After UV60 aging test, the power attenuation was reduced from 6.4% (glass sample of Comparative Example 1) to 3.2% (light-conversion glass sample of Example 1).

[0095] Example 2

[0096] The matrix glass adopts Na2O-CaO-SiO2, and the matrix glass ingredients include SiO2, Na2CO3, CaCO3, Al2O3 and MgO. The mass fraction ratios of SiO2, Na2CO3, CaCO3, Al2O3 and MgO are 70%, 13%, 11%, 3% and 3% respectively.

[0097] The matrix glass is doped with cerium oxide and thulium oxide, wherein the mass fraction of cerium oxide in the matrix glass is 0.19%, and the mass fraction of thulium oxide in the matrix glass is 0.41%.

[0098] According to the above ratio, Na2O-CaO-SiO2 matrix glass is mixed with cerium trioxide and thulium trioxide to form a uniform mixture.

[0099] The mixed material is melted at 1470° C. for 35 minutes to achieve melt forming;

[0100] The melt-formed mixture was annealed at 500° C. for 4 hours to obtain the light-converting glass sample of Example 2.

[0101] Comparative Example 2

[0102] The only difference between Comparative Example 2 and Example 2 is that cerium trioxide and thulium trioxide are not doped into the matrix glass in Comparative Example 2. Finally, a glass sample of Comparative Example 2 is obtained.

[0103] The products of Example 2 and Comparative Example 2 were tested respectively.

[0104] The results show that Figure 4 The light conversion glass sample of Example 2 can well convert 320nm ultraviolet light into 400-460nm blue-violet light.

[0105] Comparative Example 2 and Example 2 were respectively applied in photovoltaic modules, and the average power of the photovoltaic modules was increased from 701.5 W (glass sample of Comparative Example 2) to 704.1 W (light-conversion glass sample of Example 2). After UV60 aging test, the power attenuation was reduced from 6.4% (glass sample of Comparative Example 2) to 2.8% (light-conversion glass sample of Example 2).

[0106] Example 3

[0107] The matrix glass adopts Na2O-CaO-SiO2, and the matrix glass ingredients include SiO2, Na2CO3, CaCO3, Al2O3 and MgO. The mass fraction ratios of SiO2, Na2CO3, CaCO3, Al2O3 and MgO are 70%, 13%, 11%, 3% and 3% respectively.

[0108] The matrix glass is doped with cerium trioxide, thulium trioxide and samarium trioxide, wherein the mass fraction of cerium trioxide in the matrix glass is 0.19%; the mass fraction of thulium trioxide in the matrix glass is 0.43%; and the mass fraction of samarium trioxide in the matrix glass is 1.15%.

[0109] According to the above ratio, Na2O-CaO-SiO2 matrix glass is mixed with cerium trioxide, thulium trioxide and samarium trioxide to form a uniform mixture.

[0110] The mixed material is melted at 1470° C. for 35 minutes to achieve melt forming;

[0111] The melt-formed mixture was annealed at 500° C. for 4 h to obtain the light-converting glass sample of Example 3.

[0112] Comparative Example 3

[0113] The only difference between Comparative Example 3 and Example 3 is that cerium trioxide, thulium trioxide and samarium trioxide are not doped into the matrix glass in Comparative Example 3. Finally, a glass sample of Comparative Example 3 is obtained.

[0114] The products of Example 3 and Comparative Example 3 were tested respectively.

[0115] The results show that Figure 5 The light conversion glass sample of Example 3 can well convert 390nm ultraviolet light into 400-460nm blue-violet light.

[0116] Comparative Example 3 and Example 3 were respectively applied in photovoltaic modules, and the average power of the photovoltaic modules was increased from 701.5 W (glass sample of Comparative Example 3) to 704.7 W (light-conversion glass sample of Example 3). After UV60 aging test, the power attenuation was reduced from 6.4% (glass sample of Comparative Example 3) to 2.4% (light-conversion glass sample of Example 3).

[0117] Example 4

[0118] The matrix glass adopts Na2O-CaO-SiO2, and the matrix glass ingredients include SiO2, Na2CO3, CaCO3, Al2O3 and MgO. The mass fraction ratios of SiO2, Na2CO3, CaCO3, Al2O3 and MgO are 70%, 13%, 11%, 3% and 3% respectively.

[0119] Yttrium fluoride, bismuth trioxide and europium trioxide are doped into the matrix glass, wherein the mass fraction of yttrium fluoride in the matrix glass is 7.45%, the mass fraction of bismuth trioxide in the matrix glass is 0.05%, and the mass fraction of europium trioxide in the matrix glass is 0.075%.

[0120] According to the above ratio, Na2O-CaO-SiO2 matrix glass is mixed with yttrium fluoride, bismuth trioxide and europium trioxide to form a uniform mixture.

[0121] The mixed material is melted at 1470° C. for 35 minutes to achieve melt forming;

[0122] The melt-formed mixture was annealed at 500° C. for 4 h to obtain the light-converting glass sample of Example 4.

[0123] Comparative Example 4

[0124] The only difference between Comparative Example 4 and Example 4 is that yttrium fluoride, bismuth trioxide and europium trioxide are not doped into the matrix glass in Comparative Example 4. Finally, a glass sample of Comparative Example 4 is obtained.

[0125] The results show that Figure 6 The light conversion glass sample of Example 4 can well convert 300nm-400nm ultraviolet light into 420-650nm blue-violet light and red light.

[0126] Comparative Example 4 and Example 4 were respectively applied in photovoltaic modules, and the average power of the photovoltaic modules was increased from 701.5 W (glass sample of Comparative Example 4) to 704.5 W (light-conversion glass sample of Example 4). After UV60 aging test, the power attenuation was reduced from 6.4% (glass sample of Comparative Example 4) to 2.5% (light-conversion glass sample of Example 4).

[0127] Example 5

[0128] The matrix glass adopts Na2O-CaO-SiO2, and the matrix glass ingredients include SiO2, Na2CO3, CaCO3, Al2O3 and MgO. The mass fraction ratios of SiO2, Na2CO3, CaCO3, Al2O3 and MgO are 70%, 13%, 11%, 3% and 3% respectively.

[0129] Samarium trioxide and lanthanum trioxide are doped into the matrix glass, wherein the mass fraction of samarium trioxide in the matrix glass is 2.4%, and the mass fraction of lanthanum trioxide in the matrix glass is 4.2%.

[0130] The Na2O-CaO-SiO2 matrix glass is mixed with samarium trioxide and lanthanum trioxide according to the above ratio to form a uniform mixture.

[0131] The mixed material is melted at 1470° C. for 35 minutes to achieve melt forming;

[0132] The melt-formed mixture was annealed at 500° C. for 4 h to obtain the light-converting glass sample of Example 5.

[0133] Comparative Example 5

[0134] The only difference between Comparative Example 5 and Example 5 is that samarium trioxide and lanthanum trioxide are not doped into the matrix glass in Comparative Example 5. Finally, a glass sample of Comparative Example 5 is obtained.

[0135] The results show that Figure 7 The light conversion glass sample of Example 5 can better convert 340nm ultraviolet light into 420-660nm visible light.

[0136] Comparative Example 5 and Example 5 were respectively applied in photovoltaic modules, and the average power of the photovoltaic modules was increased from 701.5 W (glass sample of Comparative Example 5) to 703.9 W (light-conversion glass sample of Example 5). After UV60 aging test, the power attenuation was reduced from 6.4% (glass sample of Comparative Example 5) to 2.7% (light-conversion glass sample of Example 5).

[0137] Example 6

[0138] The matrix glass adopts Na2O-CaO-SiO2, and the matrix glass ingredients include SiO2, Na2CO3, CaCO3, Al2O3 and MgO. The mass fraction ratios of SiO2, Na2CO3, CaCO3, Al2O3 and MgO are 70%, 13%, 11%, 3% and 3% respectively.

[0139] Cerium silicate is doped into the matrix glass, wherein the mass fraction of cerium silicate in the matrix glass is 1.2%.

[0140] The Na2O-CaO-SiO2 matrix glass and cerium silicate are mixed according to the above ratio to form a uniformly mixed mixture.

[0141] The mixed material is melted at 1470° C. for 35 minutes to achieve melt forming;

[0142] The melt-formed mixture was annealed at 500° C. for 4 h to obtain the light-converting glass sample of Example 6.

[0143] Comparative Example 6

[0144] The only difference between Comparative Example 6 and Example 6 is that samarium trioxide and lanthanum trioxide are not doped into the matrix glass in Comparative Example 6. Finally, a glass sample of Comparative Example 6 is obtained.

[0145] The results show that the light conversion glass sample of Example 6 can well convert 320nm ultraviolet light into 400-460nm blue-violet light.

[0146] Comparative Example 6 and Example 6 were respectively applied in photovoltaic modules, and the average power of the photovoltaic modules was increased from 701.5 W (glass sample of Comparative Example 6) to 703.2 W (light-conversion glass sample of Example 6). After UV60 aging test, the power attenuation was reduced from 6.4% (glass sample of Comparative Example 6) to 3.1% (light-conversion glass sample of Example 6).

[0147] Example 7

[0148] The matrix glass adopts Na2O-CaO-SiO2, and the matrix glass ingredients include SiO2, Na2CO3, CaCO3, Al2O3 and MgO. The mass fraction ratios of SiO2, Na2CO3, CaCO3, Al2O3 and MgO are 70%, 13%, 11%, 3% and 3% respectively.

[0149] The matrix glass is doped with cerium oxide, wherein the mass fraction of cerium oxide in the matrix glass is 0.01%.

[0150] The Na2O-CaO-SiO2 matrix glass and cerium oxide are mixed according to the above ratio to form a uniform mixture.

[0151] The mixed material is melted at 1470° C. for 35 minutes to achieve melt forming;

[0152] The melt-formed mixture was annealed at 500° C. for 4 h to obtain the light-converting glass sample of Example 7.

[0153] Comparative Example 7

[0154] The only difference between Comparative Example 7 and Example 7 is that in Comparative Example 7, cerium oxide is not doped into the matrix glass.

[0155] The results show that the light conversion glass sample of Example 7 can convert 320nm ultraviolet light into 400-460nm blue-violet light.

[0156] Comparative Example 7 and Example 7 were respectively applied in photovoltaic modules, and the average power of the photovoltaic modules was increased from 701.5 W (glass sample of Comparative Example 7) to 701.8 W (light-conversion glass sample of Example 7). After UV60 aging test, the power attenuation was reduced from 6.4% (glass sample of Comparative Example 7) to 6.2% (light-conversion glass sample of Example 7).

[0157] It can be seen from the experimental data of Example 7 and Comparative Example 7 that although doping with a lower concentration of cerium trioxide has a light conversion effect and can reduce the power attenuation of the photovoltaic module, the effect is weaker than that of other embodiments. This is because the lower doping concentration causes the lower light conversion efficiency, so the effect is not as strong as that of other embodiments.

[0158] Example 8

[0159] The matrix glass adopts Na2O-CaO-SiO2, and the matrix glass ingredients include SiO2, Na2CO3, CaCO3, Al2O3 and MgO. The mass fraction ratios of SiO2, Na2CO3, CaCO3, Al2O3 and MgO are 70%, 13%, 11%, 3% and 3% respectively.

[0160] The matrix glass is doped with cerium oxide, wherein the mass fraction of cerium oxide in the matrix glass is 10%.

[0161] The Na2O-CaO-SiO2 matrix glass and cerium oxide are mixed according to the above ratio to form a uniform mixture.

[0162] The mixed material is melted at 1470° C. for 35 minutes to achieve melt forming;

[0163] The melt-formed mixture was annealed at 500° C. for 4 hours to obtain the light-converting glass sample of Example 1.

[0164] Comparative Example 8

[0165] The only difference between Comparative Example 8 and Example 8 is that cerium trioxide is not doped into the matrix glass in Comparative Example 8. Finally, a glass sample of Comparative Example 8 is obtained.

[0166] The products of Example 8 and Comparative Example 8 were tested respectively.

[0167] The results show that the light conversion glass sample of Example 8 can convert 320nm ultraviolet light into 400-460nm blue-violet light.

[0168] Comparative Example 8 and Example 8 were respectively applied in photovoltaic modules, and the average power of the photovoltaic modules was increased from 701.5 W (glass sample of Comparative Example 1) to 702 W (light-conversion glass sample of Example 8). After UV60 aging test, the power attenuation was reduced from 6.4% (glass sample of Comparative Example 8) to 6% (light-conversion glass sample of Example 8).

[0169] It can be observed from the experimental data of Example 8 and Comparative Example 8 that under the condition of high cerium oxide doping concentration, although there is a light conversion effect and the power attenuation of the photovoltaic module can be reduced, its effect is relatively weak compared with other embodiments. This phenomenon occurs because the high doping concentration leads to fluorescence quenching to a certain extent.

[0170] In the prior art, light-converting powder is usually added to the packaging film to improve its optical properties. However, this method has a significant disadvantage, that is, the dispersion of the light-converting powder is poor, which easily leads to poor uniformity inside the film. When rare earth ions are added to the packaging film, due to the poor compatibility of inorganic rare earth ions with organic packaging films, rare earth ions are easy to migrate in the film, thereby damaging other electrical devices.

[0171] In addition, the existing encapsulation film is mainly composed of organic matter, and its tolerance temperature is generally around 200° C. In a high temperature environment, the film may decompose or burn, which is very unfavorable for process control.

[0172] In the present invention, glass is a compound composed of inorganic elements such as silicon and oxygen, and has a stable crystal structure, so it has good thermal stability and chemical stability. Rare earth ions are added to glass in the form of inorganic substances, and this addition method greatly improves the compatibility of rare earth ions with glass. Since rare earth ions and glass are both inorganic substances, they can better blend with each other to form a uniform dispersion state. This uniform dispersion state is crucial for rare earth ions to play a light conversion role in glass, and can ensure that light is effectively affected by rare earth ions when propagating in glass, thereby achieving a specific light conversion effect.

[0173] In specific embodiments of the present invention, such as those shown in Examples 1, 6, 7 and 8, specific rare earth ions are introduced into the glass. These rare earth elements, due to their unique electronic structure, can absorb the energy in their 4f orbits when excited by external energy, and achieve a transition from the ground state to the excited state. This is an energy absorption process in which electrons are promoted to a higher energy level. Next, when these electrons fall back from the excited state to the ground state, they release the previously absorbed energy in the form of light. It is through this energy conversion mechanism that the light conversion effect is achieved.

[0174] In the detailed embodiments of the present invention, as specifically presented in Examples 2, 3, 4 and 5, the present invention adds a specific combination of rare earth ions to the glass. When one of the rare earth ions is excited to a high energy state, it may transfer energy to another rare earth ion by non-radiative transition, so that the latter transitions from the ground state to the excited state and finally emits specific light. This energy transfer process can occur between different rare earth ions, thereby affecting the light conversion performance of the glass.

[0175] In addition, some rare earth ions can also act as sensitizers to improve the excitation efficiency of other rare earth ions. In this way, the present invention combines different rare earth elements to optimize and improve the light conversion performance of the glass.

[0176] Whether it is a single-component rare earth element or a multi-component rare earth element, in the embodiments of the present invention, the amount of light conversion material added is limited. The doping concentration of rare earth ions has a great influence on the light conversion performance. When the doping concentration is too high, the distance between the rare earth ions is shortened, and non-radiative energy transfer is likely to occur, resulting in a decrease in luminous intensity. The present invention can improve the light conversion performance of glass by optimizing the doping concentration of rare earth ions. As a high-temperature resistant material, the excellent thermal stability of glass provides a strong guarantee for the addition of rare earth ions. There may be chemical bonding, charge transfer and other interactions between the matrix material and the rare earth ions. These interactions will affect the luminous performance and stability of the rare earth ions. During the preparation process, the glass can withstand high-temperature treatment, so that the rare earth ions can be evenly dispersed in the glass matrix without destroying its structure or affecting its performance due to high temperature. This greatly reduces the difficulty of preparation and process control, and improves production efficiency.

[0177] Therefore, the present invention converts light in the low EQE region of the photovoltaic cell in the incident light into visible light with a response close to 100%, while improving the utilization rate of sunlight, avoiding the addition of light conversion powder in the packaging film, reducing the amount of inorganic substances added to the packaging film, and improving the initial power of the photovoltaic module.

[0178] In one embodiment, the photovoltaic cell is a HJT cell.

[0179] HJT (Heterojunction with Intrinsic Thin-film) cells are intrinsic thin-film heterojunction cells. A major problem faced in practical applications is that due to the poor conductivity of amorphous silicon, a transparent conductive film (TCO) is deposited on both sides of the cell for conductivity. The transparent conductive oxide (TCO) and amorphous silicon film layer of the cell absorb ultraviolet rays, resulting in a decrease in the battery current. In addition, the HJT cell is a multi-layer structure, one of which uses amorphous or microcrystalline silicon. Due to the Si-H groups on the surface, it decays faster than other types of cells under ultraviolet exposure, resulting in a decrease in component efficiency. The conventional solution is to use a cut-off film to filter ultraviolet rays, but this method loses ultraviolet energy. The light conversion glass of the present invention and the HJT cell form a photovoltaic module, which can avoid damage to the HJT cell by ultraviolet rays without losing ultraviolet energy, and effectively improve the photoelectric conversion efficiency of the HJT cell.

[0180] It should be pointed out that although the various steps in the above embodiments are described in a specific order, those skilled in the art can understand that in order to achieve the effects of the present invention, different steps do not have to be performed in such an order. They can be performed simultaneously (in parallel) or in other orders. These changes are within the scope of protection of the present invention.

[0181] So far, the technical solutions of the present invention have been described in conjunction with the preferred embodiments shown in the accompanying drawings. However, it is easy for those skilled in the art to understand that the protection scope of the present invention is obviously not limited to these specific embodiments. Without departing from the principle of the present invention, those skilled in the art can make equivalent changes or substitutions to the relevant technical features, and the technical solutions after these changes or substitutions will fall within the protection scope of the present invention.

Claims

1. A light conversion glass, characterized in that: include: A matrix glass doped with a light conversion material, wherein the light conversion material includes a rare earth element and is used to convert ultraviolet light into visible light.

2. The glass according to claim 1, characterized in that The light conversion material includes a trivalent or divalent rare earth element.

3. The glass according to claim 1 or 2, characterized in that: The rare earth element includes one or more of yttrium, europium, cerium, samarium, thulium, neodymium, holmium, praseodymium, lanthanum, gadolinium, terbium, dysprosium, erbium, ytterbium, and lutetium.

4. The glass according to claim 1 or 2, characterized in that: The light conversion material includes oxides, fluorides or silicates of trivalent or divalent rare earth elements.

5. The glass according to claim 4, characterized in that The photoconversion material includes one or more of cerium trioxide, thulium trioxide, samarium trioxide, yttrium fluoride, bismuth trioxide, europium trioxide, lanthanum trioxide and cerium silicate.

6. The glass according to claim 1, characterized in that The mass fraction of the light conversion material in the matrix glass is 0.01%-10%.

7. The glass according to claim 1, characterized in that The matrix glass includes Na2O-CaO-SiO2 glass.

8. The glass according to claim 1, characterized in that The thickness of the matrix glass is 1 mm to 12 mm.

9. The glass according to claim 1, characterized in that The glass also includes: The anti-reflection film is arranged on the substrate glass.

10. A method for preparing light-converting glass, comprising: forming a mixture of a matrix glass and a light conversion material; Melt-forming based on the mixture; The formed mixture is annealed.

11. A photovoltaic module, comprising: The light conversion glass according to any one of claims 1 to 9; as well as Photovoltaic cells.

12. The assembly according to claim 10, characterized in that The photovoltaic cell is a HJT cell.

Citation Information

Cited By

  • Multi-layer coating for photovoltaic glass

    WO2025238653A1