Solid-state lithium ion battery and preparation method thereof
By in-situ polymerization between positive and negative electrodes, the problems of production complexity and poor interface contact of traditional solid-state lithium-ion batteries are solved, and the battery performance is improved and the cycle life is extended, which is suitable for industrial production.
Patent Information
- Application Number
- CN202411123312.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-15
- Publication Date
- 2024-11-26
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Traditional solid-state lithium-ion batteries have complex production processes, low production efficiency and high cost, and poor interface contact between solid electrodes and solid electrolyte membranes, resulting in poor battery performance and short cycle life, limiting their application and development.
The front-end polymerization method is used to form a solid electrolyte membrane between the positive and negative electrodes, reducing the charge transfer impedance at the solid interface and improving battery performance. The specific steps include mixing the polymerizable small molecule monomer, solvent, initiator and lithium salt to form a polymerizable electrolyte solution, injecting it into a metal shell for heat-initiating polymerization, and forming a solid electrolyte membrane.
It simplifies the process, improves production efficiency, reduces energy consumption, improves battery performance and cycle life, and is suitable for industrial applications.
Smart Images

Figure CN119029331A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of lithium ion batteries, and in particular relates to a solid-state lithium ion battery and a preparation method thereof. Background Art
[0002] Lithium-ion batteries have the advantages of high energy density, long cycle life, and good reliability, and have been widely developed and applied in the past decade. The energy density of lithium-ion batteries has reached a bottleneck value, which greatly limits the application of lithium-ion batteries in large-scale energy storage devices. In addition, the organic electrolytes commonly used in traditional commercial lithium-ion batteries have problems such as easy leakage, explosion, flammability, and environmental unfriendliness, which have become safety hazards in the application of lithium-ion batteries. With the rapid development of the new energy vehicle industry, the requirements for the energy density of power batteries are getting higher and higher, and the development of new lithium battery systems has become an urgent need.
[0003] The method of using all-solid-state electrolytes to replace traditional organic electrolytes can not only greatly improve the energy density of lithium-ion batteries, but also fundamentally solve safety hazards. Solid electrolytes can be divided into two categories: inorganic solid electrolytes and polymer solid electrolytes. Polymer solid electrolytes have become an ideal material for the new generation of solid electrolytes due to their low price, flexibility, easy processing, and high lithium stability. The polymer solid polymer system is generally composed of polymers and lithium salts. The lithium salt is dissolved in the polymer, and lithium ions are transmitted through the movement of polymer chain segments, which plays a role in material transportation.
[0004] Therefore, preparing an all-solid-state lithium battery with high energy density and strong safety has become a current research hotspot. Summary of the invention
[0005] The present invention is based on the inventor's discovery and understanding of the following facts and problems: At present, the production of solid-state batteries is mainly completed by first producing solid-state electrodes and solid-state electrolyte membranes separately, and then assembling the batteries. The manufacturing process is complex, with low production efficiency, low yield, and high cost. In addition, the interface contact between the solid electrode and the solid electrolyte membrane is poor, which will lead to problems such as poor battery performance and short cycle life, restricting the application and development of solid-state batteries.
[0006] The present invention aims to solve one of the technical problems in the related art to at least a certain extent. To this end, an embodiment of the present invention provides a method for preparing a solid-state lithium-ion battery, which uses a front-end polymerization method to form a solid electrolyte membrane by in-situ polymerization between the positive and negative electrodes, thereby reducing the charge transfer impedance at the solid interface and improving the battery performance.
[0007] The method for preparing a solid-state lithium-ion battery according to an embodiment of the present invention comprises the following steps:
[0008] (1) mixing a polymerizable small molecule monomer, a solvent, an initiator and a lithium salt to obtain a polymerizable electrolyte solution;
[0009] (2) placing the positive electrode sheet and the negative electrode sheet into a metal shell;
[0010] (3) Injecting the polymerizable electrolyte solution obtained in step (1) into the metal shell in step (2), and using front-end polymerization to polymerize the polymerizable electrolyte solution in situ to form a solid electrolyte membrane.
[0011] The advantages and technical effects brought by the preparation method of the solid-state lithium-ion battery of the embodiment of the present invention are as follows: 1. In the embodiment of the present invention, the front-end polymerization method is used to in-situ polymerize between the positive and negative electrodes to form a solid electrolyte membrane, which can reduce the charge transfer impedance at the solid interface and improve the battery performance; 2. In the embodiment of the present invention, the external energy supply required for the front-end polymerization is one-time, that is, the energy supply can be stopped once it is triggered. In the subsequent polymerization process, the heat energy generated by the reaction can be used to complete the entire polymerization reaction in a relatively short time, and it has the characteristics of fast speed and low energy consumption; 3. The method of the embodiment of the present invention has a simple process, is easy to operate, has high production efficiency, and is suitable for promotion and application in industrial production.
[0012] In some embodiments, in step (1), the mass of the polymerizable small molecule monomer is 32-65% of the mass of the polymerizable electrolyte solution.
[0013] In some embodiments, in step (1), the polymerizable small molecule monomer includes at least one of methyl methacrylate, acrylic acid or methacrylic acid.
[0014] In some embodiments, in step (1), the mass of the initiator is 5-10% of the mass of the polymerizable electrolyte solution.
[0015] In some embodiments, in step (1), the initiator includes at least one of azobisisobutyronitrile, benzoyl peroxide, potassium persulfate or methyl ethyl ketone peroxide.
[0016] In some embodiments, in step (2), the positive electrode active material in the positive electrode sheet includes at least one of lithium manganese oxide, lithium cobalt oxide, lithium iron phosphate, and lithium nickel cobalt aluminum oxide; the negative electrode active material in the negative electrode sheet includes at least one of metallic lithium, alloy materials, graphite, amorphous carbon, mesophase carbon microbeads, nanosilicon, silicon-carbon materials, and lithium titanate.
[0017] In some embodiments, in step (3), the front-end polymerization is initiated by thermal initiation.
[0018] In some embodiments, the thermal initiation temperature is 110-150° C., and the thermal initiation time is 15-30 s.
[0019] In some embodiments, the step (3) further comprises injecting the polymerizable electrolyte solution into the metal shell and then allowing the metal shell to stand for a while.
[0020] The embodiment of the present invention further provides a solid-state lithium-ion battery, which is prepared by the above-mentioned preparation method. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1 is a schematic diagram of a solid-state lithium-ion battery prepared in Example 1;
[0022] Reference numerals: 1-aluminum shell, 2-positive electrode, 3-solid electrolyte membrane, 4-negative electrode. DETAILED DESCRIPTION
[0023] Embodiments of the present invention are described in detail below, and examples of the embodiments are shown in the accompanying drawings. The embodiments described below with reference to the accompanying drawings are exemplary and intended to be used to explain the present invention, but should not be understood as limiting the present invention.
[0024] The method for preparing a solid-state lithium-ion battery according to an embodiment of the present invention comprises the following steps:
[0025] (1) mixing a polymerizable small molecule monomer, a solvent, an initiator and a lithium salt to obtain a polymerizable electrolyte solution;
[0026] (2) placing the positive electrode sheet and the negative electrode sheet into a metal shell;
[0027] (3) Injecting the polymerizable electrolyte solution obtained in step (1) into the metal shell in step (2), and using front-end polymerization to polymerize the polymerizable electrolyte solution in situ to form a solid electrolyte membrane.
[0028] The preparation method of the solid-state lithium-ion battery of the embodiment of the present invention adopts the front-end polymerization method to form a solid electrolyte membrane by in-situ polymerization between the positive and negative electrodes, which can reduce the charge transfer impedance at the solid interface and improve the battery performance; the external energy supply required for the front-end polymerization is one-time, that is, the energy supply can be stopped once it is triggered. In the subsequent polymerization process, the heat energy generated by the reaction can be used to complete the entire polymerization reaction in a relatively short time, and it has the characteristics of fast speed and low energy consumption; the method has a simple process, is easy to operate, has high production efficiency, and is suitable for promotion and application in industrial production.
[0029] In some embodiments, preferably, in step (1), the mass of the polymerizable small molecule monomer is 32-65% of the mass of the polymerizable electrolyte solution. Further preferably, in step (1), the polymerizable small molecule monomer includes at least one of methyl methacrylate, acrylic acid or methacrylic acid.
[0030] In the embodiments of the present invention, the dosage of the polymerizable small molecule monomer is preferably selected, which is conducive to the complete front-end polymerization; if the dosage of the polymerizable small molecule monomer is too low, the front-end polymerization cannot be carried out or the front-end polymerization thermal drive fails due to insufficient reaction heat generated during the process, and the polymerization reaction cannot be sustained; if the dosage of the polymerizable small molecule is too high, the lithium salt concentration in the solid electrolyte will be low and the conductivity will be poor.
[0031] In some embodiments, preferably, in step (1), the mass of the initiator is 5-10% of the mass of the polymerizable electrolyte solution. Further preferably, in step (1), the initiator includes at least one of azobisisobutyronitrile, benzoyl peroxide, potassium persulfate or methyl ethyl ketone peroxide.
[0032] In the embodiment of the present invention, the dosage of the initiator is optimized, which is conducive to the formation of a solid electrolyte membrane with uniform pores, so that conductive ions can pass smoothly through the electrolyte membrane, ensuring that the battery has good conductivity; if the dosage of the initiator is too low, the front-end polymerization will not occur; if the dosage of the initiator is too high, the front-end polymerization reaction will be violent, resulting in excessive pores in the solid electrolyte membrane, which may cause a battery short circuit in the later stage of the cycle.
[0033] In some embodiments, preferably, in step (1), the lithium salt comprises lithium hexafluorophosphate (LiPF 6 ), lithium bis(trifluoromethylsulfonyl)imide (LiFSI). Further preferably, the mass of the lithium salt is 15-30% of the mass of the electrolyte solution.
[0034] In some embodiments, preferably, in step (1), the solvent comprises at least one of DMS or DMC.
[0035] In some embodiments, preferably, in step (2), the positive electrode active material in the positive electrode sheet includes at least one of lithium manganese oxide, lithium cobalt oxide, lithium iron phosphate, and lithium nickel cobalt aluminum oxide; the negative electrode active material in the negative electrode sheet includes at least one of metallic lithium, alloy material, graphite, amorphous carbon, mesophase carbon microspheres, nano-silicon, silicon-carbon material, and lithium titanate. Further preferably, the metal shell includes an aluminum shell, and the graphite includes artificial graphite.
[0036] In some embodiments, preferably, in step (3), the front-end polymerization is initiated by thermal initiation. Further preferably, the thermal initiation temperature is 110 to 150° C., and the thermal initiation time is 15 to 30 seconds.
[0037] In the embodiment of the present invention, it is preferred to initiate the front-end polymerization by thermal initiation. Using a higher temperature to initiate the polymerization can achieve a one-time energy supply and reduce the time and energy consumption required for the polymerization reaction. If the thermal initiation temperature is low, the front-end polymerization will fail; if the thermal initiation temperature is high, the front-end polymerization reaction will be violent, resulting in excessive pores in the solid electrolyte membrane, which may cause a battery short circuit in the later stage of the cycle.
[0038] In some embodiments, preferably, the thermal initiation is performed by heating from the bottom.
[0039] In some embodiments, preferably, the step (3) further comprises: injecting the polymerizable electrolyte solution into the metal shell and then performing a static treatment. Further preferably, the static treatment is performed under vacuum at room temperature for 10 to 14 hours.
[0040] In the embodiment of the present invention, the polymerizable electrolyte solution is injected into the metal shell and then left to stand, so that the polymerizable electrolyte solution can fully fill the gap between the positive and negative electrode sheets, thereby ensuring the performance of the prepared solid-state lithium-ion battery.
[0041] like Figure 1 As shown, an embodiment of the present invention further provides a solid-state lithium-ion battery, which is prepared using the above-mentioned preparation method.
[0042] The technical solution of the present invention is described in detail below in conjunction with specific embodiments and drawings.
[0043] Example 1
[0044] (1) mixing acrylic acid, dimethyl carbonate, lithium hexafluorophosphate, and azobisisobutyronitrile in a mass ratio of 45:30:20:5 to form a polymerizable electrolyte solution;
[0045] (2) Alternately stacking lithium iron phosphate positive electrode sheets and artificial graphite negative electrode sheets together and placing them in a square aluminum shell;
[0046] (3) The aluminum shell is opened upward, and the polymerizable electrolyte solution is injected into the square aluminum shell;
[0047] (4) Standing at 25°C in vacuum for 12 h to allow the electrolyte solution to fully penetrate and fill the gap between the positive and negative electrode sheets;
[0048] (5) using bottom heat to initiate front-end polymerization, with an initiation temperature of 130° C. and an initiation time of 20 seconds, so that the polymerizable electrolyte solution undergoes in-situ polymerization to form a solid electrolyte membrane between the lithium iron phosphate positive electrode sheet and the artificial graphite negative electrode sheet;
[0049] (6) The positive and negative electrodes are led out, and the aluminum shell is sealed and welded with a top cover to obtain a solid-state lithium-ion battery.
[0050] Comparative Example 1
[0051] The preparation method of this comparative example is the same as that of Example 1, except that in step (1), the mass ratio of acrylic acid, dimethyl carbonate, lithium hexafluorophosphate and azobisisobutyronitrile is 30:45:20:5.
[0052] Comparative Example 2
[0053] The preparation method of this comparative example is the same as that of Example 1, except that in step (1), the mass ratio of acrylic acid, dimethyl carbonate, lithium hexafluorophosphate and azobisisobutyronitrile is 45:30:23:2.
[0054] Comparative Example 3
[0055] The preparation method of this comparative example is the same as that of Example 1, except that the initiation temperature in step (5) is 80°C.
[0056] Comparative Example 4
[0057] The preparation method of this comparative example is the same as that of Example 1, except that: the initiation temperature in step (5) is 200°C.
[0058] The preparation method of this comparative example is the same as that of Example 1, except that the initiation time in step (5) is 60 seconds.
[0059] Comparative Example 6
[0060] The preparation method of this comparative example is the same as that of Example 1, except that: in step (5), front-end polymerization is not used, conventional polymerization is used, and curing is performed at 65° C. for 24 hours to form a solid electrolyte membrane between the lithium iron phosphate positive electrode sheet and the artificial graphite negative electrode sheet.
[0061] The performance of the batteries prepared in Example 1 and Comparative Examples 1 to 6 were tested, and the results are shown in Tables 1 and 2, wherein whether the polymerizable electrolyte solution solidifies is observed to evaluate whether front-end polymerization occurs; the battery AC internal resistance reflects the solid interface impedance, and the battery AC internal resistance is measured with an external ammeter; the first efficiency of the battery is tested in a formation and capacity distribution cabinet, and a 1C / 1C cycle performance test is performed in a test cabinet.
[0062] Table 1
[0063] Whether front-end aggregation occurs Example 1 yes Comparative Example 1 no Comparative Example 2 no Comparative Example 3 no Comparative Example 4 yes Comparative Example 5 yes
[0064] Table 2
[0065]
[0066] In the present invention, the terms "one embodiment", "some embodiments", "examples", "specific examples", or "some examples" etc. mean that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representations of the above terms do not necessarily refer to the same embodiment or example. Moreover, the described specific features, structures, materials or characteristics may be combined in any one or more embodiments or examples in a suitable manner. In addition, those skilled in the art may combine and combine the different embodiments or examples described in this specification and the features of the different embodiments or examples, without contradiction.
[0067] Although the above embodiments have been shown and described, it is to be understood that the above embodiments are exemplary and are not to be construed as limitations on the present invention. Changes, modifications, substitutions and variations of the above embodiments by those of ordinary skill in the art are all within the scope of protection of the present invention.
Claims
1. A method for preparing a solid-state lithium-ion battery, It is characterized in that The following steps are involved: (1) mixing a polymerizable small molecule monomer, a solvent, an initiator and a lithium salt to obtain a polymerizable electrolyte solution; (2) placing the positive electrode sheet and the negative electrode sheet into a metal shell; (3) Injecting the polymerizable electrolyte solution obtained in step (1) into the metal shell in step (2), and using front-end polymerization to polymerize the polymerizable electrolyte solution in situ to form a solid electrolyte membrane.
2. The method for preparing a solid-state lithium-ion battery according to claim 1, It is characterized in that In the step (1), the mass of the polymerizable small molecule monomer is 32-65% of the mass of the polymerizable electrolyte solution.
3. The method for preparing a solid-state lithium-ion battery according to claim 1 or 2, It is characterized in that In the step (1), the polymerizable small molecule monomer includes at least one of methyl methacrylate, acrylic acid or methacrylic acid.
4. The method for preparing a solid-state lithium-ion battery according to claim 1, It is characterized in that In the step (1), the mass of the initiator is 5-10% of the mass of the polymerizable electrolyte solution.
5. The method for preparing a solid-state lithium-ion battery according to claim 1 or 4, It is characterized in that In the step (1), the initiator includes at least one of azobisisobutyronitrile, benzoyl peroxide, potassium persulfate or methyl ethyl ketone peroxide.
6. The method for preparing a solid-state lithium-ion battery according to claim 1, It is characterized in that In the step (2), the positive electrode active material in the positive electrode sheet includes at least one of lithium manganese oxide, lithium cobalt oxide, lithium iron phosphate, and lithium nickel cobalt aluminum oxide; the negative electrode active material in the negative electrode sheet includes at least one of metallic lithium, alloy materials, graphite, amorphous carbon, mesophase carbon microspheres, nano-silicon, silicon-carbon materials, and lithium titanate.
7. The method for preparing a solid-state lithium-ion battery according to claim 1, It is characterized in that In the step (3), the front-end polymerization is initiated by thermal initiation.
8. The method for preparing a solid-state lithium-ion battery according to claim 7, It is characterized in that The temperature of the thermal initiation is 110-150° C., and the time of the thermal initiation is 15-30 seconds.
9. The method for preparing a solid-state lithium-ion battery according to claim 1, It is characterized in that The step (3) further comprises injecting the polymerizable electrolyte solution into the metal shell and then allowing the metal shell to stand for a while.
10. A solid-state lithium-ion battery, It is characterized in that The preparation method is described in any one of claims 1 to 9.
Citation Information
Patent Citations
Method for preparing macroporous quick-response polyacrylamide hydrogel by adopting frontal polymerization of acrylamide deep-eutectic solvent
CN111040074A
Solid-state lithium battery and production method thereof
CN113054241A
In-situ polymerization electrolyte, method for preparing in-situ all-solid-state battery by adopting in-situ polymerization electrolyte and in-situ all-solid-state battery
CN113299982A
Lithium battery assembly process for heating and curing an electrolyte in situ
CN113540574A
Separator-free solid-state lithium ion battery and preparation method thereof
CN115483431A