Solid polymer electrolyte membrane for silicon-based all-solid-state battery as well as preparation method and application of solid polymer electrolyte membrane
By using a solid polymer electrolyte membrane containing carboxyl groups in silicon-based all-solid-state batteries, the problems of poor solid/solid interface impedance and cyclic stability are solved, and higher ionic conductivity and electrochemical window width are achieved, thereby improving battery performance and stability.
Patent Information
- Application Number
- CN202411214601.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-01
- Publication Date
- 2024-11-26
AI Technical Summary
The solid/solid interface impedance in silicon-based all-solid state batteries is large, the cycle stability of silicon materials is poor, and the solid electrolyte membrane preparation method is complex, which limits the improvement of battery performance and commercial applications.
A solid polymer electrolyte membrane containing carboxyl groups is composed of a polymer matrix, lithium salt and carboxyl group-containing polymer. It is prepared by solution casting method, and the electrode structural integrity is improved by hydrogen bonds, strong ion-dipole interactions and chemical bonds. The contact between the electrode and the current collector reduces the interface impedance.
It improves the ionic conductivity, electrochemical window width and mechanical strength of the solid electrolyte, enhances the battery circulation performance, reduces the internal resistance of electrode polarization, adapts to the volume expansion of silicon material, and improves the energy density and stability of the battery.
Smart Images

Figure BDA0005021217700000111 
Figure BDA0005021217700000131 
Figure HDA0005021217710000011
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of energy storage materials and solid-state lithium-ion batteries, and specifically relates to a solid polymer electrolyte membrane for silicon-based all-solid-state batteries, and a preparation method and application thereof. Background Art
[0002] In recent years, in order to meet the rapid development of electric vehicles, portable electronic devices and grid energy storage, higher requirements have been placed on the energy density and safety of rechargeable lithium batteries. In this context, all-solid-state lithium batteries (ASSLBs) have attracted widespread attention due to their great potential in improving energy density and safety.
[0003] Since Wright and others began to pay attention to solid polymer electrolytes (SPEs), they have become one of the key materials for the development of ASSLBs. Studies have found that complexes of polyethylene oxide (PEO) and alkali metal salts show excellent performance in ion transport. A lot of research has been carried out to improve the ionic conductivity, electrochemical window and thermal stability of SPEs, involving polymer blending, cross-linked polymer matrix, plasticizer incorporation, ionic liquid impregnation, inorganic filler doping and other methods. In the application field of lithium batteries, although great progress has been made, the key challenge facing SPEs is the growth of lithium dendrites, which seriously hinders the widespread application of SPEs in high-performance lithium batteries. In contrast, the Si negative electrode has the highest theoretical capacity (4200mAh g -1 , lithiation forms Li 4.4 Si alloys) are considered to be more promising negative electrode materials. In the case of using Si negative electrodes, the problem of lithium dendrite growth is significantly reduced, thus overcoming this limitation to a certain extent.
[0004] For silicon-based all-solid-state batteries, interface issues are one of the key factors that restrict their performance improvement and commercial application. Studies have found that stress has a great influence on the properties of solid-state batteries. Piper and others from the Lee team systematically studied the effect of external stress on the performance of sulfide all-solid-state batteries. By increasing the pressure from 3MPa to 230MPa, the battery capacity decreased, the charging platform disappeared, the lithium insertion potential decreased, and the battery cycle stability was enhanced. Yamamoto and others believe that there is an extreme value for the battery capacity to change with the applied pressure. When the applied pressure is less than the critical pressure, increasing the applied pressure can effectively optimize the electrical contact inside the electrode and give full play to the capacity of the active material; when the critical pressure is exceeded, the increased external pressure excessively restricts the volume expansion of Si and aggravates the pulverization of Si particles. Although a certain external pressure can maintain the stable cycle of the battery, it will be achieved by sacrificing part of the total capacity.
[0005] In order to better solve the interface problem, we use functional group modification technology to effectively maintain the integrity of the electrode structure, maintain the contact between the inside of the electrode and the electrode and the current collector, reduce the interface impedance, and maintain the stable cycle of the battery through the solid electrolyte membrane with polar groups such as -COOH and -OH and the Si particles in the form of hydrogen bonds, strong ion-dipole interactions, or even chemical bonds. Therefore, the present invention needs to prepare a new type of solid polymer electrolyte to solve the above problems. Summary of the invention
[0006] In order to solve the technical problems of large solid / solid interface impedance between solid electrolyte and electrode in silicon-based all-solid-state batteries, poor cycle stability of silicon materials, and complex preparation method of solid electrolyte membrane, the present invention provides a solid polymer electrolyte membrane for silicon-based all-solid-state batteries, and its preparation method and application.
[0007] In order to solve the above technical problems, the present invention adopts the following technical solutions:
[0008] In a first aspect, the present invention provides a solid polymer electrolyte membrane for a silicon-based all-solid-state battery, comprising a polymer matrix, a lithium salt and an additive, wherein the additive is a carboxyl-containing polymer.
[0009] Preferably, the solid polymer electrolyte membrane for silicon-based all-solid-state batteries consists of a polymer matrix, a lithium salt and additives.
[0010] Preferably, the polymer matrix is polypropylene carbonate (PPC), polyethylene oxide (PEO) or polyvinylidene fluoride (PVDF).
[0011] Preferably, the lithium salt is lithium bis(trifluoromethanesulfonyl)imide (LiTFSI) or lithium perchlorate (LiClO4).
[0012] Preferably, the carboxyl-containing polymer is polyacrylic acid (PAA), sodium alginate (SA) or carboxymethyl cellulose (CMC), and the mass percentage content of the carboxyl-containing polymer in the solid polymer electrolyte membrane is 2-10%. More preferably, the carboxyl-containing polymer is PAA, and the mass percentage content of the carboxyl-containing polymer in the solid polymer electrolyte membrane is 10%.
[0013] As further preferred, the polymer matrix is PPC, PEO or PVDF, the carboxyl-containing polymer is PAA, and the lithium salt is lithium bistrifluoromethanesulfonyl imide (LiTFSI) or lithium perchlorate (LiClO4).
[0014] Preferably, in the solid polymer electrolyte membrane, the mass ratio of the polymer matrix to the lithium salt is 2-3:1.
[0015] In a second aspect, the present invention provides a method for preparing a solid polymer electrolyte membrane for a silicon-based all-solid-state battery according to the first aspect, comprising the following steps:
[0016] (1) dissolving the polymer matrix, the carboxyl group-containing polymer and the lithium salt in a solvent (), and stirring magnetically at room temperature until the solution is uniform;
[0017] (2) Casting the solution obtained in step (1) into a polytetrafluoroethylene mold, evaporating it in a forced air oven for 8-12 hours, then evaporating it in a vacuum oven for 8-12 hours, and then placing it in a glove box under an argon atmosphere for more than 24 hours to volatilize the residual solvent, thereby obtaining a solid polymer electrolyte membrane.
[0018] Preferably, the solvent is N,N-dimethylformamide (DMF) or deionized water (H2O).
[0019] Preferably, in step (1), the mass amount of the solvent is 5-7 times the total mass of the polymer matrix, the carboxyl-containing polymer and the lithium salt.
[0020] Preferably, in step (2), the temperatures in the blast oven and the vacuum oven are set to 60-80° C., respectively, and the total evaporation time in the blast oven and the vacuum oven is 20-24 h.
[0021] Preferably, in step (3), the thickness of the solid polymer electrolyte membrane is 50-100 μm.
[0022] In a third aspect, the present invention provides an application of the solid polymer electrolyte membrane described in the first aspect in a silicon-based all-solid-state battery.
[0023] Compared with the prior art, the present invention has the following beneficial effects:
[0024] (1) The solid polymer electrolyte of the present invention has an ingenious design. The polymer matrix acts as a soft chain to provide elasticity; the carboxyl-containing polymer acts as a rigid chain to provide adhesion; by blending the two, the combination of rigid and soft polymer chains provides great flexibility and mechanical strength, which can adapt to the volume expansion of silicon and maintain the integrity of the electrode structure. The present invention can improve the ionic conductivity of the new solid polymer electrolyte by regulating the proportion of the carboxyl-containing polymer, that is, by changing the content of the additive, and can improve the electrochemical window width and increase the ion migration number.
[0025] (2) The method for preparing a solid polymer electrolyte proposed by the present invention is simple in process. The method adopts a solution casting method to prepare a new solid polymer electrolyte membrane, which can increase the flexibility of the membrane. In addition, DMF or H2O as a solvent can well dissolve the carboxyl-containing polymer additive to form a uniform solution, which can finally be dried to form a uniformly distributed solid polymer electrolyte membrane.
[0026] (3) The solid polymer electrolyte of the present invention is used for silicon-based all-solid-state batteries. The carboxyl-containing polymer in the polymer solid electrolyte serves as a binder and contains a large number of carboxyl groups, which can bind to the silicon oxide (SiO x ) and silanol (-Si-OH) and other groups form covalent bonds, which can effectively reduce the contact resistance of the electrode / electrolyte interface, and have a beneficial effect on reducing the battery polarization internal resistance and improving the battery cycle performance. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] Figure 1 : (a), (e), (f) are EIS test graphs of PPC, PPC-PAA (15%), and PPC-PAA (20%) prepared in Comparative Example 1, Comparative Example 2, and Comparative Example 3 at different temperatures; (b), (c), (d) are EIS test graphs of PPC-PAA (2%), PPC-PAA (5%), and PPC-PAA (10%) prepared in Example 1, Example 2, and Example 3 at different temperatures.
[0028] Figure 2 : (a), (e), (f) are LSV test graphs of PPC, PPC-PAA (15%), and PPC-PAA (20%) prepared in Comparative Example 1, Comparative Example 2, and Comparative Example 3 at different temperatures; (b), (c), (d) are LSV test graphs of PPC-PAA (2%), PPC-PAA (5%), and PPC-PAA (10%) prepared in Example 1, Example 2, and Example 3 at different temperatures.
[0029] Figure 3 : (a) and (b) are the DC polarization curves of PPC and PPC-PAA (10%) prepared in Comparative Example 1 and Example 3 at room temperature and the impedance diagrams before and after polarization, respectively.
[0030] Figure 4 : Cycling performance diagram of lithium symmetric batteries assembled with PPC and PPC-PAA (10%) prepared in Comparative Example 1 and Example 3.
[0031] Figure 5: (a) and (b) are the cycle performance diagrams of Li / PPC / Si and Li / PPC-PAA (10%) / Si batteries assembled with PPC and PPC-PAA (10%) prepared in Comparative Example 1 and Example 3, respectively.
[0032] Figure 6 : Cycling performance diagram of LFP / PPC / Si and LFP / PPC-PAA (10%) / Si batteries assembled with PPC and PPC-PAA (10%) prepared in Comparative Example 1 and Example 3.
[0033] Figure 7 : (a) is the EIS test graph of PEO prepared in Example 4 at different temperatures; (b) and (c) are the EIS test graphs of PEO-SA (10%) and PEO-CMC (10%) prepared in Example 5 and Example 6 at different temperatures.
[0034] Figure 8 : (a) is the LSV test graph of PEO prepared in Example 4 at different temperatures; (b) and (c) are the LSV test graphs of PEO-SA (10%) and PEO-CMC (10%) prepared in Example 5 and Example 6 at different temperatures. DETAILED DESCRIPTION
[0035] The present invention is further described in detail below in conjunction with specific implementation methods. The protection scope of the present invention includes but is not limited to the following implementation cases.
[0036] If no specific conditions are specified in the examples of the present invention, the experiments were carried out under conventional conditions or conditions recommended by the manufacturer. If no manufacturer is specified for the reagents or instruments used, they are all conventional products that can be obtained by conventional technical means or purchased commercially.
[0037] The present invention will be further described below by means of specific examples.
[0038] In the embodiment of the present invention, PPC, molecular weight: 50,000; PAA, molecular weight: 450,000; PEO, molecular weight: 60,000; sodium alginate, molecular weight: 400,000; CMC, molecular weight: 250,000; PVDF, molecular weight: 400,000.
[0039] Embodiment 1:
[0040] (1) 1 g of polypropylene carbonate (PPC), 0.028 g of polyacrylic acid (PAA), and 0.35 g of lithium bis(trifluoromethanesulfonyl)imide (LiTFSI) were dissolved in 10 mL of dimethylformamide (DMF) and magnetically stirred at room temperature for 12 h until a uniform solution was formed;
[0041] (2) The solution obtained in (1) was cast into a polytetrafluoroethylene mold, first evaporated in an 80°C forced air oven for 12 h, and then evaporated in an 80°C vacuum oven for 12 h.
[0042] (3) The membrane obtained in (2) was placed in a glove box (under argon atmosphere) for more than 24 hours to volatilize the residual solvent, thereby obtaining a PPC-PAA (2%) solid electrolyte membrane with a thickness of 50-100 μm.
[0043] Embodiment 2:
[0044] (1) 1 g of polypropylene carbonate (PPC), 0.071 g of polyacrylic acid (PAA), and 0.35 g of lithium bis(trifluoromethanesulfonyl)imide (LiTFSI) were dissolved in 10 mL of dimethylformamide (DMF) and magnetically stirred at room temperature for 12 h until a uniform solution was formed;
[0045] (2) The solution obtained in (1) was cast into a polytetrafluoroethylene mold, first evaporated in an 80°C forced air oven for 12 h, and then evaporated in an 80°C vacuum oven for 12 h.
[0046] (3) The membrane obtained in (2) was placed in a glove box (under argon atmosphere) for more than 24 hours to volatilize the residual solvent, thereby obtaining a PPC-PAA (5%) solid electrolyte membrane with a thickness of 50-100 μm.
[0047] Embodiment 3:
[0048] (1) 1 g of polypropylene carbonate (PPC), 0.15 g of polyacrylic acid (PAA), and 0.35 g of lithium bis(trifluoromethanesulfonyl)imide (LiTFSI) were dissolved in 10 mL of dimethylformamide (DMF) and magnetically stirred at room temperature for 12 h until a uniform solution was formed;
[0049] (2) The solution obtained in (1) was cast into a polytetrafluoroethylene mold, first evaporated in an 80°C forced air oven for 12 h, and then evaporated in an 80°C vacuum oven for 12 h.
[0050] (3) The membrane obtained in (2) was placed in a glove box (under argon atmosphere) for more than 24 hours to volatilize the residual solvent, thereby obtaining a PPC-PAA (10%) solid electrolyte membrane with a thickness of 50-100 μm.
[0051] Embodiment 4:
[0052] (1) 0.6 g polyethylene oxide (PEO), 0.091 g polyacrylic acid (PAA) and 0.2175 g lithium bis(trifluoromethanesulfonyl)imide (LiTFSI) were dissolved in 15 mL dimethylformamide (DMF) and magnetically stirred at room temperature for 12 h until a uniform solution was formed;
[0053] (2) The solution obtained in (1) was cast into a polytetrafluoroethylene mold, first evaporated in a 60°C forced air oven for 12 h, and then evaporated in a 60°C vacuum oven for 12 h.
[0054] (3) The membrane obtained in (2) was placed in a glove box (under argon atmosphere) for more than 24 hours to volatilize the residual solvent, thereby obtaining a PEO-PAA (10%) solid electrolyte membrane with a thickness of 50-100 μm.
[0055] Embodiment 5:
[0056] (1) 0.6 g polyethylene oxide (PEO), 0.091 g sodium alginate (SA), and 0.2175 g lithium bis(trifluoromethanesulfonyl)imide (LiTFSI) were dissolved in 15 mL deionized water (H2O) and magnetically stirred at room temperature for 12 h until a uniform solution was formed;
[0057] (2) The solution obtained in (1) was cast into a polytetrafluoroethylene mold, first evaporated in a 60°C forced air oven for 8 h, and then evaporated in a 60°C vacuum oven for 12 h.
[0058] (3) The film obtained in (2) was placed in a glove box (under argon atmosphere) for more than 12 hours to volatilize the residual solvent, thereby obtaining a PEO-SA (10%) solid electrolyte membrane with a thickness of 50-100 μm.
[0059] Embodiment 6:
[0060] (1) 0.6 g polyethylene oxide (PEO), 0.091 g carboxymethyl cellulose (CMC), and 0.2175 g lithium bis(trifluoromethanesulfonyl)imide (LiTFSI) were dissolved in 15 mL deionized water (H2O) and magnetically stirred at room temperature for 12 h until a uniform solution was formed;
[0061] (2) The solution obtained in (1) was cast into a polytetrafluoroethylene mold, first evaporated in a 60°C forced air oven for 8 h, and then evaporated in a 60°C vacuum oven for 12 h.
[0062] (3) The membrane obtained in (2) was placed in a glove box (under argon atmosphere) for more than 12 hours to volatilize the residual solvent, thereby obtaining a PEO-CMC (10%) solid electrolyte membrane with a thickness of 50-100 μm.
[0063] Embodiment 7:
[0064] (1) 0.6 g polyvinylidene fluoride (PVDF), 0.1 g polyacrylic acid (PAA) and 0.3 g lithium perchlorate (LiClO4) were dissolved in 12 mL dimethylformamide (DMF) and magnetically stirred at room temperature for 12 h until a uniform solution was formed;
[0065] (2) The solution obtained in (1) was cast into a polytetrafluoroethylene mold, first evaporated in an 80°C forced air oven for 12 h, and then evaporated in an 80°C vacuum oven for 12 h.
[0066] (3) The membrane obtained in (2) was placed in a glove box (under argon atmosphere) for more than 24 hours to volatilize the residual solvent, thereby obtaining a PVDF-PAA (10%) solid electrolyte membrane with a thickness of 50-100 μm.
[0067] In order to further illustrate the key points of the present invention, comparative examples are added for illustration.
[0068] Comparative Example 1 (Compared with Example 1, Example 2, and Example 3):
[0069] (1) 1 g of polypropylene carbonate (PPC) and 0.35 g of lithium bis(trifluoromethanesulfonyl)imide (LiTFSI) were dissolved in 10 mL of dimethylformamide (DMF) and magnetically stirred at room temperature for 12 h until a uniform solution was formed;
[0070] (2) The solution obtained in (1) was cast into a polytetrafluoroethylene mold, first evaporated in a forced air oven at 80°C for 12 h, and then evaporated in a vacuum oven at 80°C for 12 h.
[0071] (3) The film obtained in (2) was placed in a glove box (under argon atmosphere) for more than 24 hours to volatilize the residual solvent, thereby obtaining a PPC solid electrolyte membrane with a thickness of 50-100 μm.
[0072] Comparative Example 2 (Compared with Example 1, Example 2, and Example 3):
[0073] (1) 1 g of polypropylene carbonate (PPC), 0.238 g of polyacrylic acid (PAA), and 0.35 g of lithium bis(trifluoromethanesulfonyl)imide (LiTFSI) were dissolved in 10 mL of dimethylformamide (DMF) and magnetically stirred at room temperature for 12 h until a uniform solution was formed;
[0074] (2) The solution obtained in (1) was cast into a polytetrafluoroethylene mold, first evaporated in a forced air oven at 80°C for 12 h, and then evaporated in a vacuum oven at 80°C for 12 h.
[0075] (3) The membrane obtained in (2) was placed in a glove box (under argon atmosphere) for more than 24 hours to volatilize the residual solvent, thereby obtaining a PPC-PAA (15%) solid electrolyte membrane with a thickness of 50-100 μm.
[0076] Comparative Example 3 (Compared with Example 1, Example 2, and Example 3):
[0077] (1) 1 g of polypropylene carbonate (PPC), 0.34 g of polyacrylic acid (PAA), and 0.35 g of lithium bis(trifluoromethanesulfonyl)imide (LiTFSI) were dissolved in 10 mL of dimethylformamide (DMF) and magnetically stirred at room temperature for 12 h until a uniform solution was formed;
[0078] (2) The solution obtained in (1) was cast into a polytetrafluoroethylene mold, first evaporated in a forced air oven at 80°C for 12 h, and then evaporated in a vacuum oven at 80°C for 12 h.
[0079] (3) The membrane obtained in (2) was placed in a glove box (under argon atmosphere) for more than 24 hours to volatilize the residual solvent, thereby obtaining a PPC-PAA (20%) solid electrolyte membrane with a thickness of 50-100 μm.
[0080] Comparative Example 4:
[0081] (1) 0.6 g of polyethylene oxide (PEO) and 0.2175 g of lithium bis(trifluoromethanesulfonyl)imide (LiTFSI) were dissolved in 15 mL of deionized water (H2O) and magnetically stirred at room temperature for 12 h until a uniform solution was formed;
[0082] (2) The solution obtained in (1) was cast into a polytetrafluoroethylene mold, first evaporated in a 60°C forced air oven for 8 h, and then evaporated in a 60°C vacuum oven for 12 h.
[0083] (3) The film obtained in (2) was placed in a glove box (under argon atmosphere) for more than 12 hours to volatilize the residual solvent, thereby obtaining a PEO solid electrolyte membrane with a thickness of 50-100 μm.
[0084] Comparative Example 5:
[0085] (1) 0.6 g of polyvinylidene fluoride (PVDF) and 0.3 g of lithium perchlorate (LiClO4) were dissolved in 12 mL of dimethylformamide (DMF) and magnetically stirred at room temperature for 12 h until a uniform solution was formed;
[0086] (2) The solution obtained in (1) was cast into a polytetrafluoroethylene mold, first evaporated in an 80°C forced air oven for 12 h, and then evaporated in an 80°C vacuum oven for 12 h.
[0087] (3) The membrane obtained in (2) was placed in a glove box (under argon atmosphere) for more than 24 hours to volatilize the residual solvent, thereby obtaining a PVDF solid electrolyte membrane with a thickness of 50-100 μm.
[0088] The solid electrolyte membranes prepared in the examples and comparative examples were cut into discs with a diameter of 19 mm, and subjected to EIS and LSV tests by an electrochemical workstation (model: ivium-N-stat of the Netherlands), respectively testing the ionic conductivity and electrochemical window at different temperatures. In the EIS test, the assembled battery was a steel sheet / electrolyte / steel sheet blocking battery (SS / / SS), and the battery was assembled from bottom to top in the order of negative electrode shell, shrapnel, stainless steel gasket, electrolyte, stainless steel gasket, and positive electrode shell; in the LSV test, the assembled battery was a lithium sheet / electrolyte / steel sheet button battery (Li / / SS), and the battery was assembled from bottom to top in the order of negative electrode shell, shrapnel, lithium sheet, electrolyte, stainless steel gasket, and positive electrode shell.
[0089] The EIS test can obtain the equivalent internal resistance of the solid electrolyte membrane, and then calculate the conductivity of the solid electrolyte membrane in each embodiment and comparative example by the formula:
[0090]
[0091] Where L is the thickness of the membrane, R is the membrane bulk resistance, and S is the effective contact area between the electrolyte and the stainless steel sheet.
[0092] The electrochemical window can be directly read out from the LSV test curve.
[0093] After analysis, we can find that Figure 1 In (a), when the PAA ratio is 0, the calculated room temperature ionic conductivity is 7.855×10 -7 S / cm; Figure 1 In (b), when the PAA content is 2%, the calculated room temperature ionic conductivity is 1.467×10 -6 S / cm; Figure 1 In (c), when the PAA content is 5%, the calculated room temperature ionic conductivity is 1.646×10 -6 S / cm; Figure 1 In (d), when the PAA content is 10%, the calculated room temperature ionic conductivity is 1.715×10 -6 S / cm; Figure 1 In (e), when the PAA content is 15%, the calculated room temperature ionic conductivity is 2.727×10 -7 S / cm. Figure 1 In (f), when the PAA content is 20%, the calculated room temperature ionic conductivity is 3.915×10 -7 S / cm. Figure 1As shown in the figure, the room temperature ionic conductivity of the solid electrolyte membrane was improved by the introduction of PAA. The conductivity increased first and then decreased with the increase of PAA. When the PAA content was 0.15 g, the room temperature ionic conductivity was as high as 1.715×10 -6 S / cm, which is 10 times higher than the room temperature ionic conductivity of PPC-based solid electrolytes. -8 ~10 -6 S / cm, meeting the application requirements. Figure 7 In (a), when SA or CMC is not added to the traditional PEO membrane, the calculated room temperature ionic conductivity is 1.161×10 -6 S / cm; Figure 7 In (b), when the SA content is 10%, the calculated room temperature ionic conductivity is 1.445×10 -6 S / cm; Figure 7 In (c), when the CMC content is 10%, the calculated room temperature ionic conductivity is 1.274×10 -6 S / cm. Figure 7 As shown in Figure 2, after the introduction of CMC and SA, the room temperature ionic conductivity of the prepared solid electrolyte membrane has been improved, which is 10 higher than that of the PEO-based solid electrolyte. -7 ~10 -6 S / cm, which meets the application requirements. In summary, the introduction of carboxyl functional groups into polymers can affect the microstructure of polymers, optimize the ion transmission path, thereby promoting the dissociation of electrolyte salts, increasing the number of freely moving ions, reducing the ion transmission resistance in polymers, and thus improving conductivity.
[0094] After analysis, we can find that Figure 2 In (a), when the PAA ratio is 0, the electrochemical window is 4.60 V; Figure 2 In (b), when the PAA content is 2%, the electrochemical window is 4.63V; Figure 2 In (c), when the PAA content is 5%, the electrochemical window is 4.74V; Figure 2 In (d), when the PAA content is 10%, the electrochemical window is 4.94V; Figure 2 In (e), when the PAA content is 15%, the electrochemical window is 4.49V; Figure 2 In (f), when the PAA content is 20%, the electrochemical window is 4.38 V. Therefore, when the PAA content is appropriately changed, the electrochemical window of the solid electrolyte membrane is also improved, and its law is basically consistent with the change of room temperature ionic conductivity. When the PAA content is 0.15g, the electrochemical window can be stabilized at about 5V, which has a certain application space.
[0095] After analysis, we can find that Figure 8 In (a), at room temperature, when SA or CMC is not added to the conventional PEO membrane, the decomposition potential of the PEO solid electrolyte membrane is 4.49 V (vs. Li + / Li), indicating that the electrolyte begins to oxidize. Figure 8 In (b), when the SA content is 10%, the electrochemical window is 5.02V; Figure 8 In (c), when the CMC accounts for 10%, the electrochemical window is 4.76V. At room temperature, the introduction of a certain amount of SA or CMC can improve the stable potential of the electrolyte membrane. Since the charge and discharge test range of lithium-ion batteries is generally around 3.0-4.5V, the wider the stable voltage range in which the electrolyte does not decompose, the longer the battery can work stably and the higher the positive electrode material, the higher the battery energy density can be.
[0096] The solid electrolyte membranes prepared in Example 3 and Comparative Example 1 were cut into discs with a diameter of 19 mm. The assembled battery was a lithium sheet / electrolyte / lithium sheet symmetrical battery (Li / / Li). The battery was assembled from bottom to top in the order of negative electrode shell, spring sheet, lithium sheet, electrolyte, lithium sheet, and positive electrode shell. EIS and CA tests were performed on the electrochemical workstation to test the lithium ion migration number at room temperature.
[0097] The ion migration number of the solid electrolyte membrane in each of Example 3 and Comparative Example 1 is calculated by the formula:
[0098]
[0099] Where I0 and R0 are the initial current and impedance before polarization, respectively. ss , R ss are the steady-state current and impedance after polarization, and V is the applied step voltage of 10 mV.
[0100] After analysis, we can find that Figure 3 In (a), when the PAA ratio is 0, the ion migration number of the solid electrolyte membrane is is 0.269; Figure 3 In (b), when the PAA content is 10%, the ion migration number of the solid electrolyte membrane is It is 0.489.
[0101] According to the test results, the performance of the PPC-PAA solid electrolyte membrane made by the present invention is consistent with the theory, and when the PAA accounts for 10%, its room temperature ion conductivity is the highest, the electrochemical window is the widest, the ion migration number is significantly improved, and the performance is optimal. In the range of 2% to 10% of PAA, it has high conductivity, wide electrochemical window and high ion migration number, and is widely used in lithium-ion batteries.
[0102] The solid electrolyte membranes prepared in Example 3 and Comparative Example 1 were cut into discs with a diameter of 19 mm. The assembled battery was a lithium sheet / electrolyte / lithium sheet symmetrical battery. The battery was assembled from bottom to top in the order of negative electrode shell, spring sheet, lithium sheet, electrolyte, lithium sheet, and positive electrode shell. The interface stability between the electrolyte and the lithium metal negative electrode was evaluated by testing it using a CT2001A battery testing system. The specific process of the test: Under normal temperature conditions, the symmetrical lithium battery was subjected to lithium deposition / stripping for 0.5 h each at a constant current density, and the test time was 1000 h.
[0103] After analysis, we can find that Figure 4 When the PAA content is 10%, the Li / PPC-PAA (10%) / Li battery can maintain a stable polarization voltage of about 0.1V and cycle for 1000h without short circuit. The significant improvement in electrode kinetics and lithium metal stability after adding PAA not only increases the lithium ion migration number, but also makes the interface properties between the electrolyte and lithium more stable.
[0104] The solid electrolyte membranes prepared in Example 3 and Comparative Example 1 were cut into discs with a diameter of 19 mm and tested using a CT2001A battery testing system. Half-cell constant current charge and discharge test: The assembled battery is a lithium sheet / electrolyte / Si button cell, and the battery is assembled from bottom to top in the order of negative electrode shell, shrapnel, lithium sheet, electrolyte, silicon pole piece, and positive electrode shell. Li / PPC / Si and Li / PPC-PAA (10%) / Si were subjected to long cycle tests at room temperature and 0.1C rate conditions, respectively. Full-cell constant current charge and discharge test: The assembled battery is a Si / electrolyte / LFP button cell, and the battery is assembled from bottom to top in the order of negative electrode shell, shrapnel, silicon pole piece, electrolyte, lithium iron phosphate pole piece, and positive electrode shell. LFP / PPC / Si and LFP / PPC-PAA (10%) / Si were subjected to long cycle tests at room temperature and 0.2C rate conditions, respectively.
[0105] After analysis, we can find that Figure 5 In (a), when the PAA ratio is 0, the discharge capacity of the Li / PPC / Si battery is only 873 mAh g after 300 cycles. -1 . Figure 5 In (b), when the PAA content is 10%, the discharge capacity of the Li / PPC-PAA (10%) / Si battery is stable at about 1445.8 mAh g after 350 cycles. -1 . Figure 6 When the PAA ratio is 0, the discharge capacity of the LFP / PPC / Si battery is only 121.2 mAh g after 50 cycles. -1When the PAA content is 10%, the discharge capacity of the LFP / PPC-PAA (10%) / Si battery is stable at about 133 mAh g after 50 cycles. -1 The PAA in the polymer solid electrolyte contains a large number of carboxyl groups, which can react with the silicon oxide (SiO x ) and silanol (-Si-OH) and other groups form covalent bonds, effectively reducing the contact resistance of the electrode / electrolyte interface, which has a beneficial effect on reducing the battery polarization internal resistance and improving the battery cycle performance.
Claims
1. A solid polymer electrolyte membrane for silicon-based all-solid-state batteries, Features: The solid polymer electrolyte membrane for silicon-based all-solid-state batteries comprises a polymer matrix, a lithium salt and an additive, wherein the additive is a carboxyl-containing polymer.
2. The solid polymer electrolyte membrane for silicon-based all-solid-state batteries according to claim 1, Features: The solid polymer electrolyte membrane for silicon-based all-solid-state batteries consists of a polymer matrix, a lithium salt and an additive.
3. The solid polymer electrolyte membrane for silicon-based all-solid-state batteries according to claim 1 or 2, Features: The polymer matrix is polypropylene carbonate, polyethylene oxide or polyvinylidene fluoride.
4. The solid polymer electrolyte membrane for silicon-based all-solid-state batteries according to claim 1 or 2, Features: The lithium salt is lithium bis(trifluoromethanesulfonyl)imide or lithium perchlorate.
5. The solid polymer electrolyte membrane for silicon-based all-solid-state batteries according to claim 1 or 2, Features: The carboxyl-containing polymer is polyacrylic acid, sodium alginate or carboxymethyl cellulose, and the mass percentage content of the carboxyl-containing polymer in the solid polymer electrolyte membrane is 2-10%.
6. The solid polymer electrolyte membrane for silicon-based all-solid-state batteries according to claim 5, Features: The carboxyl-containing polymer is polyacrylic acid, and the mass percentage content of the carboxyl-containing polymer in the solid polymer electrolyte membrane is 10%.
7. The solid polymer electrolyte membrane for silicon-based all-solid-state batteries according to claim 1 or 2, Features: The polymer matrix is polypropylene carbonate, polyethylene oxide or polyvinylidene fluoride, the carboxyl-containing polymer is polyacrylic acid, and the lithium salt is lithium bis(trifluoromethanesulfonyl)imide or lithium perchlorate.
8. The solid polymer electrolyte membrane for silicon-based all-solid-state batteries according to claim 1 or 2, Features: In the solid polymer electrolyte membrane, the mass ratio of the polymer matrix to the lithium salt is 2-3:
1.
9. A method for preparing a solid polymer electrolyte membrane for a silicon-based all-solid-state battery as claimed in any one of claims 1 to 8, Features: The preparation method comprises the following steps: (1) dissolving the polymer matrix, the carboxyl group-containing polymer and the lithium salt in a solvent, and stirring magnetically at room temperature until the mixture is uniformly dissolved; (2) Casting the solution obtained in step (1) into a polytetrafluoroethylene mold, evaporating it in a forced air oven for 8-12 hours, then evaporating it in a vacuum oven for 8-12 hours, and then placing it in a glove box under an argon atmosphere for more than 24 hours to volatilize the residual solvent, thereby obtaining a solid polymer electrolyte membrane.
10. Use of the solid polymer electrolyte membrane according to any one of claims 1 to 8 in a silicon-based all-solid-state battery.
Citation Information
Cited By
Preparation method of high-safety soft package lithium battery
CN121416633A