Preparation method for microminiature LTCC (Low Temperature Co-Fired Ceramic) filter
Through the alternating overprinting of ceramic paste and electrode silver paste and multiple hole filling processes, the problems of shrinkage difference and alignment deviation in the preparation of micro-small LTCC filters are solved, and smaller design errors and simplified production processes are achieved, suitable for large-scale Rapid production.
Patent Information
- Application Number
- CN202411152896.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-21
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2044-08-21
AI Technical Summary
The existing micro-small LTCC filter preparation methods require precision high-end equipment, and there are problems of shrinkage differences in the growing ceramic belt and stack alignment deviation, resulting in large differences in design and physical objects, and lack of convenient preparation methods.
The dielectric layer and electrode pattern are prepared by alternately printing of ceramic paste and electrode silver paste. Through multiple overprinting and hole filling processes, the high solid content and appropriate viscosity of ceramic paste are combined to reduce shrinkage differences, and the difference is dried, cut and glue discharge A sintering process is used to produce a micro-sized LTCC filter.
It reduces shrinkage differences during processing, reduces design and physical differences, simplifies the preparation process, is suitable for large-scale rapid production, and avoids the use of high-end equipment.
Smart Images

Figure CN119029522A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of filter preparation, and in particular to a preparation method for a micro-LTCC filter. Background Art
[0002] LTCC filters, with a frequency range of 300kHz to 300GHz, are low-pass filter circuits composed of inductors and capacitors. They allow the current of useful signals to pass through, while attenuating interference signals with higher frequencies. Therefore, they are generally used as wireless RF components in mobile communication equipment and other fields. For example: mobile phones, WLAN, Bluetooth, power amplifiers, automotive electronics, etc. With the increase in market demand and functional characteristics, the miniaturization of LTCC filters is a future-oriented trend.
[0003] LTCC is a 3D design structure composed of a dielectric layer and a metal electrode. The production process of the dielectric layer is to weigh ethanol, toluene, polyether phosphate, polyvinyl butyral, diisobutyl phthalate, and LTCC microwave dielectric ceramic powder in proportion and perform ball milling to produce ceramic slurry. The ceramic slurry is then vacuum defoamed and then the ceramic slurry obtained after vacuum defoaming is cast on a casting machine. The casting process requires the use of a carrier film to coat the ceramic slurry on the carrier film and dry it to obtain a roll of LTCC raw ceramic tape with a thickness of 20μm to 90μm. The solid content of the ceramic slurry powder can reach 40% to 60%.
[0004] Since LTCC is a three-dimensional design structure, in order to realize the circuit design of each layer and the through-conduction requirements, it is necessary to use a sheet of raw porcelain tape for post-processing. Therefore, the existing technical preparation method mainly uses a rolled raw porcelain tape for cutting process to form a sheet of raw porcelain tape, and then uses laser drilling, silver paste to slurry in micropores and precision printing to prepare a circuit pattern. After the circuit pattern is heated and dried, a raw porcelain tape covered with a metal electrode is obtained. After heating and drying, multiple pieces of raw porcelain tapes with metal electrodes are obtained and stacked, cut into granules, debonded, sintered, and finally processed through a post-processing process such as rolling corners, silver end, sintering, electroplating, external inspection and package testing to make LTCC filter products, such as Figure 1 As shown. Due to future design requirements, the preparation of LTCC filters will gradually be oriented towards micro-LTCC filters. However, there are certain degrees of variation in multiple process technologies in the preparation of LTCC filters, especially in the process accuracy of micro-LTCC filters and large-size products. In order to reduce the shrinkage difference between the green ceramic tape and the electrode silver paste and the alignment deviation when the green ceramic tape is stacked, more precise high-end equipment or more excellent preparation methods are required. Summary of the invention
[0005] In order to solve the above technical problems, the purpose of the present invention is to provide a method for preparing a micro-LTCC filter, so as to solve the problem that the existing micro-LTCC filter needs to rely on precise high-end equipment and lacks a convenient production and preparation method.
[0006] The technical solution of the present invention to solve the above technical problems is as follows:
[0007] A method for preparing a micro-LTCC filter comprises the following steps:
[0008] First, the first layer of electrode pattern is printed on the transfer film using electrode silver paste as raw material, and then ceramic paste and electrode silver paste are alternately used as raw materials to be laminated and printed and dried to prepare dielectric layer and electrode pattern to obtain a blank, which is then dried, cut, debonded and sintered, and finally obtained through post-processing technology.
[0009] Furthermore, the fourth layer is a dielectric layer with holes, and the fifth layer is an electrode pattern for filling the holes in the fourth layer or filling and printing the holes. The preparation of the fourth and fifth layers is repeated several times. After reaching the target number of layers, the top layer is prepared using ceramic paste as raw material; wherein the target number of layers is 5+2n, n=0~100.
[0010] Furthermore, the transfer film includes an OPP film or a release PET film.
[0011] Furthermore, the solid content of the electrode silver paste is 75-92wt%.
[0012] Further, the ceramic paste is prepared by mixing the following components in parts by weight: 75-92 parts of LTCC microwave dielectric ceramic powder, 1-5 parts of polypropylene butyral resin, 1-5 parts of polyester, 5-15 parts of diethylene glycol monobutyl ether and 5-15 parts of pinene alcohol, and mixing them evenly to obtain the obtained product;
[0013] The LTCC microwave dielectric ceramic powder comprises the following components in parts by weight: 50-60 parts of SiO2, 40-50 parts of Al2O3, 0.5-2 parts of B2O3 and 1-3 parts of TiO2.
[0014] Furthermore, the solid content of the ceramic paste is 75-92 wt %, and the viscosity of the ceramic paste is 100,000-600,000 Cp.
[0015] Furthermore, each layer is dried after printing at a temperature of 40 to 100° C. for 5 to 15 minutes.
[0016] Furthermore, the thickness of each layer is 5 to 120 μm.
[0017] Furthermore, the debinding temperature is 250-450° C. for 1-5 hours, and the sintering temperature is 850-950° C. for 1-5 hours.
[0018] Furthermore, post-processing processes include corner rolling, silver termination, sintering and electroplating.
[0019] The present invention has the following beneficial effects:
[0020] The present invention adopts a ceramic paste method to replace the ceramic slurry casting method in the traditional preparation process to prepare the micro-LTCC filter, thereby reducing the shrinkage difference in the processing process. When preparing micro-products, the shrinkage rate can be fixed to calculate the design ratio of the dielectric layer and the metal electrode before and after sintering, so that the difference between the designed product and the actual product is smaller, reducing the design error, the preparation process does not require high-end precision equipment, the production process is shorter, and it is suitable for large-scale rapid production. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1 This is a flow chart of the preparation of LTCC filters in traditional technology;
[0022] Figure 2 The present invention is a flow chart of the preparation of a micro-LTCC filter;
[0023] Figure 3 It is a schematic diagram of the overprinting method in the preparation process of the micro-LTCC filter of the present invention. DETAILED DESCRIPTION
[0024] The principles and features of the present invention are described below in conjunction with the accompanying drawings. The examples are only used to explain the present invention and are not used to limit the scope of the present invention. If specific conditions are not specified in the embodiments, they are carried out according to normal conditions or conditions recommended by the manufacturer. If the manufacturer is not specified for the reagents or instruments used, they are all conventional products that can be purchased commercially.
[0025] Embodiment 1:
[0026] A preparation method for a micro-LTCC filter (preparation flow chart as shown in Figure 2 The schematic diagram of the overprinting process is shown in Figure 3 As shown), comprising the following steps:
[0027] (1) Preparation of ceramic paste with a solid content of 80 wt% by weight: 80 parts of LTCC microwave dielectric ceramic powder, 3 parts of polypropylene butyral resin, 3 parts of polyester, 7 parts of diethylene glycol monobutyl ether and 7 parts of terpineol were mixed by weight, and mixed evenly by three rollers and a centrifugal mixer to obtain a ceramic paste;
[0028] The LTCC microwave dielectric ceramic powder includes the following components in parts by weight: 54 parts of SiO2, 43 parts of Al2O3, 1 part of B2O3 and 2 parts of TiO2.
[0029] (2) Preparation of the first layer: A release PET film was used as a transfer film on a printing device, and a screen was placed on the transfer film using electrode silver paste (manufacturer: NAMICS CORPORATION; model: 7396; solid content 85%) as a raw material to print and prepare an electrode pattern with a printing thickness of 15 μm. After printing, the electrode was placed in an oven and dried at 80° C. for 10 min to complete the external circuit electrode and obtain the first layer;
[0030] (3) Preparation of the second layer: Replace the screen, and print a dielectric layer with a thickness of 50 μm using ceramic paste as a raw material on the basis of the first layer, and then put it into an oven and dry it at 80° C. for 10 min to obtain the second layer;
[0031] (4) Preparation of the third layer: Replace the screen, and print the electrode pattern on the basis of the second layer using the electrode silver paste as the raw material, with a printing thickness of 15 μm, and then put it into an oven and dry it at 80° C. for 10 min to obtain the third layer;
[0032] (5) Preparation of the fourth layer: Replace the screen, and print a dielectric layer with a thickness of 50 μm and holes using ceramic paste as a raw material on the basis of the third layer, and then put it into an oven and dry it at 80° C. for 10 min to obtain the fourth layer;
[0033] (6) Preparation of the fifth layer: Replace the screen, and print the electrode silver paste as the raw material to fill the holes on the basis of the fourth layer and print the electrode pattern with a thickness of 15 μm, then put it into the oven and dry it at 80° C. for 10 min to obtain the fifth layer;
[0034] (7) Repeat step (5) and step (6) once, and after reaching the seventh layer, use ceramic paste as a raw material to print on the seventh layer to prepare a dielectric layer with a thickness of 50 μm, then put it into an oven, dry it at 80° C. for 10 min, cut it into granules, debind it at 350° C. for 2 h, sinter it at 900° C. for 2 h, and finally roll the corners, end the silver, sinter it and electroplate it to obtain the product.
[0035] Embodiment 2:
[0036] A method for preparing a micro-LTCC filter comprises the following steps:
[0037] (1) Preparation of a ceramic paste with a solid content of 85 wt % by weight: 85 parts of LTCC microwave dielectric ceramic powder, 3 parts of polypropylene butyral resin, 3 parts of polyester, 4.5 parts of diethylene glycol monobutyl ether and 4.5 parts of terpineol were mixed by weight, and mixed evenly by three rollers and a centrifugal mixer to obtain a ceramic paste;
[0038] The LTCC microwave dielectric ceramic powder includes the following components in parts by weight: 54 parts of SiO2, 43 parts of Al2O3, 1 part of B2O3 and 2 parts of TiO2.
[0039] (2) Preparation of the first layer: A release PET film was used as a transfer film on a printing device, and a screen was placed on the transfer film using electrode silver paste (manufacturer: NAMICS CORPORATION; model: 7396; solid content 85%) as a raw material to print and prepare an electrode pattern with a printing thickness of 15 μm. After printing, the electrode was placed in an oven and dried at 80° C. for 10 min to complete the external circuit electrode and obtain the first layer;
[0040] (3) Preparation of the second layer: Replace the screen, and print a dielectric layer with a thickness of 50 μm using ceramic paste as a raw material on the basis of the first layer, and then put it into an oven and dry it at 80° C. for 10 min to obtain the second layer;
[0041] (4) Preparation of the third layer: Replace the screen, and print the electrode pattern on the basis of the second layer using the electrode silver paste as the raw material, with a printing thickness of 15 μm, and then put it into an oven and dry it at 80° C. for 10 min to obtain the third layer;
[0042] (5) Preparation of the fourth layer: Replace the screen, and print a dielectric layer with a thickness of 50 μm and holes using ceramic paste as a raw material on the basis of the third layer, and then put it into an oven and dry it at 80° C. for 10 min to obtain the fourth layer;
[0043] (6) Preparation of the fifth layer: Replace the screen, and print the electrode silver paste as the raw material to fill the holes on the basis of the fourth layer and print the electrode pattern with a thickness of 15 μm, then put it into the oven and dry it at 80° C. for 10 min to obtain the fifth layer;
[0044] (7) Repeat step (5) and step (6) once, and after reaching the seventh layer, use ceramic paste as a raw material to print on the seventh layer to prepare a dielectric layer with a thickness of 50 μm, then put it into an oven, dry it at 80° C. for 10 min, cut it into granules, debind it at 350° C. for 2 h, sinter it at 900° C. for 2 h, and finally roll the corners, end the silver, sinter it and electroplate it to obtain the product.
[0045] Embodiment 3:
[0046] A method for preparing a micro-LTCC filter comprises the following steps:
[0047] (1) Preparation of a ceramic paste with a solid content of 92 wt % by weight: 92 parts of LTCC microwave dielectric ceramic powder, 3 parts of polypropylene butyral resin, 3 parts of polyester, 1 part of diethylene glycol monobutyl ether and 1 part of terpineol were mixed by weight, and mixed evenly by a three-drum and centrifugal mixer to obtain a ceramic paste;
[0048] The LTCC microwave dielectric ceramic powder includes the following components in parts by weight: 54 parts of SiO2, 43 parts of Al2O3, 1 part of B2O3 and 2 parts of TiO2.
[0049] (2) Preparation of the first layer: A release PET film was used as a transfer film on a printing device, and a screen was placed on the transfer film using electrode silver paste (manufacturer: NAMICS CORPORATION; model: 7396; solid content 85%) as a raw material to print and prepare an electrode pattern with a printing thickness of 15 μm. After printing, the electrode was placed in an oven and dried at 80° C. for 10 min to complete the external circuit electrode and obtain the first layer;
[0050] (3) Preparation of the second layer: Replace the screen, and print a dielectric layer with a thickness of 50 μm using ceramic paste as a raw material on the basis of the first layer, and then put it into an oven and dry it at 80° C. for 10 min to obtain the second layer;
[0051] (4) Preparation of the third layer: Replace the screen, and print the electrode pattern on the basis of the second layer using the electrode silver paste as the raw material, with a printing thickness of 15 μm, and then put it into an oven and dry it at 80° C. for 10 min to obtain the third layer;
[0052] (5) Preparation of the fourth layer: Replace the screen, and print a dielectric layer with a thickness of 50 μm and holes using ceramic paste as a raw material on the basis of the third layer, and then put it into an oven and dry it at 80° C. for 10 min to obtain the fourth layer;
[0053] (6) Preparation of the fifth layer: Replace the screen, and print the electrode silver paste as the raw material to fill the holes on the basis of the fourth layer and print the electrode pattern with a thickness of 15 μm, then put it into the oven and dry it at 80° C. for 10 min to obtain the fifth layer;
[0054] (7) Repeat step (5) and step (6) once, and after reaching the seventh layer, use ceramic paste as a raw material to print on the seventh layer to prepare a dielectric layer with a thickness of 50 μm, then put it into an oven, dry it at 80° C. for 10 min, cut it into granules, debind it at 350° C. for 2 h, sinter it at 900° C. for 2 h, and finally roll the corners, end the silver, sinter it and electroplate it to obtain the product.
[0055] Comparative Example 1:
[0056] A method for preparing a micro-LTCC filter comprises the following steps:
[0057] (1) using ethanol, toluene, polyether phosphate, polyvinyl butyral and diisobutyl phthalate as raw materials, mixing and ball milling, and then vacuum degassing to obtain a ceramic slurry with a solid content of 50wt%;
[0058] (2) using the ceramic slurry obtained in step (1) as a raw material for tape casting, and drying to obtain a LTCC green ceramic tape with a thickness of 50 μm;
[0059] (3) cutting the LTCC raw ceramic tape obtained in step (2) into pieces, punching holes with laser, injecting electrode silver paste into micropores to obtain a circuit pattern, and finally drying at 80° C. for 10 min to obtain a raw ceramic tape covered with metal electrodes;
[0060] (4) The four raw porcelain strips covered with metal electrodes obtained in step (3) are first subjected to isostatic pressing, then cut into granules, debinded at 350° C. for 2 h, sintered at 900° C. for 2 h, and finally rolled, silvered, sintered and electroplated to obtain the product.
[0061] Comparative Example 2:
[0062] A method for preparing a micro-LTCC filter comprises the following steps:
[0063] (1) Preparation of a ceramic paste with a solid content of 60 wt % by weight: 60 parts of LTCC microwave dielectric ceramic powder, 3 parts of polypropylene butyral resin, 3 parts of polyester, 17 parts of diethylene glycol monobutyl ether and 17 parts of terpineol were mixed by weight, and mixed evenly by a three-drum and centrifugal mixer to obtain a ceramic paste;
[0064] The LTCC microwave dielectric ceramic powder includes the following components in parts by weight: 54 parts of SiO2, 43 parts of Al2O3, 1 part of B2O3 and 2 parts of TiO2.
[0065] (2) Preparation of the first layer: A release PET film was used as a transfer film on a printing device, and a screen was placed on the transfer film using electrode silver paste (manufacturer: NAMICS CORPORATION; model: 7396; solid content 85%) as a raw material to print and prepare an electrode pattern with a printing thickness of 15 μm. After printing, the electrode was placed in an oven and dried at 80° C. for 10 min to complete the external circuit electrode and obtain the first layer;
[0066] (3) Preparation of the second layer: Replace the screen, and print a dielectric layer with a thickness of 50 μm using ceramic paste as a raw material on the basis of the first layer, and then put it into an oven and dry it at 80° C. for 10 min to obtain the second layer;
[0067] (4) Preparation of the third layer: Replace the screen, and print the electrode pattern on the basis of the second layer using the electrode silver paste as the raw material, with a printing thickness of 15 μm, and then put it into an oven and dry it at 80° C. for 10 min to obtain the third layer;
[0068] (5) Preparation of the fourth layer: Replace the screen, and print a dielectric layer with a thickness of 50 μm and holes using ceramic paste as a raw material on the basis of the third layer, and then put it into an oven and dry it at 80° C. for 10 min to obtain the fourth layer;
[0069] (6) Preparation of the fifth layer: Replace the screen, and print the electrode silver paste as the raw material to fill the holes on the basis of the fourth layer and print the electrode pattern with a thickness of 15 μm, then put it into the oven and dry it at 80° C. for 10 min to obtain the fifth layer;
[0070] (7) Repeat step (5) and step (6) once, and after reaching the seventh layer, use ceramic paste as a raw material to print on the seventh layer to prepare a dielectric layer with a thickness of 50 μm, then put it into an oven, dry it at 80° C. for 10 min, cut it into granules, debind it at 350° C. for 2 h, sinter it at 900° C. for 2 h, and finally roll the corners, end the silver, sinter it and electroplate it to obtain the product.
[0071] Test example:
[0072] The miniature LTCC filters prepared in Examples 1-3 and Comparative Examples 1-2 were characterized. The four sides of the green body before debinding and sintering were cut off using a cutter. The cut four sides were placed under a video microscope for inspection and measurement. The widest point A and the narrowest point B were measured, and the stacking offset = (AB) / 2 was calculated. The frequency deviation caused by the stacking offset was detected using a Rohde network analyzer.
[0073] The experimental results are shown in Table 1.
[0074] Table 1 Performance characteristics
[0075]
[0076] As shown in Table 1, the miniature LTCC filter prepared by the embodiment of the present invention by overprinting ceramic paste and silver paste to prepare multiple dielectric layers and circuit layers can effectively avoid stacking offset, reduce the frequency deviation caused by stacking offset, and will not crack during the sintering process. The stacking offset phenomenon of the miniature LTCC filter prepared by the traditional method or the low solid content ceramic paste (60wt%) in Comparative Example 1-2 is significantly higher than that of the embodiment of the present invention. Among them, because the solid content of the ceramic paste in Comparative Example 2 is low, it will cause large shrinkage variation of the dielectric layer during sintering, resulting in offset and thickness difference after sintering, resulting in poor performance. The preparation method of the present invention not only shortens the preparation process compared to the traditional preparation method, but also does not require the use of high-end precision instruments, effectively avoiding the problem of electrical differences caused by variations between multiple process technologies when making miniature LTCC filters.
[0077] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.
Claims
1. A method for preparing a micro-LTCC filter, It is characterized in that The following steps are involved: First, the first layer of electrode pattern is printed on the transfer film using electrode silver paste as raw material, and then ceramic paste and electrode silver paste are alternately used as raw materials to be laminated and printed and dried to prepare dielectric layer and electrode pattern to obtain a blank, which is then dried, cut, debonded and sintered, and finally obtained through post-processing technology.
2. The method for preparing a micro-LTCC filter according to claim 1, It is characterized in that The fourth layer is a dielectric layer with holes, and the fifth layer is an electrode pattern for filling the holes in the fourth layer or filling and printing the holes. The preparation of the fourth and fifth layers is repeated several times. After reaching the target number of layers, the top layer is prepared using ceramic paste as raw material; wherein the target number of layers is 5+2n, n=0~100.
3. The method for preparing a micro-LTCC filter according to claim 1, It is characterized in that The transfer film includes an OPP film or a release PET film.
4. The method for preparing a micro-LTCC filter according to claim 1, It is characterized in that The solid content of the electrode silver paste is 75-92 wt %.
5. The method for preparing a micro-LTCC filter according to claim 1, It is characterized in that The ceramic paste is prepared by mixing the following components in parts by weight: 75-92 parts of LTCC microwave dielectric ceramic powder, 1-5 parts of polypropylene butyral resin, 1-5 parts of polyester, 5-15 parts of diethylene glycol monobutyl ether and 5-15 parts of pinene alcohol, and mixing them evenly; The LTCC microwave dielectric ceramic powder includes the following components by weight: SiO 2 50-60 parts, Al 2 O 3 40~50 copies, B 2 O 3 0.5~2 parts and TiO 2 1 to 3 servings.
6. The method for preparing a micro-LTCC filter according to claim 4, It is characterized in that The solid content of the ceramic paste is 75-92wt%, and the viscosity of the ceramic paste is 100,000-600,000 Cp.
7. The method for preparing a micro-LTCC filter according to claim 1, It is characterized in that The drying temperature after printing each layer is 40-100°C and the drying time is 5-15 minutes.
8. The method for preparing a micro-LTCC filter according to claim 1, It is characterized in that The thickness of each layer is 5 to 120 μm.
9. The method for preparing a micro-LTCC filter according to claim 1, It is characterized in that The debinding temperature is 250-450° C. for 1-5 hours, and the sintering temperature is 850-950° C. for 1-5 hours.
10. The method for preparing a micro-LTCC filter according to claim 1, It is characterized in that The post-processing technology includes corner rolling, silver termination, sintering and electroplating.
Citation Information
Patent Citations
Low temperature co-fired ceramic (LTCC) filter production process and LTCC filter
CN102231452A
Low temperature co-fired ceramic method by mixed conductor structure
CN103601501A
LTCC filter capable of reducing layer thickness difference and preparation method thereof
CN114243238A
Surface gold conductor paste for low-temperature co-fired ceramic and preparation method of surface gold conductor paste
CN118412164A
Laminated circuit board and prodroduction method for electronic part, and laminated electronic part
CN1406385A
Cited By
LTCC (Low Temperature Co-Fired Ceramic) filter for inhibiting sintering shrinkage and preparation method thereof
CN121485619A