Composite material and preparation method thereof, photoelectric device and preparation method thereof, and display device

By connecting the fatty alcohol compounds with fluorine substituents on the surface of silica nanomaterials, the composite materials are prepared, which solves the problems of complex curing of ultraviolet glue and water-oxygen erosion, and achieves a high light-transmitting and hydrophobic packaging layer, extends the device life and Maintain luminous performance.

CN119031746APending Publication Date: 2024-11-26GUANGDONG JUHUA RES INST OF ADVANCED DISPLAY +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202310598899.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-24
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

The curing method of existing packaging materials is complex and has an impact on device performance, especially in water-oxygen environments that are prone to erosion.

Method used

By connecting a fatty alcohol compound with fluorine substituents on the surface of silica nanomaterials, a composite material was prepared, and nanoparticles and sheet-like nanomaterials were prepared by alkali catalytic or acid catalytic methods to form high light-transmittance and good hydrophobic properties. Encapsulation layer to avoid ultraviolet light.

Benefits of technology

It realizes a simple operation, environmentally friendly and curable packaging layer without ultraviolet light irradiation, improves water and oxygen barrier properties and anti-fouling characteristics, extends device life, and maintains high light transmission to avoid the impact on luminous performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119031746A_ABST
    Figure CN119031746A_ABST
Patent Text Reader

Abstract

The invention discloses a composite material and a preparation method thereof, a photoelectric device and a preparation method thereof, and a display device, the composite material comprises a silicon dioxide nanomaterial with the surface connected with a first compound, and the structural general formula of the first compound is R1-R2-R3; in the formula (I), R1 and R3 are respectively and independently selected from-CF3,-CHF2,-C (OH) F2,-CH2F,-CHF (OH) or-CH2OH; r2 comprises substituted or unsubstituted C3-C10 alkylene, and the substituent group is selected from-F or-OH; r1 to R3 contain at least one-F and at least one-OH. The invention aims to solve the problem that the ultraviolet glue curing mode of the existing packaging material is complicated.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of semiconductors, and in particular to a composite material and a preparation method thereof, an optoelectronic device and a preparation method thereof, and a display device. Background Art

[0002] For some devices that are extremely sensitive to water and oxygen, exposure to water and oxygen environments will greatly affect device performance. The packaging process can ensure that the device is effectively protected from water and oxygen corrosion. At present, UV glue curing is usually used to prepare the packaging layer. This UV glue requires ultraviolet light to cure, which is complicated to operate. In addition, ultraviolet light can easily affect device performance. Summary of the invention

[0003] In view of this, the present application provides a composite material and a preparation method thereof, an optoelectronic device and a preparation method thereof, and a display device, aiming to solve the problem of complex curing methods of UV glue of existing packaging materials.

[0004] The embodiment of the present application is implemented as follows:

[0005] In a first aspect, the present application provides a composite material, the composite material comprising a silicon dioxide nanomaterial having a first compound connected to the surface, the first compound having a general structural formula of R1-R2-R3;

[0006] Wherein, R1 and R3 are each independently selected from -CF3, -CHF2, -C(OH)F2, -CH2F, -CHF(OH) or -CH2OH; R2 includes substituted or unsubstituted C3~C10 alkylene, and the substituent is selected from -F or -OH; R1 to R3 contain at least one -F and at least one -OH.

[0007] Optionally, in some embodiments of the present application, in the composite material, the mass percentage of the first compound is 5-20%; and / or,

[0008] The light transmittance of the composite material is 80-95%; and / or,

[0009] R1 is selected from -CF3 or -CHF2; and / or,

[0010] R2 comprises a plurality of subunits interconnected to form the alkylene group, wherein each occurrence of the subunit is independently selected from one of -CH2-, -CF2-, and -CHF-; and / or,

[0011] R3 is selected from -CH2OH; and / or,

[0012] In the general structural formula of the first compound, the number of fluorine atoms is greater than or equal to 4.

[0013] Optionally, in some embodiments of the present application, the first compound includes one or more of CF3CF2(CH2)2CH2OH, CF3(CF2)5(CH2)5CH2OH, CF3(CF2)5CH2CH2OH, CF3(CF2)7CH2CH2OH, and CHF2(CF2)7CH2OH.

[0014] Optionally, in some embodiments of the present application, the silicon dioxide nanomaterial includes a first nanomaterial;

[0015] The morphology of the first nanomaterial includes a spherical shape; and / or,

[0016] The average particle size of the first nanomaterial is 5 to 60 nm; and / or,

[0017] In the composite material, the weight percentage of the first nano material is 60% to 95%.

[0018] Optionally, in some embodiments of the present application, the silicon dioxide nanomaterial includes a second nanomaterial, and the second nanomaterial has a morphology of flakes or blocks.

[0019] Optionally, in some embodiments of the present application, the composite material further includes a third nanomaterial, and the third nanomaterial includes flaky silicon dioxide or bulk silicon dioxide.

[0020] Optionally, in some embodiments of the present application, the first nanomaterial includes first nanoparticles and second nanoparticles, the average particle size of the first nanoparticles is 5 to 20 nm, and the average particle size of the second nanoparticles is 30 to 60 nm; in the first nanomaterial, the weight percentage of the first nanoparticles is 5% to 70%.

[0021] Optionally, in some embodiments of the present application, the composite material is composed of the first nanomaterial having the first compound connected to the surface and the second nanomaterial having the first compound connected to the surface.

[0022] In a second aspect, the present application also proposes a method for preparing a composite material, characterized in that it comprises the following steps:

[0023] Providing a first solution containing silicon dioxide nanomaterial and a first compound;

[0024] The first solution is mixed with the first compound to react to obtain a composite material;

[0025] Among them, the general structural formula of the first compound is R1-R2-R3; R1 and R3 are each independently selected from -CF3, -CHF2, -C(OH)F2, -CH2F, -CHF(OH) or -CH2OH; R2 includes substituted or unsubstituted C3~C10 alkylene, and the substituent is selected from -F or -OH; R1 to R3 contain at least one -F and at least one -OH.

[0026] Optionally, in some embodiments of the present application, the step of providing a first solution containing silicon dioxide nanomaterials comprises:

[0027] Providing a first silicon source, an alkaline catalyst and a first solvent; mixing the first silicon source, the alkaline catalyst and the first solvent, and performing a base-catalyzed reaction to obtain a first solution containing a silicon dioxide nanomaterial, wherein the silicon dioxide nanomaterial includes a first nanomaterial, and the shape of the first nanomaterial includes a sphere; and / or,

[0028] A second silicon source, an acidic catalyst and a second solvent are provided; the second silicon source, the acidic catalyst and the second solvent are mixed, and an acid-catalyzed reaction is performed to obtain a first solution containing a silicon dioxide nanomaterial, wherein the silicon dioxide nanomaterial includes a second nanomaterial, and the second nanomaterial has a morphology of flakes or blocks.

[0029] Optionally, in some embodiments of the present application, the first silicon source includes one or more of ethyl orthosilicate, methyl orthosilicate, and propyl orthosilicate; and / or,

[0030] The first compound includes one or more of 4,4,5,5,5-pentafluoropentanol, 6-perfluorohexylhexanol, 1H,1H,2H,2H-perfluoro-1-octanol, 2-perfluorooctylethanol, and 1H,1H,9H-hexafluorononanol; and / or,

[0031] The alkaline catalyst comprises aqueous ammonia; and / or,

[0032] The first solvent is selected from one or more of C1 to C5 alcohol solvents; and / or,

[0033] The molar ratio of the first silicon source to the alkaline catalyst is 90-99:10-1; and / or,

[0034] The volume ratio of the first silicon source to the first solvent is 1:9-11; and / or,

[0035] The base-catalyzed reaction time is 2 to 24 hours; and / or,

[0036] The acidic catalyst includes one or more of hydrochloric acid, sulfuric acid, hydroiodic acid, and hydrobromic acid; and / or,

[0037] The second silicon source includes one or more of ethyl orthosilicate, methyl orthosilicate, and propyl orthosilicate; and / or,

[0038] The second solvent is selected from one or more of C1 to C5 alcohol solvents; and / or,

[0039] The molar ratio of the second silicon source to the acidic catalyst is 90-98:10-2; and / or,

[0040] The acid-catalyzed reaction time is less than or equal to 2 hours; and / or,

[0041] The temperature of the acid catalyzed reaction is 10-30°C.

[0042] Optionally, in some embodiments of the present application, the silica nanomaterial includes a first nanomaterial; and after the step of mixing the first solution with the first compound and reacting, the step further includes: adding a third nanomaterial, wherein the third nanomaterial includes flaky silica or blocky silica.

[0043] Optionally, in some embodiments of the present application, the step of mixing the first silicon source, the alkaline catalyst and the first solvent to obtain a first solution containing a silicon dioxide nanomaterial by base-catalyzed reaction, wherein the silicon dioxide nanomaterial includes the first nanomaterial, comprises:

[0044] The first silicon source, the alkaline catalyst and the first solvent are mixed and reacted at 40 to 60° C. to obtain a first solution containing a silicon dioxide nanomaterial, wherein the silicon dioxide nanomaterial includes a first nanomaterial, and the first nanomaterial includes first nanoparticles with an average particle size of 5 to 20 nm; and / or,

[0045] The first silicon source, the alkaline catalyst and the first solvent are mixed and reacted at 70-100° C. to obtain a first solution containing silicon dioxide nanomaterials, wherein the silicon dioxide nanomaterials include first nanomaterials, and the first nanomaterials include second nanoparticles with an average particle size of 30-60 nm.

[0046] Optionally, in some embodiments of the present application, in the step of mixing the first solution with the first compound:

[0047] The mixing time is 1 to 24 hours; and / or,

[0048] The mixing temperature is 10 to 80° C.; and / or,

[0049] The ratio of the mass of the silicon dioxide nanomaterial in the first solution to the mass of the first compound is 80-98:20-2.

[0050] In a third aspect, the present application further proposes an optoelectronic device, comprising a device body and an encapsulation layer arranged on the surface of the device body, wherein the material of the encapsulation layer comprises the composite material described above, or a composite material prepared by the preparation method described above.

[0051] Optionally, in some embodiments of the present application, the thickness of the encapsulation layer is 10-100 nm; and / or,

[0052] The water contact angle of the encapsulation layer is 105° to 140°; and / or,

[0053] The roll angle of the encapsulation layer is 1-10°.

[0054] Optionally, in some embodiments of the present application, the composite material includes at least one of a third nanomaterial and a second nanomaterial having a first compound connected to its surface, and a first nanomaterial having a first compound connected to its surface;

[0055] The material of the encapsulation layer includes a mixture of at least one of a third nanomaterial and a second nanomaterial having a first compound connected to its surface, and a first nanomaterial having a first compound connected to its surface; or

[0056] The encapsulation layer includes a first encapsulation layer and a second encapsulation layer stacked in sequence in a direction away from the surface of the device body, the material of the first encapsulation layer includes a first nanomaterial with a first compound connected to the surface, and the material of the second encapsulation layer includes at least one of a third nanomaterial and a second nanomaterial with the first compound connected to the surface.

[0057] Optionally, in some embodiments of the present application, the device body includes a first electrode, a functional layer and a second electrode;

[0058] The first electrode and the second electrode are each independently selected from a doped metal oxide particle electrode, a composite electrode of metal and metal oxide, a graphene electrode, a carbon nanotube electrode, a metal electrode or an alloy electrode; the material of the doped metal oxide particle electrode is selected from one or more of indium-doped tin oxide, fluorine-doped tin oxide, antimony-doped tin oxide, aluminum-doped zinc oxide, gallium-doped zinc oxide, indium-doped zinc oxide, magnesium-doped zinc oxide and aluminum-doped magnesium oxide; the composite electrode of metal and metal oxide is selected from AZO / Ag / AZO, AZO / Al / AZO, ITO / Ag / ITO, ITO / Al / ITO, ZnO / Ag / ZnO, ZnO / Al / ZnO, TiO2 / Ag / TiO2, TiO2 / Al / TiO2, ZnS / Ag / ZnS, ZnS / Al / ZnS; the material of the metal electrode is selected from one or more of Ag, Al, Cu, Mo, Au, Pt, Si, Ca, Mg and Ba; and / or,

[0059] The functional layer includes a light-emitting layer, and the material of the light-emitting layer includes one or more selected from organic light-emitting materials and quantum dot light-emitting materials, and the organic light-emitting material is selected from 4,4'-bis(N-carbazole)-1,1'-biphenyl:tri[2-(p-tolyl)pyridine iridium(III), 4,4',4"-tri(carbazole-9-yl)triphenylamine:tri[2-(p-tolyl)pyridine iridium, diaromatic anthracene derivatives, distilbene aromatic derivatives, pyrene derivatives, fluorene derivatives, TBPe fluorescent materials, TTPX fluorescent materials, TBRb fluorescent materials, DBP fluorescent materials. The quantum dot luminescent material is selected from at least one of single structure quantum dots, core-shell structure quantum dots and perovskite semiconductor materials; the material of the single structure quantum dots, the core material of the core-shell structure quantum dots and the shell material of the core-shell structure quantum dots are selected from at least one of II-VI group compounds, IV-VI group compounds, III-V group compounds and I-III-VI group compounds. at least one; the II-VI group compound is selected from CdS, CdSe, CdTe, ZnS, ZnSe, ZnTe, ZnO, HgS, HgSe, HgTe, CdSeS, CdSeTe, CdSTe, ZnSeS, ZnSeTe, ZnSTe, HgSeS, HgSeTe, HgSTe, CdZnS, CdZnSe, CdZnTe, CdHgS, CdHgSe, CdHgTe, HgZnS, HgZnSe, HgZnTe, CdZnSeS, CdZnSeT e, CdZnSTe, CdHgSeS, CdHgSeTe, CdHgSTe, HgZnSeS, HgZnSeTe and HgZnSTe; the IV-VI group compound is selected from at least one of SnS, SnSe, SnTe, PbS, PbSe, PbTe, SnSeS, SnSeTe, SnSTe, PbSeS, PbSeTe, PbSTe, SnPbS, SnPbSe, SnPbTe, SnPbSSe, SnPbSeTe and SnPbSTe;The III-V compound is selected from the group consisting of GaN, GaP, GaAs, GaSb, AlN, AlP, AlAs, AlSb, InN, InP, InAs, InSb, GaNP, GaNAs, GaNSb, GaPAs, GaPSb, and AlN P, AlNAs, AlNSb, AlPAs, AlPSb, InNP, InNAs, InNSb, InPAs, InPSb, GaAlNP, GaAlNAs, GaAlNSb, GaAlPAs, GaAlPSb, GaInN P, GaInNAs, GaInNSb, GaInPAs, GaInPSb, InAlNP, InAlNAs, InAlNSb, InAlPAs and InAlPSb; the I-III-VI group compound is selected from at least one of CuInS2, CuInSe2 and AgInS2; the perovskite semiconductor material is selected from doped or undoped inorganic perovskite semiconductors, or organic-inorganic hybrid perovskite semiconductors; the inorganic perovskite semiconductor has a general structural formula of AMX3, wherein A is Cs; + ion, M is a divalent metal cation selected from Pb 2+ Sn 2+ , Cu 2+ 、Ni 2+ 、Cd 2+ Cr 2+ , Mn 2+ 、Co 2+ , Fe 2+ ,Ge 2+ , Yb 2+ 、Eu 2+ At least one of, X is a halogen anion selected from Cl - Br - ,I - At least one of the following; the general structural formula of the organic-inorganic hybrid perovskite semiconductor is BMX3, wherein B is an organic amine cation selected from CH3(CH2) n-2 NH3 + or [NH3(CH2) n NH3] 2+ , where n≥2, M is a divalent metal cation selected from Pb 2+ Sn 2+ , Cu 2+ 、Ni 2+ 、Cd 2+ Cr 2+ , Mn 2+ 、Co 2+ , Fe 2+ ,Ge 2+ , Yb 2+ 、Eu2+ At least one of, X is a halogen anion selected from Cl - Br - ,I - At least one of .

[0060] In a fourth aspect, the present application also proposes a method for preparing an optoelectronic device, comprising the following steps:

[0061] providing a device body, the device body comprising a first electrode, a functional layer, and a second electrode;

[0062] Providing a composite material, the composite material comprising the composite material described above, or a composite material prepared by the preparation method described above;

[0063] providing a third solvent, and dispersing the composite material in the third solvent to form a dispersion;

[0064] The dispersion is disposed on the surface of the device body to form a packaging layer, thereby obtaining a photoelectric device.

[0065] Optionally, in some embodiments of the present application, the third solvent includes one or more of C1 to C5 alcohol solvents; and / or,

[0066] In the dispersion, the concentration of the composite material is 5 to 30 mg / ml; and / or,

[0067] The dispersion is disposed on the surface of the device body by a spray coating method.

[0068] In a fifth aspect, the present application further proposes a display device, comprising the optoelectronic device as described above, or the optoelectronic device manufactured by the manufacturing method described above.

[0069] In the present application, by connecting the first compound to the surface of the silica nanomaterial, the surface energy of the material can be further reduced, higher hydrophobicity, higher water contact angle and rolling angle can be obtained, and its water and oxygen barrier performance, anti-fouling properties and self-cleaning properties can be improved; at the same time, the preparation process is not only simple to operate and environmentally friendly, but also does not require ultraviolet light irradiation and the curing method is simple. BRIEF DESCRIPTION OF THE DRAWINGS

[0070] In order to more clearly illustrate the technical solutions in the embodiments of the present application, the drawings required for use in the description of the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present application. For those skilled in the art, other drawings can be obtained based on these drawings without creative work.

[0071] Figure 1It is a schematic diagram of a process for preparing a composite material proposed in an embodiment of the present application;

[0072] Figure 2 is a schematic structural diagram of an optoelectronic device proposed in one embodiment of the present application;

[0073] Reference numerals:

[0074] 100 - photoelectric device; 10 - anode; 20 - light-emitting layer; 30 - electron transport layer; 40 - cathode; 50 - hole transport layer; 60 - hole injection layer; 70 - encapsulation layer. DETAILED DESCRIPTION

[0075] The technical solutions in the embodiments of the present application will be clearly and completely described below in conjunction with the drawings in the embodiments of the present application. Obviously, the described embodiments are only part of the embodiments of the present application, rather than all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by those skilled in the art without making creative work belong to the scope of protection of the present application. In addition, it should be understood that the specific implementation methods described herein are only used to illustrate and explain the present application, and are not used to limit the present application.

[0076] In this application, unless otherwise specified, the directional words used, such as "upper" and "lower", refer specifically to the directions of the drawings in the accompanying drawings. In addition, in the description of the specification of this application, the term "including" means "including but not limited to".

[0077] Various embodiments of the present application may be presented in the form of a range; it should be understood that the description in the form of a range is only for convenience and brevity, and should not be understood as a rigid limitation on the scope of the present application; therefore, the range description should be considered to have specifically disclosed all possible sub-ranges and single numerical values ​​within the range. For example, the range description from 1 to 6 should be considered to have specifically disclosed sub-ranges, such as from 1 to 3, from 1 to 4, from 1 to 5, from 2 to 4, from 2 to 6, from 3 to 6, etc., as well as single numbers within the range, such as 1, 2, 3, 4, 5 and 6, which apply regardless of the range. In addition, whenever a numerical range is indicated herein, it is meant to include any cited number (fractional or integer) within the indicated range.

[0078] In this application, "and / or" describes the association relationship of associated objects, indicating that there may be three relationships. For example, A and / or B can mean: A exists alone, A and B exist at the same time, and B exists alone. A and B can be singular or plural.

[0079] In the present application, "at least one" means one or more, and "plurality" means two or more. "At least one", "at least one of the following" or similar expressions refer to any combination of these items, including any combination of single items or plural items. For example, "at least one of a, b, or c", or "at least one of a, b, and c" can all mean: a, b, c, ab (i.e., a and b), ac, bc, or abc, where a, b, c can be single or multiple, respectively.

[0080] In a first aspect, an embodiment of the present application provides a composite material, wherein the composite material includes a silicon dioxide nanomaterial having a first compound connected to the surface.

[0081] In the present application, the first compound refers to a fatty alcohol having one or more fluorine substituents, and the fatty alcohol refers to an alcohol in which a hydroxyl group is connected to an aliphatic hydrocarbon group, and has a chain skeleton formed by connecting carbon atoms. Specifically, the general structural formula of the first compound is R1-R2-R3; wherein R1 and R3 are independently selected from -CF3, -CHF2, -C(OH)F2, -CH2F, -CHF(OH) or -CH2OH; R2 includes substituted or unsubstituted C3~C10 alkylene, and the substituent is selected from -F or -OH, wherein C3~10 means that the alkylene has 3 to 10 carbon atoms, and the alkylene refers to a group formed by a straight-chain alkane or a branched alkane losing two hydrogen atoms, and the two lost hydrogens can be hydrogens connected to the same carbon atom or hydrogens on different carbon atoms. For example, a butylene group with 4 carbon atoms can be -CH2(CH2)2CH2-, -CH2CH(CH3)2-, or -C(CH2CH2CH3)-, etc.; R1 to R3 contain at least one -F and at least one -OH. The surface of silica (SiO2) nanoparticles prepared by sol-gel method or hydrothermal method is usually connected with ligands such as hydroxyl groups. The first compound is connected with the ligands such as hydroxyl groups on the surface of the silica nanomaterial, thereby modifying the first compound on the surface of the silica nanomaterial.

[0082] In the present application, by connecting the first compound to the surface of the silica nanomaterial, the surface energy of the material can be further reduced, higher hydrophobicity, higher water contact angle and rolling angle can be obtained, and its water and oxygen barrier performance, anti-fouling properties and self-cleaning properties can be improved; at the same time, the preparation process is not only simple to operate and environmentally friendly, but also does not require ultraviolet light irradiation, thereby avoiding the influence of ultraviolet light on device performance.

[0083] In some embodiments, the total number of carbon atoms in the first compound is 5 to 12; for example, the first compound may be any first compound having 5, 6, 7, 8, 9, 10, 11 or 12 carbon atoms.

[0084] In some embodiments, R1 is selected from -CF3 or -CHF2; R2 includes a plurality of subunits interconnected to form the alkylene group, and each of the subunits is independently selected from one of -CH2-, -CF2-, and -CHF-; R3 is selected from -CH2OH. In the general structural formula of the first compound, the number of fluorine atoms is greater than or equal to 4, for example, 4, 5, 6, 7, 8, 10, 15, 21, and the like.

[0085] In some specific embodiments, the first compound is not limited to 4,4,5,5,5-pentafluoropentanol (chemical formula C5H7F5O; general structural formula CF3CF2(CH2)2CH2OH; CAS: 148043-73-6), 6-perfluorohexylhexanol (chemical formula C 12 H 13 F 13 O; general structural formula is CF3(CF2)5(CH2)5CH2OH; CAS: 161981-35-7), 1H,1H,2H,2H-perfluoro-1-octanol (chemical formula is C8H5F 13 O; the general structural formula is CF3(CF2)5CH2CH2OH; CAS: 647-42-7), 2-perfluorooctylethanol (chemical formula is C 10 H5F 17 O; general structural formula is CF3(CF2)7CH2CH2OH; CAS: 678-39-7), 1H,1H,9H-hexafluorononanol (chemical formula is C9H4F 16 O; the general structural formula is CHF2(CF2)7CH2OH; CAS: 376-18-1) or more thereof.

[0086] In some embodiments, in the composite material, the mass percentage of the first compound is 5-20%; for example, it can be 5%, 6%, 8%, 10%, 12%, 15%, 18%, 20% and values ​​between any two of the above values. Within this range, it helps to comprehensively improve the hydrophobicity and light transmittance of the material.

[0087] In some embodiments, the silica nanomaterial includes a first nanomaterial, which may be silica nanoparticles prepared by a base catalysis method, and the first nanomaterial is spherical in shape and has a relatively uniform particle size.

[0088] In some embodiments, the particle size of the first nanomaterial may be 5 to 60 nm, for example, 5 to 10 nm, 10 to 40 nm, 30 to 60 nm, 50 to 60 nm, and the like.

[0089] In the present application, a silicon dioxide nanomaterial having a first compound connected to its surface is proposed, and the silicon dioxide nanomaterial includes the first nanomaterial, and the first nanomaterial can be cross-linked with each other through ligands such as hydroxyl groups to form a thin film with a micro-nano rough structure, the thin film has good hydrophobicity, can block water and oxygen, and the obtained thin film also has high light transmittance, which helps to improve the effect of the encapsulation layer 70 on the optical properties of the device, especially when used to prepare the encapsulation layer 70 of the light-emitting device, its high light transmittance can effectively avoid the effect on the luminous performance of the light-emitting device, and obtain highly monochromatic RGB primary color light; at the same time, the preparation process is not only simple to operate, but also its synthesis can be carried out in green solvents such as alcohols, and it is environmentally friendly; since the process of preparing the encapsulation layer 70 using the composite material does not require ultraviolet light irradiation, there is no need to purchase additional ultraviolet equipment, which helps to reduce costs and can also avoid ultraviolet light affecting device performance; in addition, by connecting the first compound to the surface of the silicon dioxide nanomaterial, the surface energy of the material can be further reduced, and higher hydrophobicity, higher water contact angle and rolling angle can be obtained, and its water and oxygen blocking performance, anti-fouling properties and self-cleaning properties can be improved.

[0090] The first nanomaterial may be composed of a first nanomaterial of a single particle size, or may be composed of a first nanomaterial of multiple particle sizes. In some embodiments, the first nanomaterial includes a first nanoparticle and a second nanoparticle. The average particle size of the first nanoparticle is 5 to 20 nm, for example, it may be 5 nm, 6 nm, 8 nm, 10 nm, 12 nm, 13 nm, 14 nm, 15 nm, 16 nm, 18 nm, 20 nm, and a value between any two of the above values. The average particle size of the second nanoparticle is 30 to 60 nm; for example, it may be 30 nm, 32 nm, 35 nm, 38 nm, 40 nm, 45 nm, 49 nm, 50 nm, 53 nm, 55 nm, 60 nm, and a value between any two of the above values. By introducing nanoparticles of a specific particle size range and different particle sizes, it is helpful to significantly improve the surface roughness of the encapsulation film constructed of the composite material and improve its hydrophobic properties.

[0091] Further, in some embodiments, in the first nano material, the weight percentage of the first nanoparticles is 5% to 70%, for example, it can be 5%, 6%, 10%, 15%, 20%, 25%, 30%, 35%, 40%, 45%, 50%, 55%, 60%, 65%, 70% and values ​​between any two of the above values. It can be understood that in some embodiments, the first nano material is composed of first nanoparticles and second nanoparticles, the weight percentage of the first nanoparticles is 5% to 70%, and correspondingly, the weight percentage of the second nanoparticles is 95% to 30%, and the sum of the weight percentages of the two is 100%. The first nanoparticles and the second nanoparticles are mixed in a specific ratio, and the composite material obtained can construct a micro-nano rough structure when it is made into a film, further improving the hydrophobicity of the composite material and improving its resistance to water and oxygen.

[0092] In some embodiments, the light transmittance of the composite material is 80-95%, for example, 80%, 82%, 85%, 87%, 88%, 89%, 90%, 93%, 94%, 95% and any value between the above two values. The composite material has a high light transmittance and is suitable for the packaging process of the optoelectronic device 100.

[0093] In some other embodiments, the silicon dioxide nanomaterial includes a second nanomaterial, and the second nanomaterial includes flaky silicon dioxide or bulk silicon dioxide. The second nanomaterial can be prepared by an acid catalysis method.

[0094] In some other embodiments, when the composite material includes a first nanomaterial having a first compound connected to its surface, the composite material may further include a third nanomaterial, wherein the third nanomaterial includes flaky silicon dioxide or bulk silicon dioxide. Similarly, the third nanomaterial may be prepared by an acid catalysis method.

[0095] It can be understood that the composite material may include a first nanomaterial having a first compound connected to its surface; may include a second nanomaterial having the first compound connected to its surface; may include a first nanomaterial having the first compound connected to its surface, and a second nanomaterial having the first compound connected to its surface; may include a first nanomaterial having the first compound connected to its surface, and a third nanomaterial; may also include a first nanomaterial having the first compound connected to its surface, a second nanomaterial having the first compound connected to its surface, and a third nanomaterial.

[0096] It is understandable that when the composite material includes multiple materials, each material can be stored separately or mixed to form a mixture. Taking the composite material including a first nanomaterial with a first compound connected to the surface and a second nanomaterial with the first compound connected to the surface as an example, in actual application, the composite material can be a combination product consisting of the first nanomaterial with the first compound connected to the surface that can be stored independently and the second nanomaterial with the first compound connected to the surface that can be stored independently; it can also be a mixture obtained by mixing the first nanomaterial with the first compound connected to the surface and the silica nanoparticles with the first compound connected to the surface, which is not limited in this application.

[0097] In some embodiments, when the composite material contains, in addition to the first nanomaterial with the first compound connected to the surface, a third nanomaterial and / or the second nanomaterial with the first compound connected to the surface, the weight percentage of the first nanomaterial in the composite material is 60% to 95%; correspondingly, in the composite material, the weight percentage of the third nanomaterial and / or the second nanomaterial with the first compound connected to the surface is 5% to 40%, for example, it can be 5%, 6%, 10%, 15%, 20%, 25%, 30%, 35%, 40% and a value between any two of the above values. For example, when the composite material includes the first nanomaterial with the first compound connected to the surface, the second nanomaterial with the first compound connected to the surface, and the third nanomaterial, in the composite material, the weight percentage of the third nanomaterial is 5% to 40%, and the weight percentage of the second nanomaterial with the first compound connected to the surface is 5% to 40%, and the total weight percentage of the third nanomaterial and the second nanomaterial with the first compound connected to the surface is 5% to 40%. It can be understood that in some embodiments, the silica nanomaterial is composed of a first nanomaterial and silica nanoparticles, the weight percentage of the silica nanoparticles is 5% to 40%, and correspondingly, the weight percentage of the first nanomaterial is 95% to 60%, and the sum of the weight percentages of the two is 100%.

[0098] In some embodiments, the composite material includes at least one of a third nanomaterial and a second nanomaterial having a first compound connected to its surface, and a mixture of the first nanomaterial having a first compound connected to its surface. By introducing flaky silica or block silica, on the one hand, alkaline substances that may remain in the first nanomaterial can be neutralized to prevent the alkaline substances from reacting with the device film material and thereby affecting carrier transport. On the other hand, the second nanomaterial and the third nanomaterial are microscopically flaky or blocky, and when combined with the first nanomaterial, they can further construct a rough surface at the micro-nano level.

[0099] In the second aspect, the present application also proposes a method for preparing a composite material, see Figure 1 , the preparation method comprises the following steps:

[0100] S10, providing a first solution containing a silicon dioxide nanomaterial and a first compound;

[0101] S20, mixing the first solution and the first compound, reacting them to obtain a composite material.

[0102] In S10, the general structural formula of the first compound is R1-R2-R3; R1 and R3 are each independently selected from -CF3, -CHF2, -C(OH)F2, -CH2F, -CHF(OH) or -CH2OH; R2 includes a substituted or unsubstituted C3~C10 alkylene, and the substituent is selected from -F or -OH; R1 to R3 contain at least one -F and at least one -OH.

[0103] In some embodiments, the number of carbon atoms of the first compound is 5 to 12; the number of fluorine atoms is greater than or equal to 4; in other embodiments, the first compound includes one or more of 4,4,5,5,5-pentafluoropentanol, 6-perfluorohexylhexanol, 1H,1H,2H,2H-perfluoro-1-octanol, 2-perfluorooctylethanol, and 1H,1H,9H-hexafluorononanol.

[0104] In some embodiments, the silicon dioxide nanomaterial includes a first nanomaterial and / or a second nanomaterial. The first nanomaterial is a spherical silicon dioxide nanoparticle; the second nanomaterial is a flaky silicon dioxide or a bulk silicon dioxide.

[0105] In some embodiments, the composite material includes a first nanomaterial having a first compound connected to its surface; accordingly, the first solution includes the first nanomaterial. The step of providing the first solution containing the silicon dioxide nanomaterial includes: providing a first silicon source, an alkaline catalyst and a first solvent; mixing the first silicon source, the alkaline catalyst and the first solvent, and performing a base-catalyzed reaction to obtain the first solution containing the silicon dioxide nanomaterial, wherein the silicon dioxide nanomaterial includes the first nanomaterial, and the morphology of the first nanomaterial includes a sphere.

[0106] In some embodiments, the first silicon source includes one or more of ethyl orthosilicate, methyl orthosilicate, and propyl orthosilicate.

[0107] In some embodiments, the alkaline catalyst includes but is not limited to ammonia water, and the first nanomaterial can be prepared using ammonia water as a catalyst.

[0108] In some embodiments, the first solvent is used to provide a liquid reaction environment, which includes but is not limited to one or more of C1-C5 alcohol solvents, for example, methanol, ethanol, n-propanol, isopropanol, n-butanol, pentanol, and the like.

[0109] In some embodiments, the molar ratio of the first silicon source to the alkaline catalyst is 90-99:10-1, for example, 90:10, 91:9, 92:8, 93:7, 94:6, 95:5, 96:4, 97:3, 98:2, 99:1, etc. It can be understood that, based on the total molar amount of the first silicon source and the alkaline catalyst as 100%, the molar amount of the first silicon source accounts for 90-99%, and the remainder is the alkaline catalyst.

[0110] In some embodiments, the volume ratio of the first silicon source to the first solvent is 1:9-11, for example, 1:9, 1:9.2, 1:9.5, 1:10, 1:10.5, 1:11, and the like.

[0111] In some embodiments, the first silicon source, the alkaline catalyst and the first solvent are mixed, and a first solution containing silica nanomaterial is obtained by a base-catalyzed reaction, wherein the silica nanomaterial includes a first nanomaterial, and the time of the base-catalyzed reaction is 2 to 24 hours; for example, it can be 2 hours, 3 hours, 4 hours, 5 hours, 10 hours, 12 hours, 15 hours, 18 hours, 20 hours, 22 hours, 24 hours and values ​​between any two of the above values.

[0112] In some embodiments, the first silicon source, the alkaline catalyst and the first solvent are mixed, and a base-catalyzed reaction is performed to obtain a first solution containing a silica nanomaterial, wherein the silica nanomaterial includes a first nanomaterial. In the step, the temperature of the base-catalyzed reaction can be 40 to 100°C, for example, 40°C, 50°C, 60°C, 70°C, 80°C, 90°C, 100°C and values ​​between any two of the above values.

[0113] In some embodiments, the silicon dioxide nanomaterial may include a single type of silicon dioxide nanomaterial, for example, a first nanomaterial; it may also include flaky or block silicon dioxide, for example, a second nanomaterial; the silicon dioxide nanomaterial may also include a plurality of different silicon dioxide nanomaterials, for example, it may be composed of a first nanoparticle and a second nanoparticle, it may be composed of a first nanomaterial and a second nanomaterial of a single particle size, or it may be composed of a first nanoparticle, a second nanoparticle, and a second nanomaterial. According to different situations, different silicon dioxide nanomaterials are prepared according to different methods during actual preparation.

[0114] For example, in some embodiments, the silicon dioxide nanomaterial includes first nanoparticles and / or second nanoparticles, the first nanoparticles have an average particle size of 5 to 20 nm, and the second nanoparticles have an average particle size of 30 to 60 nm.

[0115] Specifically, in one embodiment, the silicon dioxide nanomaterial includes first nanoparticles. Accordingly, the first silicon source, the alkaline catalyst and the first solvent are mixed and reacted to obtain a first solution containing the silicon dioxide nanomaterial, and the step of the silicon dioxide nanomaterial including the first nanomaterial specifically includes: mixing the first silicon source, the alkaline catalyst and the first solvent, reacting at 40 to 60° C. to obtain a first solution containing the silicon dioxide nanomaterial, the silicon dioxide nanomaterial includes the first nanomaterial, and the first nanomaterial includes the first nanomaterial with an average particle size of 5 to 20 nm, that is, a solution containing the first nanoparticles is obtained.

[0116] In another embodiment, the silicon dioxide nanomaterial includes second nanoparticles. Accordingly, the first silicon source, the alkaline catalyst and the first solvent are mixed and reacted to obtain a first solution containing the silicon dioxide nanomaterial, and the step of the silicon dioxide nanomaterial including the first nanomaterial specifically includes: mixing the first silicon source, the alkaline catalyst and the first solvent, reacting at 70 to 100° C. to obtain a first solution containing the silicon dioxide nanomaterial, the silicon dioxide nanomaterial includes the first nanomaterial, and the first nanomaterial includes the first nanomaterial with an average particle size of 30 to 60 nm, that is, a solution containing the second nanoparticles is obtained.

[0117] In another embodiment, the silica nanomaterial includes first nanoparticles and second nanoparticles. Accordingly, the first silicon source, the alkaline catalyst and the first solvent are mixed and reacted to obtain a first solution containing the silica nanomaterial. The step of the silica nanomaterial including the first nanomaterial specifically includes: mixing the first silicon source, the alkaline catalyst and the first solvent, reacting at 40 to 60° C. to obtain a first solution containing the silica nanomaterial, the silica nanomaterial includes the first nanomaterial, the first nanomaterial includes the first nanomaterial with an average particle size of 5 to 20 nm, and thus obtaining a solution containing the first nanoparticles; mixing the first silicon source, the alkaline catalyst and the first solvent, reacting at 70 to 100° C. to obtain a first solution containing the silica nanomaterial, the silica nanomaterial includes the first nanomaterial, the first nanomaterial includes the first nanomaterial with an average particle size of 30 to 60 nm, and thus obtaining a solution containing the second nanoparticles; and mixing the solution containing the first nanoparticles with the solution containing the second nanoparticles.

[0118] For another example, in some embodiments, the composite material includes a second nanomaterial having a first compound connected to its surface, and accordingly, the silicon dioxide nanomaterial includes a second nanomaterial. Specifically, the step of providing a first solution containing a silicon dioxide nanomaterial includes: providing a second silicon source, an acidic catalyst, and a second solvent; mixing the second silicon source, the acidic catalyst, and the second solvent, and performing an acid-catalyzed reaction to obtain a solution containing the second nanomaterial, wherein the second nanomaterial has a morphology of flakes or blocks.

[0119] Wherein, the second silicon source includes one or more of ethyl orthosilicate, methyl orthosilicate, and propyl orthosilicate. The second solvent is used to provide a liquid reaction environment, which includes but is not limited to one or more of C1-C5 alcohol solvents, such as methanol, ethanol, n-propanol, isopropanol, n-butanol, amyl alcohol, etc. The acidic catalyst includes but is not limited to one or more of hydrochloric acid, sulfuric acid, hydroiodic acid, and hydrobromic acid.

[0120] In some embodiments, the molar ratio of the second silicon source to the acidic catalyst is 90-98:10-2; for example, it can be 90:10, 91:9, 92:8, 93:7, 94:6, 95:5, 96:4, 97:3, 98:2, etc. It can be understood that, based on the total molar amount of the second silicon source and the acidic catalyst as 100%, the molar amount of the second silicon source accounts for 90-99%, and the remainder is the acidic catalyst.

[0121] In some embodiments, the acid-catalyzed reaction time is less than or equal to 2 hours; for example, it can be 0.1 h, 0.2 h, 0.5 h, 0.6 h, 0.8 h, 0.9 h, 1 h, 1.3 h, 1.5 h, 1.8 h, 2 h, etc.

[0122] In some embodiments, the reaction temperature is 10-30°C; for example, it can be 10°C, 15°C, 20°C, 25°C, 30°C, and values ​​between any two of the above values.

[0123] In some embodiments, when the composite material includes a first nanomaterial having a first compound connected to its surface and a second nanomaterial having a second compound connected to its surface, the first solution contains both the first nanomaterial and the second nanomaterial. Specifically, after preparing a solution containing the first nanomaterial and a solution containing the second nanomaterial, the two are mixed to obtain a solution containing two types of silicon dioxide nanomaterials at the same time, that is, the first solution. The first solution is used in step S20 to obtain a composite material containing both the first nanomaterial having the first compound connected to its surface and the second nanomaterial having the second compound connected to its surface.

[0124] In step S20:

[0125] In some embodiments, the ratio of the mass of the silica nanomaterial in the first solution to the mass of the first compound is 80-98:20-2. For example, it can be 80:20, 82:18, 85:15, 90:10, 93:7, 95:5, 98:2, etc. It can be understood that, based on the total mass of the silica nanomaterial and the first compound as 100%, the mass percentage of the silica nanomaterial is 80-98%, and the remainder is the first compound; in addition, when the silica nanomaterial contains multiple types of silica nanomaterials, the mass of the silica nanomaterial refers to the total mass of all types of silica nanomaterials.

[0126] In some embodiments, the mixing time is 1 to 24 hours; for example, it can be 1 hour, 2 hours, 3 hours, 4 hours, 5 hours, 10 hours, 12 hours, 15 hours, 18 hours, 20 hours, 22 hours, 24 hours, and values ​​between any two of the above values.

[0127] In some embodiments, the mixing temperature can be 10-80°C, for example, 10°C, 20°C, 30°C, 40°C, 50°C, 60°C, 70°C, 80°C and values ​​between any two of the above values.

[0128] In some embodiments, the composite material also includes a third nanomaterial, and the third nanomaterial includes flaky silicon dioxide or bulk silicon dioxide. The preparation method of the third nanomaterial can refer to the preparation method of the second nanomaterial mentioned above, that is, it is prepared by acid catalyst reaction, and its detailed steps are not repeated here. In this embodiment, when performing step S20, after the step of mixing the first solution with the first compound and reacting, it also includes: adding a third nanomaterial, and the third nanomaterial includes flaky silicon dioxide or bulk silicon dioxide. In this way, a composite material containing at least a third nanomaterial and a first nanomaterial with a first compound connected to the surface can be obtained.

[0129] In a third aspect, the present application further proposes an optoelectronic device 100, wherein the optoelectronic device 100 includes but is not limited to a light emitting device, a photovoltaic cell and a photodetector, see Figure 2 The optoelectronic device 100 includes a device body and an encapsulation layer 70 disposed on the surface of the device body. The material of the encapsulation layer 70 includes the composite material described above, or a composite material prepared by the preparation method described above.

[0130] The optoelectronic device 100 proposed in the present application uses the above-mentioned composite material to make the encapsulation layer 70, which can not only effectively block water and oxygen, avoid water and oxygen erosion, and help extend the life, but also the encapsulation layer 70 has a high light transmittance and has little impact on the luminous effect of the device; in addition, when the composite material is used to prepare the encapsulation layer 70, the operation is simple, the cost is low, and the environmental friendliness is high.

[0131] In some embodiments, the thickness of the encapsulation layer 70 is 10 to 100 nm; for example, it can be 10 nm, 20 nm, 30 nm, 40 nm, 50 nm, 60 nm, 70 nm, 80 nm, 90 nm, 100 nm, and a value between any two of the above values.

[0132] In some embodiments, the water contact angle of the encapsulation layer 70 is 105° to 140°; for example, it can be 105°, 106°, 110°, 115°, 120°, 125°, 130°, 135°, 140°, and values ​​between any two of the above values. The water contact angle refers to the angle between the tangent of the solid-liquid interface at the intersection of the liquid and solid phases when water is dropped onto the surface of the encapsulation layer, and the part of the tangent on the liquid side and the solid-liquid boundary line. The encapsulation layer 70 has a higher water contact angle, and has better water and oxygen barrier properties, anti-fouling properties, and self-cleaning properties.

[0133] In some embodiments, the roll angle of the encapsulation layer 70 is 1-10°; for example, it can be 1°, 2°, 3°, 4°, 5°, 6°, 7°, 8°, 9°, 10°, and any value between the above two values. The encapsulation layer 70 has good water and oxygen barrier properties, anti-fouling properties, and self-cleaning properties.

[0134] In some embodiments, the composite material is a combination product consisting of an independently existing third nanomaterial and / or an independently existing second nanomaterial having a first compound connected to its surface, and an independently existing first nanomaterial having a first compound connected to its surface. When using it to prepare the encapsulation layer 70, the components can be mixed to prepare a single encapsulation layer 70, or different films can be prepared in sequence to construct a plurality of stacked encapsulation film layers. As an example, in some embodiments, the encapsulation layer 70 includes a first encapsulation layer and a second encapsulation layer stacked in sequence in a direction away from the surface of the device body, the material of the first encapsulation layer includes a first nanomaterial having a first compound connected to its surface, and the material of the second encapsulation layer includes at least one of a third nanomaterial and a second nanomaterial having a first compound connected to its surface. In another embodiment, the encapsulation layer 70 is a single film layer, and its material includes at least one of a third nanomaterial and a second nanomaterial having a first compound connected to its surface, and a mixture of a first nanomaterial having a first compound connected to its surface.

[0135] The device body includes a first electrode, a functional layer, and a second electrode. The first electrode is one of the cathode 40 and the anode 10 , and the second electrode is the other of the cathode 40 and the anode 10 .

[0136] The anode 10 may be an anode 10 for a photoelectric device 100 known in the art, for example, may be selected from but not limited to a doped metal oxide particle electrode, a composite electrode of a metal and a metal oxide, a graphene electrode, a carbon nanotube electrode, a metal electrode or an alloy electrode, the material of the doped metal oxide particle electrode is selected from one or more of indium-doped tin oxide, fluorine-doped tin oxide, antimony-doped tin oxide, aluminum-doped zinc oxide, gallium-doped zinc oxide, indium-doped zinc oxide, magnesium-doped zinc oxide and aluminum-doped magnesium oxide, the composite electrode of a metal and a metal oxide is selected from AZO / Ag / AZO, AZO / Al / AZO, ITO / Ag / ITO, ITO / Al / ITO, ZnO / Ag / ZnO, ZnO / Al / ZnO, TiO2 / Ag / TiO2, TiO2 / Al / TiO2, ZnS / Ag / ZnS, ZnS / Al / ZnS, and the material of the metal electrode is selected from one or more of Ag, Al, Cu, Mo, Au, Pt, Si, Ca, Mg and Ba.

[0137] The cathode 40 can be a cathode 40 for the optoelectronic device 100 known in the art, for example, can be selected from but not limited to a doped metal oxide particle electrode, a composite electrode of metal and metal oxide, a graphene electrode, a carbon nanotube electrode, a metal electrode or an alloy electrode, the material of the doped metal oxide particle electrode is selected from one or more of indium-doped tin oxide, fluorine-doped tin oxide, antimony-doped tin oxide, aluminum-doped zinc oxide, gallium-doped zinc oxide, indium-doped zinc oxide, magnesium-doped zinc oxide and aluminum-doped magnesium oxide, the composite electrode of metal and metal oxide is selected from AZO / Ag / AZO, AZO / Al / AZO, ITO / Ag / ITO, ITO / Al / ITO, ZnO / Ag / ZnO, ZnO / Al / ZnO, TiO2 / Ag / TiO2, TiO2 / Al / TiO2, ZnS / Ag / ZnS, ZnS / Al / ZnS, and the material of the metal electrode is selected from one or more of Ag, Al, Cu, Mo, Au, Pt, Si, Ca, Mg and Ba.

[0138] In some embodiments, the functional layer includes a light-emitting layer 20, and the light-emitting layer 20 may be an organic light-emitting layer or a quantum dot light-emitting layer. When the light-emitting layer 20 is an organic light-emitting layer, the optoelectronic device 100 may be an organic light-emitting device; when the light-emitting layer 20 is a quantum dot light-emitting layer, the optoelectronic device 100 may be a quantum dot light-emitting device.

[0139] The material of the organic light-emitting layer is a material known in the art for the organic light-emitting layer of the optoelectronic device 100, for example, it can be selected from but not limited to 4,4'-bis(N-carbazole)-1,1'-biphenyl:tri[2-(p-tolyl)pyridine iridium(III), 4,4',4"-tri(carbazole-9-yl)triphenylamine:tri[2-(p-tolyl)pyridine iridium, diaromatic anthracene derivatives, distilbene aromatic derivatives, pyrene derivatives, fluorene derivatives, TBPe fluorescent materials, TTPX fluorescent materials, TBRb fluorescent materials, DBP fluorescent materials, delayed fluorescent materials, TTA materials, thermally activated delayed materials, polymers containing BN covalent bonds, hybrid localized charge transfer excited state materials, and exciplex light-emitting materials. One or more of the following.

[0140] The material of the quantum dot light-emitting layer is a quantum dot material known in the art for the quantum dot light-emitting layer of the optoelectronic device 100, for example, it can be selected from but not limited to at least one of a single structure quantum dot, a core-shell structure quantum dot and a perovskite semiconductor material; the material of the single structure quantum dot, the core material of the core-shell structure quantum dot and the shell material of the core-shell structure quantum dot are respectively selected from at least one of II-VI group compounds, IV-VI group compounds, III-V group compounds and I-III-VI group compounds; the II-VI group compound is selected from CdS, CdSe, CdTe, ZnS, ZnSe, ZnTe, ZnO, Hg At least one of S, HgSe, HgTe, CdSeS, CdSeTe, CdSTe, ZnSeS, ZnSeTe, ZnSTe, HgSeS, HgSeTe, HgSTe, CdZnS, CdZnSe, CdZnTe, CdHgS, CdHgSe, CdHgTe, HgZnS, HgZnSe, HgZnTe, CdZnSeS, CdZnSeTe, CdZnSTe, CdHgSeS, CdHgSeTe, CdHgSTe, HgZnSeS, HgZnSeTe and HgZnSTe; the IV-VI group compounds The compound is selected from at least one of SnS, SnSe, SnTe, PbS, PbSe, PbTe, SnSeS, SnSeTe, SnSTe, PbSeS, PbSeTe, PbSTe, SnPbS, SnPbSe, SnPbTe, SnPbSSe, SnPbSeTe, and SnPbSTe; the III-V compound is selected from at least one of GaN, GaP, GaAs, GaSb, AlN, AlP, AlAs, AlSb, InN, InP, InAs, InSb, GaNP, GaNAs, GaNSb, GaPAs, GaPSb, and AlNP , AlNAs, AlNSb, AlPAs, AlPSb, InNP, InNAs, InNSb, InPAs, InPSb, GaAlNP, GaAlNAs, GaAlNSb, GaAlPAs, GaAlPSb, GaInNP, GaInNAs, GaInNSb, GaInPAs, GaInPSb, InAlNP, InAlNAs, InAlNSb, InAlPAs and InAlPSb; the I-III-VI group compound is selected from at least one of CuInS2, CuInSe2 and AgInS2.

[0141] As an example, the core-shell structured quantum dots may be selected from but not limited to at least one of CdZnSe / CdZnSe / ZnSe / CdZnS / ZnS, CdZnSe / CdZnSe / CdZnS / ZnS CdSe / CdSeS / CdS, InP / ZnSeS / ZnS, CdZnSe / ZnSe / ZnS, CdSeS / ZnSeS / ZnS, CdSe / ZnS, CdSe / ZnSe / ZnS, ZnSe / ZnS, ZnSeTe / ZnS, CdSe / CdZnSeS / ZnS and InP / ZnSe / ZnS.

[0142] It should be noted that, for the material of the aforementioned single structure quantum dot, or the material of the core of the core-shell structure quantum dot, or the material of the shell of the core-shell structure quantum dot, the chemical formula provided only indicates the elemental composition, but does not indicate the content of each element. For example, CdZnSe only indicates that it is composed of three elements, Cd, Zn and Se. If the content of each element is indicated, it corresponds to Cd x Zn 1-x Se,0 <x<1。

[0143] The perovskite semiconductor material may be selected from but not limited to doped or undoped inorganic perovskite semiconductors, or organic-inorganic hybrid perovskite semiconductors; the inorganic perovskite semiconductor has a general structural formula of AMX3, wherein A is Cs + ion, M is a divalent metal cation selected from Pb 2+ Sn 2+ , Cu 2+ 、Ni 2+ 、Cd 2+ Cr 2+ , Mn 2+ 、Co 2+ , Fe 2+ ,Ge 2+ , Yb 2+ 、Eu 2+ At least one of, X is a halogen anion selected from Cl - Br - ,I - At least one of the following; the general structural formula of the organic-inorganic hybrid perovskite semiconductor is BMX3, wherein B is an organic amine cation selected from CH3(CH2) n-2 NH3 + or [NH3(CH2) n NH3] 2+ , where n≥2, M is a divalent metal cation selected from Pb 2+ Sn 2+ , Cu 2+ 、Ni 2+ 、Cd2+ Cr 2+ , Mn 2+ 、Co 2+ , Fe 2+ ,Ge 2+ , Yb 2+ 、Eu 2+ At least one of, X is a halogen anion selected from Cl - Br - ,I - At least one of .

[0144] The functional layer further includes one or two layers of a hole transport layer 50 and a hole injection layer 60. When the functional layer includes a stacked hole transport layer 50 and a hole injection layer 60, the hole injection layer 60 is located between the hole transport layer 50 and the anode 10. The hole functional layer can be prepared using a material with hole transport properties known in the art for use in an optoelectronic device 100. For example, the material of the hole transport layer 50 is not limited to 4,4'-N,N'-dicarbazolyl-biphenyl, N,N'-diphenyl-N,N'-bis(1-naphthyl)-1,1'-biphenyl-4,4"-diamine, N,N'-diphenyl-N,N'-bis(3-methylphenyl)-(1,1'-biphenyl)-4,4'-diamine, N,N'-bis(3-methylphenyl)-N,N'-bis(phenyl)-spiro, N,N'-bis(4-(N,N'-diphenyl-amino)phenyl)-N,N'-diphenylbenzidine, 4,4',4'-tri(N-carbazolyl)-triphenylamine ... 4',4'-Tris(N-3-methylphenyl-N-phenylamino)triphenylamine, poly[(9,9'-dioctylfluorene-2,7-diyl)-co-(4,4'-(N-(4-sec-butylphenyl)diphenylamine))], poly(4-butylphenyl-diphenylamine), polyaniline, polypyrrole, poly(p-phenylenevinylene), poly(phenylenevinylene), poly[2-methoxy-5-(2-ethylhexyloxy)-1,4-phenylenevinylene] and poly[2-methoxy-5-(3',7'-dimethyloctyloxy)-1,4-phenylenevinylene], copper phthalocyanine, aromatic tertiary amines, polynuclear aromatic tertiary amines , 4,4'-bis(p-carbazolyl)-1,1'-biphenyl compounds, N,N,N',N'-tetraaryl benzidine, PEDOT:PSS and its derivatives, poly(N-vinyl carbazole) and its derivatives, polymethacrylate and its derivatives, poly(9,9-octylfluorene) and its derivatives, poly(spirofluorene) and its derivatives, N,N'-di(naphthalene-1-yl)-N,N'-diphenyl benzidine, spiro NPB, doped graphene, undoped graphene, C60, doped or undoped NiO, doped or undoped MoO3, doped or undoped WO3, doped or undoped V2O5, doped or undoped P-type gallium nitride, doped or undoped CrO3, doped or undoped CuO. The material of the hole injection layer 60 includes, but is not limited to, at least one of 2,3,6,7,10,11-hexacyano-1,4,5,8,9,12-hexaazatriphenylene, PEDOT, PEDOT:PSS, PEDOT:PSS doped with s-MoO3 derivatives, 4,4',4'-tris(N-3-methylphenyl-N-phenylamino)triphenylamine, tetracyanoquinodimethane, copper phthalocyanine, nickel oxide, molybdenum oxide, tungsten oxide, vanadium oxide, molybdenum sulfide, tungsten sulfide and copper oxide.

[0145] The functional layer includes one or both of the electron transport layer 30 and the electron injection layer. When the functional layer includes the stacked electron transport layer 30 and the electron injection layer, the electron injection layer is located between the electron transport layer 30 and the cathode 40. The electronic functional layer can be prepared using materials with electron transport properties known in the art for use in optoelectronic devices 100. For example, the material of the electron transport layer 30 includes, but is not limited to, one or more of metal oxides, doped metal oxides, IIB-VIA group materials, IIIB-VA group materials and IB-IIIB-VIA group materials; the metal oxides include one or more of ZnO, TiO2, SnO2, Al2O3, V2O5, V3O8, CrO3, WO3, Fe2O3, Fe3O4, CuO, MoO2, Nb2O5, BaO, MoO3, CdO, BaO, Ta2O5, BaTiO3, and PbCrO4; the metal oxides in the doped metal oxides include one or more of ZnO, TiO2, SnO2, V2O5, V3O8, CrO3, WO3 , Fe2O3, Fe3O4, CuO, MoO2, Nb2O5, BaO, MoO3, CdO, BaO, Ta2O5, BaTiO3, PbCrO4, the doping elements include one or more of Al, Mg, Li, In, Ga; the IIB-VIA group semiconductor materials include one or more of ZnS, ZnSe, CdS, CdSe; the IIIB-VA group semiconductor materials include one or more of InP, GaP; the IB-IIIB-VIA group semiconductor materials include one or more of CuInS, CuGaS; the material of the electron injection layer includes but is not limited to at least one of cesium carbonate, cesium fluoride, cesium azide and lithium fluoride.

[0146] When the functional layer is provided with multiple film layers, and the multiple film layers are selected from the light-emitting layer 20, the electron injection layer, the electron transport layer 30, the hole transport layer 50, and the hole injection layer 60, the film layer stacking order of the photoelectric device 100 is the anode 10, the hole injection layer 60, the hole transport layer 50, the light-emitting layer 20, the electron transport layer 30, the electron injection layer and the cathode 40; it can be understood that the photoelectric device 100 can be an upright device or an inverted device. In some embodiments, the photoelectric device 100 is an upright device, and accordingly, the photoelectric device 100 includes an anode 10, a hole injection layer 60, a hole transport layer 50, a light-emitting layer 20, an electron transport layer 30, an electron injection layer and a cathode 40 stacked in sequence from bottom to top; in other embodiments, the photoelectric device 100 is an inverted device, and accordingly, the photoelectric device 100 includes a cathode 40, an electron injection layer, an electron transport layer 30, a light-emitting layer 20, a hole transport layer 50, a hole injection layer 60 and an anode 10 stacked in sequence from bottom to top.

[0147] It is understandable that the optoelectronic device 100 may also be provided with some functional layers conventionally used in optoelectronic devices 100 that help improve the performance of the optoelectronic device 100, such as an electron blocking layer, a hole blocking layer, an interface modification layer, etc.

[0148] It can be understood that the materials of each layer of the optoelectronic device 100 can be adjusted according to the actual requirements of the optoelectronic device 100 .

[0149] In a fourth aspect, the present application further provides a method for preparing an optoelectronic device 100, the method comprising the following steps:

[0150] S10, providing a device body, wherein the device body includes a first electrode, a functional layer, and a second electrode;

[0151] S20, providing a composite material, wherein the composite material includes the composite material described above, or a composite material prepared by the preparation method described above;

[0152] S30, providing a third solvent, and dispersing the composite material in the third solvent to form a dispersion;

[0153] S40 , disposing the dispersion on the surface of the device body to form an encapsulation layer 70 , thereby obtaining the optoelectronic device 100 .

[0154] In some embodiments, the third solvent includes one or more of C1-C5 alcohol solvents, such as methanol, ethanol, n-propanol, isopropanol, n-butanol, pentanol, etc. The above solvents can not only disperse the composite material well to prepare a uniform film layer, but also evaporate easily. After being sprayed into a liquid film, the solvent can evaporate naturally to form the encapsulation layer 70.

[0155] In some embodiments, in the dispersion, the concentration of the composite material is 5 to 30 mg / ml; for example, 5 mg / ml, 8 mg / ml, 10 mg / ml, 15 mg / ml, 20 mg / ml, 30 mg / ml and values ​​between any two of the above values.

[0156] In some embodiments, the dispersion is disposed on the surface of the device body by spraying, which is simple to operate and low in cost.

[0157] In some embodiments, step S40 may be performed in an environment where both the oxygen content and the water content are lower than 0.1 ppm, which helps to ensure the stability of the optoelectronic device 100 .

[0158] In the preparation method of the optoelectronic device 100, the preparation method of the anode 10, the light-emitting layer 20, the electron injection layer, the electron transport layer 30, the hole transport layer 50, the hole injection layer 60 and the cathode 40 can be achieved by conventional techniques in the art, such as chemical methods or physical methods. Among them, the chemical method includes chemical vapor deposition, continuous ion layer adsorption and reaction, anodization, electrolytic deposition, and coprecipitation. The physical method includes physical plating and solution method, among which the physical plating method includes: thermal evaporation coating, electron beam evaporation coating, magnetron sputtering, multi-arc ion plating, physical vapor deposition, atomic layer deposition, pulsed laser deposition, etc.; the solution method can be spin coating, printing, inkjet printing, blade coating, printing, dip pulling, immersion, spraying, roll coating, casting, slit coating, strip coating, etc.

[0159] In a fourth aspect, the present application further proposes a display device, which may be a smart phone, a portable phone, a tablet computer, a personal digital assistant (PDA), a portable multimedia player (Portable Multimedia Player), a television, a game console, a watch-type electronic device, a head-mounted display, a display of a personal computer, a notebook computer, a car navigation system, a car dashboard, a digital camera, a portable camera, an external advertising board, an electro-optical board, a medical device, a detection device, a refrigerator, a washing machine, etc. The display device includes the optoelectronic device 100 as described above.

[0160] The technical scheme and technical effects of the present application are described in detail below through specific embodiments and comparative examples. The following embodiments are only some embodiments of the present application and do not specifically limit the present application.

[0161] Example 1

[0162] The composite material of this embodiment is spherical silicon dioxide nanoparticles with the first compound connected to the surface.

[0163] The preparation method of the composite material is as follows:

[0164] (1) Tetraethyl orthosilicate, ammonia water and ethanol are mixed and reacted at 60° C. for 8 hours to obtain a mixed solution, wherein the mixed solution contains a first nanomaterial with an average particle size of 15 nm; wherein the molar ratio of tetraethyl orthosilicate to ammonia water is 95:5.

[0165] (2) The mixed solution and 6-perfluorohexyl alcohol are mixed at 25° C. for 4 hours in a ratio of 90:10 between the total mass of the silica nanomaterial in the mixed solution and the mass of the first compound to obtain spherical silica nanoparticles with 6-perfluorohexyl alcohol connected to the surface, thereby obtaining a composite material.

[0166] (3) The composite material obtained in step (2) is dispersed in ethanol to prepare a composite material solution with a concentration of 10 mg / ml for later use.

[0167] Example 2

[0168] The scheme of this embodiment is basically the same as that of embodiment 1, except that, in this embodiment, the first compound connected to the surface of the silica spherical nanoparticles is 4,4,5,5,5-pentafluoropentanol. Accordingly, in step (2):

[0169] The first compound was changed to 4,4,5,5,5-pentafluoropentanol.

[0170] The other steps and parameters remain unchanged.

[0171] Example 3

[0172] The scheme of this embodiment is basically the same as that of embodiment 1, except that, in this embodiment, the first compound connected to the surface of the silica spherical nanoparticles is 1H, 1H, 2H, 2H-perfluoro-1-octanol and 6-perfluorohexylhexanol. Accordingly, in step (2):

[0173] The first compound is changed to a mixture of 1H,1H,2H,2H-perfluoro-1-octanol and 6-perfluorohexylhexanol, and the molar ratio of the two is 1:1.

[0174] The other steps and parameters remain unchanged.

[0175] Example 4

[0176] The scheme of this embodiment is basically the same as that of embodiment 1, except that, in this embodiment, in the composite material, the spherical silica nanoparticles include first nanoparticles and second nanoparticles, the average particle size of the first nanoparticles is 5 to 20 nm, and the average particle size of the second nanoparticles is 30 to 60 nm. Accordingly, step (1) is changed to:

[0177] Tetraethyl orthosilicate, ammonia water and ethanol were mixed and reacted at 60° C. for 8 hours to obtain a solution containing first nanoparticles with an average particle size of 15 nm; wherein the molar ratio of tetraethyl orthosilicate to ammonia water was 95:5.

[0178] Tetraethyl orthosilicate, ammonia water and ethanol were mixed and reacted at 80° C. for 8 hours to obtain a solution containing second nanoparticles with an average particle size of 60 nm; wherein the molar ratio of tetraethyl orthosilicate to ammonia water was 95:5.

[0179] The two solutions are mixed in a weight ratio of 1:1 between the first nanoparticles and the second nanoparticles to prepare a mixed solution for use in the subsequent step (2).

[0180] In step (2), the ratio of the total mass of the silicon dioxide nanomaterial in the mixed solution to the mass of the first compound is adjusted accordingly to the ratio of the total mass of the first nanomaterials of the two particle sizes to the mass of the first compound.

[0181] The other steps and parameters remain unchanged.

[0182] Example 5

[0183] The scheme of this embodiment is basically the same as that of embodiment 1, except that in this embodiment, in the composite material, the silicon dioxide nanomaterial further comprises flaky silicon dioxide nanoparticles formed by acid catalysis. Accordingly, step (1) is changed to:

[0184] Tetraethyl orthosilicate, ammonia water and ethanol are mixed and reacted at 60° C. for 8 hours to obtain a base-catalyzed mixed solution, wherein the base-catalyzed mixed solution contains a first nanomaterial with an average particle size of 15 nm; wherein the molar ratio of tetraethyl orthosilicate to ammonia water is 95:5.

[0185] Tetraethyl orthosilicate, hydrochloric acid and ethanol are mixed and reacted at 25° C. for 1.5 hours to obtain an acid-catalyzed mixed solution, wherein the acid-catalyzed mixed solution contains flaky silicon dioxide nanoparticles; wherein the molar ratio of tetraethyl orthosilicate to the acid catalyst is 95:5.

[0186] The two solutions were mixed in a weight ratio of 80:20 between the first nanomaterial and the silicon dioxide nanoparticles to prepare a mixed solution for use in the subsequent step (2).

[0187] In step (2), the ratio of the total mass of the silicon dioxide nanomaterial in the mixed solution to the mass of the first compound is adjusted accordingly to the ratio of the total mass of the two silicon dioxide nanomaterials to the mass of the first compound.

[0188] The other steps and parameters remain unchanged.

[0189] Example 6

[0190] The scheme of this embodiment is basically the same as that of embodiment 1, except that, in this embodiment, the silicon dioxide nanomaterial in the composite material is composed of a first nanomaterial formed by base catalysis and flaky silicon dioxide nanoparticles formed by acid catalysis, and the spherical silicon dioxide nanoparticles include first nanoparticles and second nanoparticles, the average particle size of the first nanoparticles is 5 to 20 nm, and the average particle size of the second nanoparticles is 30 to 60 nm. Accordingly, step (1) is changed to:

[0191] Tetraethyl orthosilicate, ammonia water and ethanol were mixed and reacted at 60° C. for 8 hours to obtain a solution containing first nanoparticles with an average particle size of 15 nm; wherein the molar ratio of tetraethyl orthosilicate to ammonia water was 95:5.

[0192] Tetraethyl orthosilicate, ammonia water and ethanol were mixed and reacted at 80° C. for 8 hours to obtain a solution containing second nanoparticles with an average particle size of 60 nm; wherein the molar ratio of tetraethyl orthosilicate to ammonia water was 95:5.

[0193] The two solutions were mixed at a weight ratio of 1:1 between the first nanoparticles and the second nanoparticles to obtain a spherical particle mixture.

[0194] Tetraethyl orthosilicate, hydrochloric acid and ethanol are mixed and reacted at 25° C. for 1.5 hours to obtain an acid-catalyzed mixed solution, wherein the acid-catalyzed mixed solution contains flaky silicon dioxide nanoparticles; wherein the molar ratio of tetraethyl orthosilicate to the acid catalyst is 95:5.

[0195] The two solutions were mixed in a weight ratio of 80:20 between the first nanomaterial and the flaky silica nanoparticles to prepare a mixed solution for use in the subsequent step (2).

[0196] In step (2), the ratio of the total mass of the silicon dioxide nanomaterials in the mixed solution to the mass of the first compound is adjusted accordingly to the ratio of the total mass of the above three silicon dioxide nanomaterials to the mass of the first compound.

[0197] The other steps and parameters remain unchanged.

[0198] Example 7

[0199] The scheme of this embodiment is basically the same as that of embodiment 6, except that, in this embodiment, the mass percentage of the first compound in the composite material is 5%. Accordingly, in step (2):

[0200] The ratio of the total mass of the silicon dioxide nanomaterial to the mass of the first compound in the mixed solution is changed to 95:5.

[0201] The other steps and parameters remain unchanged.

[0202] Example 8

[0203] The scheme of this embodiment is basically the same as that of embodiment 6, except that, in this embodiment, the mass percentage of the first compound in the composite material is 20%. Accordingly, in step (2):

[0204] The ratio of the total mass of the silicon dioxide nanomaterial to the mass of the first compound in the mixed solution was changed to 80:20.

[0205] The other steps and parameters remain unchanged.

[0206] Example 9

[0207] The scheme of this embodiment is basically the same as that of embodiment 6, except that, in this embodiment, the mass percentage of the first compound in the composite material is 25%. Accordingly, in step (2):

[0208] The ratio of the total mass of the silicon dioxide nanomaterial to the mass of the first compound in the mixed solution was changed to 75:25.

[0209] The other steps and parameters remain unchanged.

[0210] Example 10

[0211] The scheme of this embodiment is basically the same as that of Embodiment 6, except that, in this embodiment, the weight percentage of the first nanoparticles in the spherical particle mixture is 5%. Accordingly, in step (1), the mixing weight ratio of the first nanoparticles to the second nanoparticles is changed to 5:95.

[0212] The other steps and parameters remain unchanged.

[0213] Embodiment 11

[0214] The scheme of this embodiment is basically the same as that of Embodiment 6, except that, in this embodiment, in the spherical particle mixture, the weight percentage of the first nanoparticles is 70%. Accordingly, in step (1), the mixing weight ratio of the first nanoparticles to the second nanoparticles is changed to 70:30.

[0215] The other steps and parameters remain unchanged.

[0216] Example 12

[0217] The scheme of this embodiment is basically the same as that of Embodiment 6, with the only difference being that, in this embodiment, in the spherical particle mixture, the weight percentage of the first nanoparticles is 75%. Accordingly, in step (1), the mixing weight ratio of the first nanoparticles to the second nanoparticles is changed to 75:25.

[0218] The other steps and parameters remain unchanged.

[0219] Example 13

[0220] The scheme of this embodiment is basically the same as that of embodiment 6, except that, in this embodiment, the weight percentage of the flaky silica nanoparticles formed by acid catalysis is 5%, and accordingly, in step (1), the mixing weight ratio of the first nanomaterial and the flaky silica nanoparticles is changed to 95:5.

[0221] The other steps and parameters remain unchanged.

[0222] Embodiment 14

[0223] The scheme of this embodiment is basically the same as that of embodiment 6, except that, in this embodiment, the weight percentage of the flaky silica nanoparticles formed by acid catalysis is 40%, and accordingly, in step (1), the mixing weight ratio of the first nanomaterial and the flaky silica nanoparticles is changed to 60:40.

[0224] The other steps and parameters remain unchanged.

[0225] Embodiment 15

[0226] The scheme of this embodiment is basically the same as that of embodiment 6, except that, in this embodiment, the weight percentage of the flaky silica nanoparticles formed by acid catalysis is 50%, and accordingly, in step (1), the mixing weight ratio of the first nanomaterial and the flaky silica nanoparticles is changed to 50:50.

[0227] The other steps and parameters remain unchanged.

[0228] Example 16

[0229] The scheme of this embodiment is basically the same as that of embodiment 1, except that the present embodiment is a sheet-like silica nanoparticle with 6-perfluorohexylhexanol attached to the surface. Accordingly, in the preparation method of this embodiment, step (1) is changed to:

[0230] Tetraethyl orthosilicate, hydrochloric acid and ethanol are mixed and reacted at 25° C. for 1.5 hours to obtain an acid-catalyzed mixed solution, wherein the acid-catalyzed mixed solution contains flaky silicon dioxide nanoparticles; wherein the molar ratio of tetraethyl orthosilicate to the acid catalyst is 95:5.

[0231] The other steps and parameters remain unchanged.

[0232] Comparative Example 1

[0233] The comparative example is basically the same as Example 1, except that the comparative example is SiO2 nanoparticles without surface modification. Accordingly, in the preparation method of the comparative example:

[0234] 1. Omit step (2);

[0235] 2. The first nanomaterial with an average particle size of 15 nm obtained in step (1) is directly used in step (3) to obtain a SiO2 nanoparticle solution with a concentration of 10 mg / ml for later use.

[0236] Comparative Example 2

[0237] The comparative example is basically the same as Example 16, except that the comparative example is a flaky silicon dioxide nanoparticle without surface modification. Accordingly, the preparation method of the comparative example is:

[0238] 1. Omit step (2);

[0239] 2. The flaky silicon dioxide nanoparticles obtained in step (1) are directly used in step (3) to obtain a SiO2 solution with a concentration of 10 mg / ml for later use.

[0240] The other steps and parameters remain unchanged.

[0241] Comparative Example 3

[0242] This comparative example is UV glue-polyacrylate.

[0243] Comparative Example 4

[0244] This comparative example is a conventional organic polymer packaging material - polymethyl methacrylate (PMMA).

[0245] The composite material solutions prepared in the examples and comparative examples 1-2 were sprayed on a glass substrate to form a film layer with a thickness of 100 nm.

[0246] The ultraviolet adhesive of comparative example 3 was coated on a glass substrate and irradiated with UV for 10 minutes to form a film layer with a thickness of 100 nm.

[0247] The polymethyl methacrylate of Comparative Example 4 was coated on a glass substrate, and after solidification, a film layer with a thickness of 100 nm was formed.

[0248] The transmittance, water contact angle and sliding angle of the film layer were measured using UV-visible absorption spectroscopy and contact angle measuring instrument, and the results are recorded in Table 1.

[0249] Table 1

[0250]

[0251]

[0252] It can be seen from Table 1 that:

[0253] Comparing Examples 1 to 15 with Comparative Examples 1 and 3, and comparing Example 16 with Comparative Example 2, each Example has a higher water contact angle and a lower rolling angle than the corresponding comparative examples, indicating that the composite material proposed in the present application has better hydrophobic properties than silica nanoparticles, silica nanoparticles and ultraviolet glue, and is more suitable for encapsulation of optoelectronic devices;

[0254] Compared with Comparative Example 4, each embodiment has a higher light transmittance, and the light transmittance is between 82% and 90%, indicating that the composite material proposed in the present application has a high light transmittance and can be used to prepare a high light transmittance film. When used to prepare the encapsulation layer of an optoelectronic device, the light emitting effect thereof can be avoided from being affected.

[0255] Compared with Example 1, Examples 4 and 6 have higher water contact angles and lower sliding angles, indicating that by using nanoparticles of different particle sizes, the surface roughness of the encapsulation layer constructed by silica nanoparticles can be improved, thereby improving the hydrophobic performance; Compared with Example 1, Examples 4 and 5 have higher water contact angles and lower sliding angles, indicating that the introduction of acid-catalyzed silica can further construct a rough surface at the micro-nano level, thereby obtaining more excellent hydrophobicity.

[0256] Device Example 1

[0257] The patterned ITO glass substrate was placed in acetone, washing liquid, deionized water, and isopropanol for ultrasonic cleaning in order, and each ultrasonic cleaning time was 20 minutes. After cleaning, it was blown dry with a nitrogen gun. Then, the ITO glass substrate was placed in oxygen plasma for further cleaning for 10 minutes, and then the surface of the ITO glass substrate was treated with ultraviolet-ozone for 15 minutes to obtain an anode with an anode thickness of 100 nm.

[0258] (2) In air, a layer of PEDOT:PSS was spin-coated on the surface of the anode at a speed of 3000 r / min for 30 seconds, and then annealed at 150°C for 20 minutes to obtain a hole injection layer with a thickness of 25 nm. After annealing, the substrate was transferred to a glove box filled with nitrogen atmosphere.

[0259] (3) TFB was spin-coated on the surface of the hole injection layer at a speed of 3000 r / min for 30 s, and then annealed at 180° C. for 30 min to obtain a hole transport layer with a thickness of 25 nm.

[0260] (4) After the semi-finished product obtained in step (3) is cooled, 20 mg / ml of green quantum dot material CdSe is spin-coated on the surface of the hole transport layer at a speed of 1500 r / min for 30 s, and then annealed at a temperature of 100° C. for 5 min to obtain a light-emitting layer with a thickness of 25 nm.

[0261] (5) A ZnO ethanol solution with a concentration of 30 mg / ml was spin-coated on the surface of the light-emitting layer at a speed of 3000 r / min for 30 s, and then annealed at a temperature of 100° C. for 15 min to obtain an electron transport layer with a thickness of 40 nm.

[0262] (6) The semi-finished product obtained in step (5) is placed in a vacuum chamber, and a layer of Al with a thickness of 100 nm is evaporated on the surface of the electron transport layer as a cathode to obtain a device body.

[0263] (7) The composite material solution prepared in Example 1 was uniformly sprayed on the surface of the device body by spraying to form an encapsulation layer with a thickness of 100 nm.

[0264] Device Examples 2 to 16

[0265] The scheme of device embodiment m is basically the same as that of device embodiment 1, except that in device embodiment m, in step (6), the composite material solution used is the composite material solution prepared in embodiment m, wherein m is 2 to 16.

[0266] Device Example 17

[0267] The scheme of device embodiment 17 is basically the same as that of device embodiment 1, except that, in device embodiment 17, step (6) is changed to:

[0268] The composite material solution prepared in Example 1 is uniformly sprayed on the surface of the device body by spraying to form a first encapsulation layer with a thickness of 80 nm;

[0269] Take the flaky silica nanoparticles prepared in Example 5, disperse them in ethanol, and prepare an acid-catalyzed particle solution with a concentration of 10 mg / ml; then, spray the acid-catalyzed particle solution evenly on the surface of the device body by spraying to form a second encapsulation layer with a thickness of 20 nm.

[0270] The first encapsulation layer and the second encapsulation layer together constitute an encapsulation layer.

[0271] Device Comparison Examples 1 to 2

[0272] The scheme of device comparative example n is basically the same as that of device embodiment 1, except that in device comparative example n, in step (6), the composite material solution used is the composite material solution prepared in comparative example n, wherein n is 1 to 2.

[0273] Device Comparison Example 3

[0274] The scheme of the device comparative example is basically the same as that of device embodiment 1, except that, in the device comparative example, step (6) is changed to:

[0275] The ultraviolet glue of comparative example 3 was coated on the surface of the device body, irradiated with UV for 10 minutes, and cured to form an encapsulation layer with a thickness of 100 nm.

[0276] Device Comparison Example 4

[0277] The scheme of the device comparative example is basically the same as that of device embodiment 1, except that, in the device comparative example, step (6) is changed to:

[0278] The polymethyl methacrylate of Comparative Example 4 was formed into an encapsulation layer having a thickness of 100 nm.

[0279] The devices prepared in the above device embodiments and device comparative examples were tested, and the results were recorded in Table 2. The test method is as follows:

[0280] (1) The optical property measurement equipment of FPD (including Ocean Optics USB2000, LabView controlled QE-PRO spectrometer, Keithley 2400, high-precision digital source meter Keithley 6485, optical fiber with an inner diameter of 50 μm, device test probes and fixtures, various related connecting wires and data cards, efficiency test cassettes and data acquisition systems) was used to detect the parameters of each optoelectronic device, such as the start-up voltage, current, brightness (L), and luminescence spectrum. Then, key parameters such as external quantum efficiency and power efficiency were calculated, and the service life of each of the above optoelectronic devices was tested using life test equipment.

[0281] (2) The test method for service life is as follows: under the drive of constant current (2mA), a 128-channel QLED life test system is used to analyze the electroluminescent life of each optoelectronic device, and the time required for each optoelectronic device to decay from the maximum brightness to 95% (T95, h) is recorded. The time required for the brightness of each optoelectronic device to decay from 100% to 95% at a brightness of 1000nit is calculated by the decay fitting formula (T95@1000nit, h).

[0282] Table 2

[0283]

[0284]

[0285] Refer to Table 2, we can see that:

[0286] Compared with device comparative examples 1 to 4, each device embodiment has a longer lifespan, indicating that the composite material proposed in the present application for preparing the encapsulation layer has a better water and oxygen resistance effect than silicon dioxide nanoparticles, silicon dioxide nanoparticles and ultraviolet glue, which helps to extend the service life of the device; at the same time, the device embodiment has a higher brightness than the device comparative example 4, indicating that the encapsulation layer of the present application has a relatively smaller impact on the luminous effect of the device;

[0287] Compared with device embodiment 1, device embodiments 4 and 6 have a longer lifespan, indicating that by using nanoparticles of different particle sizes, the surface roughness of the encapsulation layer constructed by silica nanoparticles can be improved, the hydrophobic performance can be improved, and the lifespan of the device can be improved; compared with device embodiment 1, device embodiments 4 and 5 have a longer lifespan, and compared with device embodiment 16, device embodiment 6 has a longer lifespan, indicating that the introduction of acid-catalyzed silica can further construct a rough surface at the micro-nano level and obtain more excellent hydrophobicity, thereby improving the lifespan of the device; at the same time, introducing acid-catalyzed silica before spraying can also neutralize the residual ammonia water in the silica nanoparticles, reduce the adverse effects of ammonia water on the electrode, and further extend the lifespan.

[0288] The composite materials and preparation methods thereof, optoelectronic devices and preparation methods thereof, and display devices provided in the embodiments of the present application are introduced in detail above. Specific examples are used herein to illustrate the principles and implementation methods of the present application. The description of the above embodiments is only used to help understand the methods and core ideas of the present application. At the same time, for technical personnel in this field, according to the ideas of the present application, there will be changes in the specific implementation methods and application scopes. In summary, the content of this specification should not be understood as a limitation on the present application.

Claims

1. A composite material, characterized in that: The composite material comprises a silicon dioxide nanomaterial having a first compound connected to the surface, wherein the first compound has a general structural formula of R1-R2-R3; wherein R1 and R3 are each independently selected from -CF3, -CHF2, -C(OH)F2, -CH2F, -CHF(OH) or -CH2OH; R2 includes substituted or unsubstituted C3-C10 alkylene, and the substituent is selected from -F or -OH; R1 to R3 contain at least one -F and at least one -OH.

2. The composite material according to claim 1, characterized in that In the composite material, the mass percentage of the first compound is 5 to 20%; and / or, The light transmittance of the composite material is 80-95%; and / or, R1 is selected from -CF3 or -CHF2; and / or, R2 comprises a plurality of subunits interconnected to form the alkylene group, wherein each occurrence of the subunit is independently selected from one of -CH2-, -CF2-, and -CHF-; and / or, R3 is selected from -CH2OH; and / or, In the general structural formula of the first compound, the number of fluorine atoms is greater than or equal to 4.

3. The composite material according to claim 2, characterized in that The first compound includes one or more of CF3CF2(CH2)2CH2OH, CF3(CF2)5(CH2)5CH2OH, CF3(CF2)5CH2CH2OH, CF3(CF2)7CH2CH2OH, and CHF2(CF2)7CH2OH.

4. The composite material according to claim 1, characterized in that The silicon dioxide nanomaterial includes a first nanomaterial; The morphology of the first nanomaterial includes a spherical shape; and / or, The average particle size of the first nanomaterial is 5 to 60 nm; and / or, In the composite material, the weight percentage of the first nano material is 60% to 95%.

5. The composite material according to claim 1 or 4, characterized in that: The silicon dioxide nanomaterial includes a second nanomaterial, and the second nanomaterial has a form of flake or block.

6. The composite material according to claim 4, characterized in that The composite material further includes a third nanomaterial, and the third nanomaterial includes flaky silicon dioxide or bulk silicon dioxide.

7. The composite material according to claim 4, characterized in that The first nano material includes first nano particles and second nano particles, the average particle size of the first nano particles is 5-20 nm, and the average particle size of the second nano particles is 30-60 nm; in the first nano material, the weight percentage of the first nano particles is 5%-70%.

8. A method for preparing a composite material, characterized in that: The following steps are involved: Providing a first solution containing silicon dioxide nanomaterial and a first compound; The first solution is mixed with the first compound to react to obtain a composite material; Among them, the general structural formula of the first compound is R1-R2-R3; R1 and R3 are each independently selected from -CF3, -CHF2, -C(OH)F2, -CH2F, -CHF(OH) or -CH2OH; R2 includes substituted or unsubstituted C3~C10 alkylene, and the substituent is selected from -F or -OH; R1 to R3 contain at least one -F and at least one -OH.

9. The preparation method according to claim 8, characterized in that: The step of providing a first solution containing silicon dioxide nanomaterials comprises: Providing a first silicon source, an alkaline catalyst and a first solvent; mixing the first silicon source, the alkaline catalyst and the first solvent, and performing a base-catalyzed reaction to obtain a first solution containing a silicon dioxide nanomaterial, wherein the silicon dioxide nanomaterial includes a first nanomaterial, and the shape of the first nanomaterial includes a sphere; and / or, A second silicon source, an acidic catalyst and a second solvent are provided; the second silicon source, the acidic catalyst and the second solvent are mixed, and an acid-catalyzed reaction is performed to obtain a first solution containing a silicon dioxide nanomaterial, wherein the silicon dioxide nanomaterial includes a second nanomaterial, and the second nanomaterial has a morphology of flakes or blocks.

10. The preparation method according to claim 9, characterized in that: The first silicon source includes one or more of ethyl orthosilicate, methyl orthosilicate, and propyl orthosilicate; and / or, The first compound includes one or more of 4,4,5,5,5-pentafluoropentanol, 6-perfluorohexylhexanol, 1H,1H,2H,2H-perfluoro-1-octanol, 2-perfluorooctylethanol, and 1H,1H,9H-hexafluorononanol; and / or, The alkaline catalyst comprises aqueous ammonia; and / or, The first solvent is selected from one or more of C1 to C5 alcohol solvents; and / or, The molar ratio of the first silicon source to the alkaline catalyst is 90-99:10-1; and / or, The volume ratio of the first silicon source to the first solvent is 1:9-11; and / or, The base-catalyzed reaction time is 2 to 24 hours; and / or, The acidic catalyst includes one or more of hydrochloric acid, sulfuric acid, hydroiodic acid, and hydrobromic acid; and / or, The second silicon source includes one or more of ethyl orthosilicate, methyl orthosilicate, and propyl orthosilicate; and / or, The second solvent is selected from one or more of C1 to C5 alcohol solvents; and / or, The molar ratio of the second silicon source to the acidic catalyst is 90-98:10-2; and / or, The acid-catalyzed reaction time is less than or equal to 2 hours; and / or, The temperature of the acid catalyzed reaction is 10-30°C.

11. The preparation method according to claim 9, characterized in that: The silicon dioxide nanomaterial comprises a first nanomaterial; and after the step of mixing the first solution with the first compound and reacting, the step further comprises: adding a third nanomaterial, wherein the third nanomaterial comprises flaky silicon dioxide or block silicon dioxide.

12. The preparation method according to claim 9, characterized in that: The step of mixing the first silicon source, the alkaline catalyst and the first solvent to obtain a first solution containing a silicon dioxide nanomaterial by a base-catalyzed reaction, wherein the silicon dioxide nanomaterial includes the first nanomaterial comprises: The first silicon source, the alkaline catalyst and the first solvent are mixed and reacted at 40 to 60° C. to obtain a first solution containing a silicon dioxide nanomaterial, wherein the silicon dioxide nanomaterial includes a first nanomaterial, and the first nanomaterial includes first nanoparticles with an average particle size of 5 to 20 nm; and / or, The first silicon source, the alkaline catalyst and the first solvent are mixed and reacted at 70-100° C. to obtain a first solution containing silicon dioxide nanomaterials, wherein the silicon dioxide nanomaterials include first nanomaterials, and the first nanomaterials include second nanoparticles with an average particle size of 30-60 nm.

13. The preparation method according to claim 8, characterized in that: In the step of mixing the first solution with the first compound: The mixing time is 1 to 24 hours; and / or, The mixing temperature is 10 to 80° C.; and / or, The ratio of the mass of the silicon dioxide nanomaterial in the first solution to the mass of the first compound is 80-98:20-2.

14. A photoelectric device, characterized in that: It comprises a device body and a packaging layer arranged on the surface of the device body, wherein the material of the packaging layer comprises the composite material according to any one of claims 1 to 7, or the composite material prepared by the preparation method according to any one of claims 8 to 13.

15. The optoelectronic device according to claim 14, characterized in that: The thickness of the encapsulation layer is 10 to 100 nm; and / or, The water contact angle of the encapsulation layer is 105° to 140°; and / or, The roll angle of the encapsulation layer is 1-10°.

16. The optoelectronic device according to claim 14, characterized in that: The composite material includes at least one of a third nanomaterial and a second nanomaterial having a first compound connected to the surface, and a first nanomaterial having the first compound connected to the surface; The material of the encapsulation layer includes a mixture of at least one of a third nanomaterial and a second nanomaterial having a first compound connected to its surface, and a first nanomaterial having a first compound connected to its surface; or The encapsulation layer includes a first encapsulation layer and a second encapsulation layer stacked in sequence in a direction away from the surface of the device body, the material of the first encapsulation layer includes a first nanomaterial with a first compound connected to the surface, and the material of the second encapsulation layer includes at least one of a third nanomaterial and a second nanomaterial with the first compound connected to the surface.

17. A method for preparing a photoelectric device, characterized in that: The following steps are involved: Providing a device body; Provide a composite material, the composite material comprising the composite material according to any one of claims 1 to 7, or a composite material prepared by the preparation method according to any one of claims 8 to 13; providing a third solvent, and dispersing the composite material in the third solvent to form a dispersion; The dispersion is disposed on the surface of the device body to form a packaging layer, thereby obtaining a photoelectric device.

18. The preparation method according to claim 17, characterized in that: The third solvent includes one or more of C1-C5 alcohol solvents; and / or, In the dispersion, the concentration of the composite material is 5 to 30 mg / ml; and / or, The dispersion is disposed on the surface of the device body by a spray coating method.

19. A display device, characterized in that: The invention comprises a photoelectric device as claimed in any one of claims 14 to 16, or a photoelectric device prepared by the preparation method according to claim 17 or 18.