Preparation method of cement-based energy storage device, power supply system and energy storage building
By treating carbon fiber or copper sheets and combining silicate with water-soluble salts, the performance of cement-based batteries is improved, solving the energy density, cost and safety challenges of cement-based batteries are solved, and efficient energy storage and Smart building applications.
Patent Information
- Application Number
- CN202411058752.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-02
- Publication Date
- 2024-11-26
- Estimated Expiration
- Not applicable · inactive patent
Smart Images

Figure CN119029326A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of cement-based batteries, and in particular to a preparation method of a cement-based energy storage device, a power supply system, and an energy storage building. Background Art
[0002] Cement-based electrochemical energy storage technology uses solid cement-based materials as battery electrolytes.
[0003] Cement-based materials can be made into energy storage devices to provide emergency power in the event of power outages in extreme weather, such as lighting and communications, and enhance the disaster recovery capacity of buildings in the event of power outages in disasters. On the other hand, the future development direction of buildings must be intelligent, giving buildings the ability to self-perceive and self-regulate. If cement-based materials can provide electrical energy, it means that more sensors can be buried inside concrete to solve its power supply problem.
[0004] Cement-based batteries are still in the research stage and there is still a need to improve performance. Summary of the invention
[0005] The main purpose of the present invention is to provide a method for preparing a cement-based energy storage device, aiming to improve the performance of the cement-based energy storage device.
[0006] To achieve the above-mentioned purpose, the present invention provides a method for preparing a cement-based energy storage device, wherein the cement-based energy storage device comprises:
[0007] A cathode electrode sheet connected to the positive electrode current collector;
[0008] An anode electrode sheet connected to a negative electrode current collector;
[0009] A cement-based electrolyte matrix, wherein the cement-based electrolyte matrix is disposed between the cathode electrode sheet and the anode electrode sheet, and the raw materials of the cement-based electrolyte matrix include silicate and water-soluble salt;
[0010] The positive electrode current collector includes carbon fiber, and the processing steps of the carbon fiber include:
[0011] A three-electrode system is prepared, wherein the carbon fiber is used as a working electrode, a platinum electrode is used as a counter electrode, and a Hg / HgO electrode is used as a reference electrode;
[0012] The three-electrode system is placed in a first electrolyte for cyclic voltammetry treatment. After the treatment, the three-electrode system is placed in a second electrolyte for cyclic voltammetry treatment until the measured current curve and voltage curve are stable;
[0013] Alternatively, the positive electrode current collector comprises a copper sheet, and the step of treating the copper sheet comprises: immersing the copper sheet in an acidic solution.
[0014] Optionally, at least one of the following conditions is met:
[0015] The first electrolyte and the second electrolyte include KOH solution;
[0016] The acidic solution includes a nitric acid solution.
[0017] In the present application, the first electrolyte and the second electrolyte used to treat the carbon fiber include KOH solution.
[0018] In the present application, the acidic solution used for treating the copper sheet includes a nitric acid solution.
[0019] Optionally, at least one of the following conditions is met:
[0020] The concentration of the first electrolyte is 4 mol / L, and the concentration of the second electrolyte is 2 mol / L;
[0021] The concentration of the nitric acid solution is 68%.
[0022] In the present application, the concentration of the first electrolyte is 4 mol / L, and the concentration of the second electrolyte is 2 mol / L.
[0023] In the present application, the concentration of the nitric acid solution is 68%.
[0024] Optionally, in the preparation of the three-electrode system, the carbon fiber is used as a working electrode, the platinum electrode is used as a counter electrode, and the Hg / HgO electrode is used as a reference electrode;
[0025] The step of placing the three-electrode system in a first electrolyte for cyclic voltammetry treatment, and after the treatment, placing the three-electrode system in a second electrolyte for cyclic voltammetry treatment until the measured current curve and voltage curve are stable comprises:
[0026] Cleaning carbon fiber;
[0027] A three-electrode system is constructed, wherein the carbon fiber is used as a working electrode, a platinum electrode is used as a counter electrode, and a Hg / HgO electrode is used as a reference electrode;
[0028] The three-electrode system is placed in a first electrolyte for cyclic voltammetry treatment, wherein the OpenCircuit pretreatment time in the cyclic voltammetry is 1000 s and the voltage is 100 mV / s. After the treatment, the three-electrode system is placed in a second electrolyte for cyclic voltammetry treatment, wherein the OpenCircuit pretreatment time in the cyclic voltammetry is 1000 s and the voltage is 100 mV / s, until the measured current curve and voltage curve are stable.
[0029] The process of treating carbon fiber includes cleaning the carbon fiber, building a three-electrode system, wherein the carbon fiber is used as a working electrode, a platinum electrode is used as a counter electrode, and a Hg / HgO electrode is used as a reference electrode; placing the three-electrode system in a first electrolyte for cyclic voltammetry treatment, wherein the OpenCircuit pretreatment time in the cyclic voltammetry is 1000s, and the voltage is 100mV / s; after the treatment, placing the three-electrode system in a second electrolyte for cyclic voltammetry treatment, wherein the OpenCircuit pretreatment time in the cyclic voltammetry is 1000s, and the voltage is 100mV / s, until the measured current curve and voltage curve are stable.
[0030] Optionally, at least one of the following conditions is met:
[0031] The mass ratio of the silicate to the water-soluble salt is 1:0.4;
[0032] The mass percentage of the water-soluble salt is 5%;
[0033] The water-soluble salt includes potassium hydroxide and / or sodium hydroxide;
[0034] The active material layer of the cathode electrode sheet includes silicate, water-soluble salt, and MnO2, and the anode electrode sheet includes a zinc sheet;
[0035] The cathode electrode sheet comprises a copper sheet, and the anode electrode sheet comprises a magnesium sheet;
[0036] The negative electrode current collector comprises any one of a zinc sheet, an AZ31 magnesium alloy, an AZ91 magnesium alloy, an 80-mesh AZ91 magnesium alloy mesh, an aluminum sheet, an aluminum mesh, an iron sheet, and an iron mesh;
[0037] The carbon fiber includes polyacrylonitrile-based carbon fiber or polyacrylonitrile-based carbon fiber mesh.
[0038] In the present application, the mass ratio of silicate to water-soluble salt is 1:0.4; the mass percentage of water-soluble salt is 5%; the water-soluble salt includes potassium hydroxide and / or sodium hydroxide; the active material layer of the cathode electrode includes silicate, water-soluble salt, MnO2, and the anode electrode includes a zinc sheet; the cathode electrode includes a copper sheet, and the anode electrode includes a magnesium sheet; the negative electrode collector includes any one of a zinc sheet, an AZ31 magnesium alloy, an AZ91 magnesium alloy, an 80 mesh AZ91 magnesium alloy mesh, an aluminum sheet, an aluminum mesh, an iron sheet, and an iron mesh; the carbon fiber includes a polyacrylonitrile-based carbon fiber or a polyacrylonitrile-based carbon fiber mesh.
[0039] Optionally, the active material layer of the cathode electrode includes silicate, water-soluble salt, and MnO2, and the mass ratio of the silicate to the water-soluble salt is 1:0.4. A corresponding mass of MnO2 is added to the active material layer of corresponding size, the corresponding size is 25mm×50mm×78mm, and the corresponding mass is 5g to 15g.
[0040] In the present application, the active material layer of the cathode electrode includes silicate, water-soluble salt, and MnO2, wherein the mass ratio of silicate to water-soluble salt is 1:0.4, and a corresponding mass of MnO2 is added to the active material layer of corresponding size. When the size of the active material layer is 25mm×50mm×78mm, the mass of MnO2 added therein is 5g to 15g.
[0041] Optionally, the cement-based energy storage device has a size of 50 mm×50 mm×78 mm.
[0042] The size of the cement-based energy storage device of the present application is 50 mm×50 mm×78 mm.
[0043] Optionally, the distance between the positive electrode current collector and the negative electrode current collector is 1 cm to 3 cm.
[0044] The present application also provides a power supply system, which includes a plurality of cement-based energy storage devices connected in series and / or in parallel, and the cement-based energy storage device is prepared by the method for preparing a cement-based energy storage device according to any one of claims 1 to 8.
[0045] The present application also provides an energy storage building, which includes a cement-based energy storage device prepared by the method for preparing a cement-based energy storage device.
[0046] The cement-based energy storage device includes a cathode electrode, an anode electrode, and a cement-based electrolyte matrix. The cathode electrode is connected to the positive electrode current collector, the anode electrode is connected to the negative electrode current collector, and a cement-based electrolyte matrix is provided between the cathode electrode and the anode electrode. The raw materials of the cement-based electrolyte matrix include silicate and water-soluble salt; wherein the positive electrode current collector includes carbon fiber, and the processing steps of the carbon fiber include: preparing a three-electrode system, wherein the carbon fiber is used as a working electrode, the platinum electrode is used as a counter electrode, and the Hg / HgO electrode is used as a reference electrode; placing the three-electrode system in a first electrolyte for cyclic voltammetry treatment, and after the treatment, placing the three-electrode system in a second electrolyte for cyclic voltammetry treatment until the measured current curve and voltage curve are stable; or, the positive electrode current collector includes a copper sheet, and the processing steps of the copper sheet include: soaking the copper sheet in an acidic solution. By treating the carbon fiber or the copper sheet, the efficiency of the contact between the carbon fiber or the copper sheet and the electrolyte, charge transfer, ion adsorption, electrode reaction and other processes can be improved, thereby improving the performance of the cement-based energy storage device. BRIEF DESCRIPTION OF THE DRAWINGS
[0047] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on the structures shown in these drawings without paying creative work.
[0048] Figure 1 A schematic flow chart of a method for preparing a cement-based energy storage device provided by the present invention;
[0049] Figure 2 A structural schematic diagram of a cement-based energy storage device provided by the present invention;
[0050] Figure 3 The voltage diagram of the battery discharge external circuit in Embodiments 1 to 3 of the present invention;
[0051] Figure 4 The voltage-time diagram of the external circuit of the battery discharge in Examples 4 to 6 of the present invention;
[0052] Figure 5 The voltage-time diagram of the external circuit of the battery discharge in Examples 7 to 9 of the present invention;
[0053] Figure 6 1 is a battery discharge voltage-time diagram in Examples 7, 8, 10 and 11 of the present invention.
[0054] Description of Figure Numbers:
[0055] 1. Cement-based electrolyte matrix; 2. Positive electrode current collector; 3. Negative electrode current collector.
[0056] The realization of the purpose, functional features and advantages of the present invention will be further explained in conjunction with embodiments and with reference to the accompanying drawings. DETAILED DESCRIPTION
[0057] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0058] It should be noted that if the embodiments of the present invention involve directional indications (such as up, down, left, right, front, back, etc.), the directional indications are only used to explain the relative position relationship, movement status, etc. between the components in a certain specific posture. If the specific posture changes, the directional indication will also change accordingly.
[0059] In addition, if there are descriptions involving "first", "second", etc. in the embodiments of the present invention, the descriptions of "first", "second", etc. are only used for descriptive purposes and cannot be understood as indicating or implying their relative importance or implicitly indicating the number of technical features indicated. Therefore, the features limited to "first" and "second" may explicitly or implicitly include at least one of the features. In addition, if "and / or" or "and / or" appears in the full text, its meaning includes three parallel solutions. Taking "A and / or B" as an example, it includes solution A, solution B, or solutions that satisfy both A and B. In addition, the technical solutions between the various embodiments can be combined with each other, but it must be based on the ability of ordinary technicians in this field to implement. When the combination of technical solutions is contradictory or cannot be implemented, it should be deemed that such combination of technical solutions does not exist and is not within the scope of protection required by the present invention.
[0060] It can be understood that a cement-based energy storage device is an electrochemical energy storage system that uses cement material as an electrolyte matrix. This type of energy storage device generally has the following basic components: Cathode: The cathode is the electrode where the reduction reaction occurs in the energy storage device. During the charging process, the cathode absorbs electrons; during the discharging process, the cathode releases electrons. Anode: The anode is the electrode where the oxidation reaction occurs in the energy storage device. During the charging process, the anode releases electrons; during the discharging process, the anode absorbs electrons. Positive current collector: The positive current collector is connected to the cathode, and its function is to transfer current from the external circuit to the cathode, and from the cathode back to the external circuit. Negative current collector: The negative current collector is connected to the anode, and its function is similar to the positive current collector, but in the opposite direction.
[0061] Cement-based electrolyte matrix: This is the core part of the energy storage device, which is located between the cathode and the anode. The cement-based electrolyte matrix not only physically isolates the cathode and anode to prevent them from directly contacting and causing a short circuit, but also provides a channel for ion transmission, allowing ions to move between the electrodes during charging and discharging. The working principle of cement-based energy storage devices is similar to that of traditional batteries, storing and releasing energy through the movement of ions between electrodes. The advantages of this energy storage device may include cost-effectiveness, environmental friendliness, and the use of traditional building materials (such as cement) to make the electrolyte matrix.
[0062] Cement-based electrochemical energy storage technology uses solid cement-based materials as the electrolyte of the battery. The basic idea of this application to develop cement-based energy storage technology includes adding materials that improve its electrical conductivity, such as short carbon fibers, carbon nanotubes, etc., to cement-based materials, so as to transform ordinary cement-based materials with low conductivity into electrolyte materials with good conductivity, thereby improving the efficiency of energy conversion. As an important building material, cement-based materials are characterized by large volume and wide distribution. Making them into energy storage devices can, on the one hand, reduce the cost of building electricity consumption. On the other hand, cement-based energy storage technology combined with urban community power resources can become an important supplement to power grid facilities.
[0063] Cement-based materials can be made into energy storage devices to provide emergency power in the event of power outages in extreme weather, such as meeting the needs of lighting and communications, and enhancing the disaster tolerance of buildings in the event of power outages due to disasters. On the other hand, the future development direction of buildings must be intelligent, giving buildings the ability to self-perceive and self-regulate. If cement-based materials can provide electrical energy, it means that more sensors can be buried inside the concrete to solve its power supply problem. For example, cement-based batteries power structural health monitoring sensors inside concrete. Cement-based batteries can also be combined with renewable energy such as solar panels to provide power for monitoring systems, LED lights, network connections, etc. inside and outside the building, enhancing the intelligence and practicality of the building. Cement-based batteries can provide cathodic protection for concrete infrastructure, prevent corrosion and cracks, extend the service life of the building, and reduce maintenance costs. Batteries made of concrete use existing materials and infrastructure, which can basically achieve zero pollution and avoid the problems of resource consumption and environmental pollution that are common in traditional batteries.
[0064] Cement-based batteries are still in the research stage, and some technical issues need to be resolved, such as improving energy density, reducing costs, enhancing safety, and extending life.
[0065] The present application provides a method for preparing a cement-based energy storage device, such as Figure 1 As shown, the cement-based energy storage device includes a cathode electrode piece, an anode electrode piece, and a cement-based electrolyte matrix 1, the cathode electrode piece is connected to the positive electrode collector 2, the anode electrode piece is connected to the negative electrode collector 2, and a cement-based electrolyte matrix 1 is arranged between the cathode electrode piece and the anode electrode piece, and the raw materials of the cement-based electrolyte matrix include silicate and water-soluble salt; wherein, the positive electrode collector includes carbon fiber, and the processing steps of the carbon fiber include: preparing a three-electrode system, wherein the carbon fiber is used as a working electrode, the platinum electrode is used as a counter electrode, and the Hg / HgO electrode is used as a reference electrode; placing the three-electrode system in a first electrolyte for cyclic voltammetry treatment, and after the treatment, placing the three-electrode system in a second electrolyte for cyclic voltammetry treatment until the measured current curve and voltage curve are stable; or, the positive electrode collector includes a copper sheet, and the processing steps of the copper sheet include: immersing the copper sheet in an acidic solution.
[0066] By processing carbon fibers or copper sheets, the efficiency of processes such as contact between carbon fibers or copper sheets and electrolytes, charge transfer, ion adsorption, and electrode reactions can be improved, thereby improving the performance of cement-based energy storage devices.
[0067] In one embodiment, at least one of the following conditions is met: the first electrolyte and the second electrolyte include KOH solution; and the acidic solution includes nitric acid solution.
[0068] In one embodiment, the first electrolyte and the second electrolyte for treating the carbon fiber include KOH solution. In one embodiment, the acid solution for treating the copper sheet includes nitric acid solution.
[0069] In one embodiment, at least one of the following conditions is met: the concentration of the first electrolyte is 4 mol / L, the concentration of the second electrolyte is 2 mol / L; and the concentration of the nitric acid solution is 68%.
[0070] In one embodiment, the concentration of the first electrolyte is 4 mol / L, and the concentration of the second electrolyte is 2 mol / L.
[0071] In one embodiment, the concentration of the nitric acid solution is 68%.
[0072] In one embodiment, in preparing a three-electrode system, wherein the carbon fiber is used as a working electrode, the platinum electrode is used as a counter electrode, and the Hg / HgO electrode is used as a reference electrode; placing the three-electrode system in a first electrolyte for cyclic voltammetry treatment, and after the treatment, placing the three-electrode system in a second electrolyte for cyclic voltammetry treatment until the measured current curve and voltage curve are stable, the steps include: cleaning the carbon fiber; building a three-electrode system, wherein the carbon fiber is used as a working electrode, the platinum electrode is used as a counter electrode, and the Hg / HgO electrode is used as a reference electrode; placing the three-electrode system in the first electrolyte for cyclic voltammetry treatment, the OpenCircuit pretreatment time in the cyclic voltammetry is 1000s, and the voltage is 100mV / s, and after the treatment, placing the three-electrode system in the second electrolyte for cyclic voltammetry treatment, the OpenCircuit pretreatment time in the cyclic voltammetry is 1000s, and the voltage is 100mV / s, until the measured current curve and voltage curve are stable.
[0073] That is, in the process of treating carbon fiber, including cleaning carbon fiber, building a three-electrode system, in which carbon fiber is used as a working electrode, a platinum electrode is used as a counter electrode, and a Hg / HgO electrode is used as a reference electrode; the three-electrode system is placed in a first electrolyte for cyclic voltammetry treatment, the OpenCircuit pretreatment time in the cyclic voltammetry is 1000s, and the voltage is 100mV / s. After the treatment, the three-electrode system is placed in a second electrolyte for cyclic voltammetry treatment, the OpenCircuit pretreatment time in the cyclic voltammetry is 1000s, and the voltage is 100mV / s, until the measured current curve and voltage curve are stable.
[0074] In one embodiment, at least one of the following conditions is met: the mass ratio of silicate to water-soluble salt is 1:0.4; the mass percentage of water-soluble salt is 5%; the water-soluble salt includes potassium hydroxide and / or sodium hydroxide; the active material layer of the cathode electrode includes silicate, water-soluble salt, MnO2, and the anode electrode includes a zinc sheet; the cathode electrode includes a copper sheet, and the anode electrode includes a magnesium sheet; the negative electrode current collector includes any one of zinc sheet, AZ31 magnesium alloy, AZ91 magnesium alloy, 80 mesh AZ91 magnesium alloy mesh, aluminum sheet, aluminum mesh, iron sheet, and iron mesh; the carbon fiber includes polyacrylonitrile-based carbon fiber or polyacrylonitrile-based carbon fiber mesh.
[0075] In one embodiment, the active material layer of the cathode electrode includes silicate, water-soluble salt, and MnO2, the mass ratio of silicate to water-soluble salt is 1:0.4, and a corresponding mass of MnO2 is added to the active material layer of corresponding size, the corresponding size is 25mm×50mm×78mm, and the corresponding mass is 5g to 15g.
[0076] That is, the active material layer of the cathode electrode includes silicate, water-soluble salt, and MnO2, wherein the mass ratio of silicate to water-soluble salt is 1:0.4, and a corresponding mass of MnO2 is added to the active material layer of corresponding size. When the size of the active material layer is 25mm×50mm×78mm, 5g to 15g of MnO2 is added therein.
[0077] In one embodiment, the size of the cement-based energy storage device is 50 mm×50 mm×78 mm.
[0078] In one embodiment, the distance between the positive current collector and the negative current collector is 1 cm to 3 cm. It is understandable that the electrode spacing refers to the distance between the positive and negative electrodes in the battery, that is, the distance between the positive current collector and the negative current collector. It is generally believed that the electrode spacing will affect the current density and current efficiency of the battery. In general, the smaller the electrode spacing, the higher the current density, the higher the current efficiency, and the better the performance of the battery. However, the electrode spacing cannot be too small, otherwise it will increase the internal resistance of the battery, resulting in a decrease in voltage, or even electrode breakdown, causing damage to the battery or potential safety hazards. Therefore, the choice of electrode spacing needs to strike a balance between battery performance and safety. In the present application, the distance between the positive current collector and the negative current collector includes 1 cm, 2 cm, and 3 cm.
[0079] The present application also provides a power supply system, which includes a plurality of cement-based energy storage devices connected in series and / or in parallel, and the cement-based energy storage device is prepared by the preparation method of the cement-based energy storage device as described above.
[0080] It is understandable that the organizational form of the battery structure refers to the internal structure of the battery and the collaborative working connection between the batteries, which has a great influence on the performance of the battery. On the one hand, it affects the energy density of the battery, because a reasonable organizational form can improve the utilization rate of the active materials inside the battery. On the other hand, it affects the life of the battery by affecting the aging mechanism of the battery.
[0081] Multiple cement-based energy storage devices can be connected in series or in parallel to form a power system to work together. Series connection can increase the voltage of the external circuit, and parallel connection can increase the current of the external circuit. Alternatively, parallel connection can be considered to increase the life of the battery without changing the voltage of the original battery system. By combining different numbers and types of batteries, specific voltage and higher power requirements can be met.
[0082] The present application also provides an energy storage building, which includes a cement-based energy storage device prepared by the preparation method of the cement-based energy storage device as described above.
[0083] It is understandable that carbon fiber has good performance as a current collector component of aluminum batteries, and on this basis, carbon fiber materials are further optimized. Carbon fiber is an inert material. Although it has a high electronic conductivity, its surface is flat and smooth, and there are few active sites, which is not conducive to the electrode reaction in the application of the battery. Therefore, it is necessary to increase the active sites on the surface of the carbon fiber through activation treatment to improve its electrochemical activity. The activation treatment of carbon fiber can increase the hydrophilicity, porosity, specific surface area, edge sites, functional groups, etc. on the surface of the carbon fiber material without reducing the electronic conductivity, thereby improving the efficiency of its contact with the electrolyte, charge transfer, ion adsorption, electrode reaction and other processes. In some embodiments, carbon fiber, as a current collector material for the battery, needs to undergo an oxidation reaction with the anions in the electrolyte to release electrons. Therefore, the introduction of oxygen atoms on the surface of carbon fiber can first increase the hydrophilicity of the fiber surface, which will be beneficial to the electron transfer between the interfaces. Secondly, the oxygen atoms on the surface of carbon fiber can also act as active sites to participate in the electrode reaction, which can effectively improve the utilization rate of the electrode.
[0084] In one embodiment, the specific steps of activating the carbon fiber are as follows:
[0085] Step 1: Weigh 11.2g and 22.4g of analytical pure KOH and 100mL of deionized water respectively to prepare 2mol / L and 4mol / L KOH solutions. Put the weighed analytical pure KOH into a larger beaker, add a small amount of deionized water, and stir with a glass rod to completely dissolve it. The solution obtained at this time is the KOH solution to be used in the electrochemical treatment. Step 2: Cut a carbon fiber mesh of 60mm×30mm×0.5mm as the object to be treated. First, rinse the surface of the carbon fiber mesh with deionized water until there are no obvious impurities on the surface, and then clean the surface of the carbon fiber mesh with anhydrous ethanol. After the treatment is completed, dry it for use. Step 3: Build the three-electrode system required for cyclic voltammetry, connect the working electrode to the carbon fiber mesh, use a platinum electrode as the counter electrode of the three-electrode system, use an Hg / HgO electrode as the reference electrode, and use the prepared 4mol / L potassium hydroxide solution as the solution. Treat the carbon fiber mesh according to a certain time and voltage. Step 4: Wash the electrochemically treated carbon fiber mesh thoroughly under flowing deionized water, and dry it for later use. Step 5: Place the dried carbon fiber mesh in a 2mol / LKOH solution and use a three-electrode system to perform cyclic voltammetry (CV) on it. The OpenCircuit pretreatment time in the cyclic voltammetry method is controlled at 1000s, and the voltage is controlled at 100mV / s. After that, use the same 100mV / s current to perform cyclic current treatment until the measured current-voltage curve is stable. Step 6: Take the carbon fiber mesh out of the solution, dry it and set it aside.
[0086] In one embodiment, the copper sheet is treated by directly placing the copper sheet in a 68% nitric acid solution for 20 seconds, then rinsing it with clean water and anhydrous ethanol, and drying it to obtain a copper current collector with a corroded surface.
[0087] In one embodiment, the dimensions of the positive electrode current collector and the negative electrode current collector are uniformly controlled to be 60 mm×30 mm×0.5 mm. The assembled battery is connected to a 10Ω resistor, and the current and voltage of the resistor are measured using an ammeter and a voltmeter with real-time data acquisition function.
[0088] Example
[0089] Example 1
[0090] Preparation of cement-based electrolyte matrix: Add KOH solution to sodium silicate material, perform curing and solidification in sequence to obtain cement-based electrolyte matrix. The mass ratio of sodium silicate to KOH solution is 1:0.4, and the mass concentration of KOH solution is 5%.
[0091] Preparation of cathode electrode sheet: KOH solution and MnO2 powder are added to the sodium silicate material, and the materials are cured and solidified in sequence to obtain a cathode electrode sheet matrix, wherein 5g MnO2 powder is added to a 25mm×50mm×78mm cathode electrode sheet matrix.
[0092] Among them, before curing, an anode electrode sheet (a high-purity zinc sheet with a purity greater than 99.99%) and a negative electrode current collector (zinc sheet) are inserted into a cement-based electrolyte matrix with a size of 25mm×50mm×78mm, and the negative electrode current collector is exposed outside the cement-based electrolyte matrix. A positive electrode current collector (copper sheet) is inserted into a cathode electrode sheet matrix with a size of 25mm×50mm×78mm, and the positive electrode current collector is exposed outside the cathode electrode sheet matrix.
[0093] The distance between the zinc sheet and the copper sheet is 1 cm. In the discharge experiment, a 10Ω resistor is set as the external circuit load. After the battery is made, let it stand until the cement-based material is finally set, and then measure the open circuit voltage of the battery. After the cement-based material is finally set, connect a 10Ω resistor load to the external circuit, discharge the battery continuously, and measure the voltage and current values of the external circuit.
[0094] Example 2
[0095] The method of this embodiment is the same as that of embodiment 1, except that the amount of MnO2 powder added is 10g.
[0096] Example 3
[0097] The method of this embodiment is the same as that of embodiment 1, except that the amount of MnO2 powder added is 15g.
[0098] Measuring the current and voltage of the battery's external circuit can provide information about the battery's current state. By observing changes in current and voltage, the battery's charge level, discharge state, and overall performance can be determined. There is a relationship between the battery's current and voltage and its capacity. By measuring the battery's current and voltage under a specific load, the battery's capacity, or the amount of electrical energy the battery can provide, can be estimated. Long-term current and voltage monitoring can be used to predict the life of the battery. The battery discharge external circuit voltage diagram with different MnO2 powder additions is shown in Figure 1. Figure 3 As shown, the external circuit voltage of the battery with 5g, 10g and 20g MnO2 powder added is mainly concentrated in the areas of 0.035mV, 0.095mV and 0.105mV, respectively.
[0099] Example 4
[0100] The method of this embodiment is similar to that of embodiment 1, except that no MnO2 powder is added, the cathode electrode is a copper sheet, the positive electrode current collector is a copper sheet, and the negative electrode current collector is an AZ31 magnesium alloy. The anode electrode is a magnesium sheet with a size of 60mm×30mm×0.5mm, and sandpaper is used to fully expose the active material inside the metal. In the experiment, a copper sheet was selected as the current collector unit. The anode electrode magnesium sheet and the cathode electrode copper sheet were inserted into the mixed cement-based electrolyte matrix with a spacing of 10mm.
[0101] Example 5
[0102] The method of this embodiment is the same as that of embodiment 4, except that the negative electrode current collector is AZ91 magnesium alloy.
[0103] Example 6
[0104] The method of this embodiment is the same as that of embodiment 4, except that the negative electrode current collector is an 80-mesh AZ91 magnesium alloy mesh.
[0105] The voltage-time diagram of the external circuit of magnesium alloy battery discharge is as follows Figure 4 As shown in the figure, the peak voltage and voltage level at the same discharge time of the AZ91 magnesium alloy sheet are higher than those of the AZ31 magnesium alloy sheet as the electrode material, but after 60 minutes of discharge, the final voltage levels of both tend to the same level, that is, below 0.6mV. Using the AZ91 magnesium alloy mesh as the electrode material, the peak voltage is always higher than that of the battery using the AZ91 alloy sheet as the electrode during the discharge period. Because the mesh metal electrode has a larger specific surface area, and the surface of the sheet magnesium alloy material is smoother and not easy to absorb charge, the use of mesh metal material as the electrode makes the peak voltage and discharge life higher.
[0106] Example 7
[0107] The method of the embodiment is similar to that of the embodiment 4, except that the negative electrode current collector is an aluminum sheet and a copper sheet is used as the positive electrode current collector.
[0108] Example 8
[0109] The method of this embodiment is the same as that of embodiment 7, except that polyacrylonitrile-based carbon fiber with a mesh size of 10 mm is used as the positive electrode current collector.
[0110] Example 9
[0111] The method of this embodiment is the same as that of embodiment 7, except that the negative electrode current collector is an aluminum mesh.
[0112] Aluminum electrode battery discharge external circuit voltage-time diagram Figure 4 As shown in the figure, the voltage of the battery external circuit is mainly concentrated in the range of 1.2 V to 1.4 V. The current and voltage peak values of the Al mesh-Cu sheet battery, Al sheet-C mesh, and Al sheet-Cu sheet battery and the voltage values in the same discharge time are decreasing in turn, which shows that the Al mesh has stronger electrochemical reaction performance than the Al sheet, and the carbon fiber mesh is more compatible with the electrolyte material than the copper sheet.
[0113] Example 10
[0114] The method of this embodiment is the same as that of embodiment 7, except that the positive electrode current collector is activated. Activation treatment method of copper sheet: directly put the copper sheet into 68% nitric acid solution for 20 seconds, then rinse with clean water and anhydrous ethanol, and dry to obtain a copper current collector with corroded surface.
[0115] Embodiment 11
[0116] The method of this embodiment is the same as that of Embodiment 8, except that the positive electrode current collector carbon fiber mesh is activated.
[0117] Carbon fiber has good performance as the current collector component of aluminum batteries, and on this basis, the carbon fiber material is further optimized. The specific processing steps are as follows:
[0118] The relative molecular mass of KOH is 56, so here we weigh 11.2g and 22.4g of analytical pure KOH and 100mL of deionized water respectively to prepare 2mol / L and 4mol / L KOH solutions. Put the weighed analytical pure KOH into a larger beaker, add a small amount of deionized water, and stir it with a glass rod to completely dissolve it. The solution obtained at this time is the KOH solution to be used in the electrochemical treatment. Cut a carbon fiber mesh of 60mm×30mm×0.5mm as the object to be treated. First, rinse the surface of the carbon fiber mesh with deionized water until there are no obvious impurities on the surface, and then clean the surface of the carbon fiber mesh with anhydrous ethanol. After the treatment is completed, dry it for use. Build the three-electrode system required for cyclic voltammetry, connect the working electrode to the carbon fiber mesh, use a platinum electrode as the counter electrode of the three-electrode system, use an Hg / HgO electrode as the reference electrode, and use a prepared 4mol / L potassium hydroxide solution as the solution. Treat the carbon fiber mesh according to a certain time and voltage. The electrochemically treated carbon fiber mesh was thoroughly cleaned under flowing deionized water and dried for later use. The dried carbon fiber mesh was placed in a 2mol / L KOH solution and subjected to cyclic voltammetry using a three-electrode system. The OpenCircuit pretreatment time in the cyclic voltammetry was controlled at 1000s and the voltage was controlled at 100mV / s. Afterwards, a cyclic current treatment was performed using a current of 100mV / s until the measured current-voltage curve was stable. The carbon fiber mesh was removed from the solution and dried for later use.
[0119] The battery discharge voltage-time diagram after copper sheet and carbon fiber treatment is as follows Figure 5 As shown. The voltage of the battery made after copper sheet and carbon fiber treatment is significantly higher than that of untreated materials. The surface of the material treated by electrochemical and chemical agents will change from smooth to rough, and the rougher surface will be more compatible with cement-based solid electrolyte. At the same time, the rough surface exposes more active sites, which is beneficial for the current collector to collect charges and provide charge exchange sites for active materials. The current collector element with surface treatment can enhance battery performance.
[0120] Example 12
[0121] The method of this embodiment is the same as that of Embodiment 7, except that a different current collector spacing is used in this embodiment.
[0122] The peak voltages of the electrode spacings of 1cm, 2cm, and 3cm are 95.36mV, 72.38mV, and 57.53mV, respectively, and the peak currents are 95.36mA, 72.38mA, and 57.53mA, respectively. It can be seen that the peak voltage and peak current decrease with the increase of the electrode spacing. The electrode spacing refers to the distance between the positive and negative electrodes in the battery. It is generally believed that the electrode spacing will affect the current density and current efficiency of the battery. Generally speaking, the smaller the electrode spacing, the higher the current density, the higher the current efficiency, and the better the performance of the battery. However, the electrode spacing cannot be too small, otherwise it will increase the internal resistance of the battery, resulting in a decrease in voltage, or even electrode breakdown, causing damage to the battery or safety hazards. Therefore, the choice of electrode spacing requires a balance between battery performance and safety.
[0123] Example 13
[0124] The method of this embodiment adopts the same battery solution as that of embodiment 7. Two cement-based energy storage devices are connected in series and two cement-based energy storage devices are connected in parallel.
[0125] The total voltage of parallel batteries is the same as the voltage of a single battery, and because the total capacity of the parallel circuit is increased, the circuit can provide a larger current without reducing the voltage. Compared with a single cement-based energy storage device, connecting batteries in parallel increases the voltage of the load resistor. Batteries in parallel can improve the overall discharge performance of the power system. Series-parallel batteries can make multiple batteries form a power system to work together. Series connection can increase the voltage of the external circuit, parallel connection can increase the current of the external circuit, or it can be considered that parallel connection increases the life of the battery without changing the voltage of the original battery system. By combining different numbers and types of batteries, specific voltage and higher power requirements can be met.
[0126] The above are only exemplary embodiments of the present invention, and are not intended to limit the patent scope of the present invention. All equivalent structural changes made using the contents of the present invention's specification and drawings, or directly / indirectly applied in other related technical fields, are included in the patent protection scope of the present invention.
Claims
1. A method for preparing a cement-based energy storage device, It is characterized in that The cement-based energy storage device comprises: A cathode electrode sheet connected to the positive electrode current collector; An anode electrode sheet connected to a negative electrode current collector; A cement-based electrolyte matrix, wherein the cement-based electrolyte matrix is disposed between the cathode electrode sheet and the anode electrode sheet, and the raw materials of the cement-based electrolyte matrix include silicate and water-soluble salt; The positive electrode current collector includes carbon fiber, and the processing steps of the carbon fiber include: A three-electrode system is prepared, wherein the carbon fiber is used as a working electrode, a platinum electrode is used as a counter electrode, and a Hg / HgO electrode is used as a reference electrode; The three-electrode system is placed in a first electrolyte for cyclic voltammetry treatment. After the treatment, the three-electrode system is placed in a second electrolyte for cyclic voltammetry treatment until the measured current curve and voltage curve are stable; Alternatively, the positive electrode current collector comprises a copper sheet, and the step of treating the copper sheet comprises: immersing the copper sheet in an acidic solution.
2. The method for preparing the cement-based energy storage device according to claim 1, It is characterized in that Meet at least one of the following conditions: The first electrolyte and the second electrolyte include KOH solution; The acidic solution includes a nitric acid solution.
3. The method for preparing the cement-based energy storage device according to claim 2, It is characterized in that Meet at least one of the following conditions: The concentration of the first electrolyte is 4 mol / L, and the concentration of the second electrolyte is 2 mol / L; The concentration of the nitric acid solution is 68%.
4. The method for preparing the cement-based energy storage device according to claim 1, It is characterized in that In the preparation of the three-electrode system, the carbon fiber is used as a working electrode, the platinum electrode is used as a counter electrode, and the Hg / HgO electrode is used as a reference electrode; The step of placing the three-electrode system in a first electrolyte for cyclic voltammetry treatment, and after the treatment, placing the three-electrode system in a second electrolyte for cyclic voltammetry treatment until the measured current curve and voltage curve are stable comprises: Cleaning carbon fiber; A three-electrode system is constructed, wherein the carbon fiber is used as a working electrode, a platinum electrode is used as a counter electrode, and a Hg / HgO electrode is used as a reference electrode; The three-electrode system is placed in a first electrolyte for cyclic voltammetry treatment, wherein the OpenCircuit pretreatment time in the cyclic voltammetry is 1000 s and the voltage is 100 mV / s. After the treatment, the three-electrode system is placed in a second electrolyte for cyclic voltammetry treatment, wherein the OpenCircuit pretreatment time in the cyclic voltammetry is 1000 s and the voltage is 100 mV / s, until the measured current curve and voltage curve are stable.
5. The method for preparing a cement-based energy storage device according to any one of claims 1 to 4, It is characterized in that Meet at least one of the following conditions: The mass ratio of the silicate to the water-soluble salt is 1:0.4; The mass percentage of the water-soluble salt is 5%; The water-soluble salt includes potassium hydroxide and / or sodium hydroxide; The active material layer of the cathode plate includes silicate, water-soluble salt, MnO 2 , the anode plate comprises a zinc plate; The cathode electrode sheet comprises a copper sheet, and the anode electrode sheet comprises a magnesium sheet; The negative electrode current collector comprises any one of a zinc sheet, an AZ31 magnesium alloy, an AZ91 magnesium alloy, an 80-mesh AZ91 magnesium alloy mesh, an aluminum sheet, an aluminum mesh, an iron sheet, and an iron mesh; The carbon fiber includes polyacrylonitrile-based carbon fiber or polyacrylonitrile-based carbon fiber mesh.
6. The method for preparing the cement-based energy storage device according to claim 5, It is characterized in that The active material layer of the cathode plate includes silicate, water-soluble salt, MnO 2 The mass ratio of the silicate to the water-soluble salt is 1:0.4, and the corresponding mass of MnO is added to the active material layer of corresponding size. 2 , the corresponding size is 25mm×50mm×78mm, and the corresponding mass is 5g to 15g.
7. The method for preparing a cement-based energy storage device according to any one of claims 1 to 4 and 6, It is characterized in that The size of the cement-based energy storage device is 50 mm×50 mm×78 mm.
8. The method for preparing the cement-based energy storage device according to claim 7, It is characterized in that The distance between the positive electrode current collector and the negative electrode current collector is 1 cm to 3 cm.
9. A power supply system, It is characterized in that The power supply system comprises a plurality of cement-based energy storage devices connected in series and / or in parallel, and the cement-based energy storage device is prepared by the preparation method of a cement-based energy storage device according to any one of claims 1 to 8.
10. An energy storage building, It is characterized in that The energy storage building comprises a cement-based energy storage device prepared by the method for preparing a cement-based energy storage device according to any one of claims 1 to 8.
Citation Information
Cited By
Energy storage battery and preparation method thereof
CN120184348A
Energy storage battery and preparation method thereof
CN120184348B
Structure, energy storage and heat preservation integrated multifunctional building board and preparation method thereof
CN120666872A
A multifunctional building board with integrated structure, energy storage and thermal insulation and its preparation method
CN120666872B