Amphiphobic coating and method for preparing amphiphobic coating

By forming a layer of silica nanoparticles on the polymer substrate by oxygen plasma treatment and pulse laser deposition, and forming a fluoroalkyl silane layer thereon, the manufacturing problem of transparent double-splitting coating on the polymer substrate is solved. A double sporadic coating with high transparency, fingerprint-proof and self-cleaning properties is achieved, suitable for thermally sensitive materials and improves mechanical strength and adhesion.

CN119032011APending Publication Date: 2024-11-26NANYANG TECH UNIV
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202380035134.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-04-19
Filing Date
2023-04-18
Publication Date
2024-11-26

AI Technical Summary

Technical Problem

The prior art is difficult to manufacture transparent double-splitting coatings on polymer substrates, especially since the high-temperature calcination process is not suitable for thermally sensitive polymer materials, and the mechanical stability and adhesion challenges are great, resulting in ultra double-splitting and high permeability. It is difficult to achieve light rate.

Method used

Using a polymer substrate treated with oxygen plasma, a layer of silica nanoparticles is directly deposited by pulsed laser deposition, and a fluoroalkyl silane layer is formed thereon, achieving a superhydrophobic and oleophobic double-spervious coating.

Benefits of technology

A double sporadic coating with high transparency, anti-fingerprint, anti-reflection and self-cleaning properties on polymer substrates is realized, and the preparation method is suitable for ambient conditions or room temperature, suitable for thermally sensitive materials, and improves the mechanical strength and adhesiveness of the coating. Adhesion.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119032011A_ABST
    Figure CN119032011A_ABST
Patent Text Reader

Abstract

An amphiphobic coating is provided. The amphiphobic coating includes: a polymeric substrate having an oxygen plasma treated surface; a silica layer comprising silica nanoparticles disposed directly on the oxygen plasma treated surface; and a fluoroalkylsilane layer disposed directly on the silica layer. A method of preparing the amphiphobic coating and uses thereof are also provided.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] CROSS-REFERENCE TO RELATED APPLICATIONS

[0002] This application claims priority to Singapore Patent Application No. 10202204021P filed on April 19, 2022, the contents of which are hereby incorporated by reference in their entirety for all purposes. Technical Field

[0003] Various embodiments relate to amphiphobic coatings, methods of making amphiphobic coatings, uses of the coatings, and articles comprising the coatings. Background Art

[0004] Good light transmission and surface cleanliness are among the most important requirements for optical products such as lenses, screens and protective covers. However, these requirements are difficult to meet because during handling or service, optical products can easily become contaminated with contaminants such as fingerprints, skin oil residues and dust particles, which can affect the transparency and sometimes even the aesthetic value of the product.

[0005] To mitigate the effects of such problems, surface modifications have been extensively studied. For example, surfaces with high anti-wetting properties to both water and oil (called superamphiphobic surfaces) have attracted great interest in recent years in order to endow surfaces with anti-fingerprint and self-cleaning properties.

[0006] Although nature has inspired us with examples of superhydrophobic surfaces such as lotus leaves, insect legs and wings, and strategies have been developed to construct superhydrophobic surfaces, it is still challenging to make superamphiphobic surfaces because the surface tension of oil is much lower than that of water. This makes it difficult to achieve surfaces that are both water-repellent and oil-repellent.

[0007] For optical products, the challenge also lies in the potential conflict between amphiphobicity and transparency requirements. To achieve superamphiphobicity, high surface roughness is usually desired. However, transmittance may decrease with increasing surface roughness due to increased light scattering. Therefore, it is challenging to achieve both superamphiphobicity and high transmittance at the same time.

[0008] Polymer optical lenses have attracted widespread attention due to their advantages such as light weight, strong resistance to mechanical impact, and easy to form complex shapes, especially for applications in the medical and consumer product fields. A substantial growth in the demand for polymer materials to replace oxide glass has been observed. There is a need to make the surface of polymer materials self-cleaning and anti-fingerprint while maintaining high light transmittance. However, due to the challenges associated with the low melting point of polymer materials and their inert chemical properties, there is little work on the manufacture of transparent amphiphobic coatings on polymer substrates. Most of the developed manufacturing methods require high-temperature calcination processes, which are not suitable for heat-sensitive polymer materials. In addition, mechanical stability, especially the adhesion between the coating and the substrate, remains the main challenge faced by coatings on polymer substrates.

[0009] In view of the above, there is still a need for an improved coating and method for preparing the coating to overcome or at least alleviate one or more of the above problems. Summary of the invention

[0010] In a first aspect, various embodiments are directed to an amphiphobic coating comprising: a polymer substrate having a surface treated with oxygen plasma; a silicon dioxide layer containing silicon dioxide nanoparticles disposed directly on the surface treated with oxygen plasma; and a fluoroalkylsilane layer disposed directly on the silicon dioxide layer.

[0011] In a second aspect, various embodiments relate to a method for preparing an amphiphobic coating. The method includes: providing a polymer substrate having a surface treated with oxygen plasma; directly depositing silicon dioxide on the surface treated with oxygen plasma by pulsed laser deposition to form a silicon dioxide layer containing silicon dioxide nanoparticles; and directly depositing a fluoroalkyl silane on the silicon dioxide layer to form a fluoroalkyl silane layer on the silicon dioxide layer.

[0012] In a third aspect, various embodiments relate to an amphiphobic coating prepared by the method of the second aspect.

[0013] In a fourth aspect, various embodiments relate to the use of the amphiphobic coating according to the first aspect or the amphiphobic coating prepared by the method according to the second aspect in an anti-reflective coating, an anti-fingerprint coating, an anti-fouling coating, a self-cleaning surface, a surface primer layer, an optical element, a sensor, a lens, a goggles, a mirror, a windshield, a mask, a display, a window or a cooker cover.

[0014] In a fifth aspect, various embodiments relate to an article comprising an amphiphobic coating according to the first aspect or an amphiphobic coating prepared by the method according to the second aspect, wherein the article is an optical element, a sensor, a lens, a goggles, a mirror, a windshield, a mask, a display, a window or a cooker cover. BRIEF DESCRIPTION OF THE DRAWINGS

[0015] In the accompanying drawings, like reference characters generally refer to the same parts in different views. The accompanying drawings are not necessarily drawn to scale, but generally emphasize the principles of various embodiments. In the following description, various embodiments of the present invention will be described with reference to the accompanying drawings.

[0016] Figure 1 1 is a schematic diagram of preparing an amphiphilic coating 100 according to an embodiment. In the illustrated embodiment, a polymer substrate 101 is provided. The polymer substrate 101 may be subjected to processing conditions 112 of cleaning with deionized (DI) water and ethanol, and subjected to surface treatment with oxygen plasma. This may increase surface roughness and change the surface chemistry of the surface 103 treated with oxygen plasma, resulting in more oxygen bonding. Silicon dioxide (SiO2) may be deposited directly on the surface 103 treated with oxygen plasma by pulsed laser deposition 114 to form an ultra-hydrophilic film 105 of silica nanoparticles having a large number of hydroxyl groups on the surface of the ultra-hydrophilic film 105. The ultra-hydrophilic film 105 of the silica nanoparticles may be treated with fluoroalkyl silane 116. The fluoroalkyl silane may self-assemble and react with the hydroxyl groups on the surface of the ultra-hydrophilic film 105 of the silica nanoparticles to form a fluoroalkyl silane layer 107. An ultra-hydrophobic and oleophobic amphiphilic coating 100 may be formed.

[0017] In an exemplary embodiment, a polycarbonate substrate is provided. The polycarbonate substrate is cleaned with deionized (DI) water and ethanol, and surface treated with oxygen plasma for about 15 minutes. This can increase surface roughness and change the surface chemistry of the surface treated with oxygen plasma, producing more oxygen bonding. Silicon dioxide (SiO2) is directly deposited on the surface treated with oxygen plasma for about 60 minutes using pulsed laser deposition to form a super-hydrophilic film of silicon dioxide nanoparticles with a large amount of hydroxyl groups on the surface of the super-hydrophilic film. The super-hydrophilic film of silicon dioxide nanoparticles is treated with trichloro (1H, 1H, 2H, 2H-perfluorooctyl) silane (PFTS) for about 10 minutes and heated for about 2 hours. Trichloro (1H, 1H, 2H, 2H-perfluorooctyl) silane self-assembles and reacts with the hydroxyl groups on the surface of the super-hydrophilic film of silicon dioxide nanoparticles to form a super-hydrophobic and oleophobic double-repellent coating.

[0018] Figure 2A Depicted is the surface morphology observed under a scanning electron microscope (SEM) at a deposition time of 10 minutes. The scale bar represents 100 nm.

[0019] Figure 2B Depicted are the surface morphologies observed under atomic force microscopy (AFM) at a deposition time of 10 min.

[0020] Figure 2CDepicted are the surface morphologies observed under atomic force microscopy (AFM) at a deposition time of 10 min.

[0021] Figure 2D Depicted is the surface morphology observed under a scanning electron microscope (SEM) at a deposition time of 30 minutes. The scale bar represents 100 nm.

[0022] Figure 2E The surface morphology observed under atomic force microscopy (AFM) at a deposition time of 30 minutes is depicted.

[0023] Figure 2F The surface morphology observed under atomic force microscopy (AFM) at a deposition time of 30 minutes is depicted.

[0024] Figure 2G Depicted is the surface morphology observed under a scanning electron microscope (SEM) at a deposition time of 60 minutes. The scale bar represents 100 nm.

[0025] Figure 2H The surface morphology observed under atomic force microscopy (AFM) at 60 min deposition time is depicted.

[0026] Fig.2I The surface morphology observed under atomic force microscopy (AFM) at 60 min deposition time is depicted.

[0027] Figure 2J Depicted is the surface morphology observed under a scanning electron microscope (SEM) at a deposition time of 90 minutes. The scale bar represents 100 nm.

[0028] Figure 2K Depicted are the surface morphologies observed under atomic force microscopy (AFM) at 90 min deposition time.

[0029] Figure 2L Depicted are the surface morphologies observed under atomic force microscopy (AFM) at 90 min deposition time.

[0030] Figure 3A Comparison of water contact angles at different deposition times before and after wear testing is shown.

[0031] Figure 3B A comparison of the oil contact angles at different deposition times before and after the wear test is shown.

[0032] Figure 4An overview of the water contact angle (WCA) of the silica nanoparticle film (401), the water contact angle (WCA) of the silica nanoparticle film after PFTS coating (403), the oil contact angle (OCA) of the silica nanoparticle film (405), and the oil contact angle (OCA) of the silica nanoparticle film after PFTS coating (407) is shown.

[0033] Figure 5A Field emission SEM and AFM images of the surface morphology of the prepared silica nanoparticle films with PFTS coating are shown.

[0034] Figure 5B Field emission SEM and AFM images of the surface morphology of the prepared silica nanoparticle film without PFTS coating are shown.

[0035] Fig. 6A AFM topography images and roughness measurements of the pristine PC surface are shown.

[0036] Figure 6B AFM topography images and roughness measurements of the oxygen plasma treated PC surface are shown.

[0037] Figure 6C Shown (from top to bottom) are X-ray photoelectron spectroscopy (XPS) survey spectra of oxygen plasma treated PC and pristine PC.

[0038] Fig. 7A Shown (from top to bottom) is a comparison of XPS spectra between pristine PC, silica film, and PFTS-coated silica nanoparticle film on a polycarbonate substrate.

[0039] Figure 7B High-resolution fitted XPS spectra of C1s of PFTS-coated silica films are shown.

[0040] Figure 7C High-resolution fitted XPS spectra of O1s of PFTS-coated silica films are shown.

[0041] Fig.7D High-resolution fitted XPS spectra of Si 2p of PFTS-coated silica films are shown.

[0042] Fig. 7E High-resolution fitted XPS spectra of F1s of PFTS-coated silica films are shown.

[0043] Fig. 8A The prepared PFTS-coated silica nanoparticle film is shown, which exhibits transparency and has water- and oil-repellent properties.

[0044] Figure 8BShown are the light transmittances of pristine PC and PFTS-coated silica films measured using a UV-visible spectrometer.

[0045] Figure 8C A digital image showing transparent anti-fingerprint properties is shown, showing the original PC with fingerprints.

[0046] Fig.8D A digital image showing transparent anti-fingerprint properties is shown, showing a PFTS-coated silica nanoparticle film without fingerprints.

[0047] Fig. 8E The self-cleaning process of pristine PC and silica nanoparticle film / PFTS-coated PC is shown.

[0048] Fig. 9 The transmittance in the visible light range at different film deposition times (10 minutes, 30 minutes, 60 minutes and 90 minutes) and the transmittance of the original polycarbonate are shown. According to the results obtained, the transmittance of the coated sample in the visible light range (T% ave ) is even higher than that of original polycarbonate without coating.

[0049] Fig. 10A Field emission SEM image of the prepared coated PC surface showing a crosshatch.

[0050] Fig. 10B The field emission SEM image of the PC surface after wear testing is shown. The inset is a field emission SEM image of the prepared coating for comparison.

[0051] Fig. 10C Shown are AFM topographic images and surface roughness measurements of the coated PC surface after wear testing.

[0052] Fig. 10D The water contact angle (WCA) and oil contact angle (OCA) after wear testing are shown. The oil contact angle was measured using diiodomethane as the oil sample.

[0053] Fig.10E A comparison of transmittance measurements of pristine PC, prepared coated PC, and after abrasion testing is shown.

[0054] Fig.10F The fingerprint micrograph of the PC surface after the wear test is shown. The inset is the fingerprint micrograph of the uncoated surface. DETAILED DESCRIPTION

[0055] The following detailed description refers to the accompanying drawings, which show by way of illustration specific details and embodiments in which the present invention may be practiced. These embodiments are described in sufficient detail to enable those skilled in the art to practice the present invention. Other embodiments may be utilized and structural, logical, and electrical changes may be made without departing from the scope of the present invention. The various embodiments are not necessarily mutually exclusive, as some embodiments may be combined with one or more other embodiments to form new embodiments.

[0056] In the first aspect, each embodiment relates to a kind of amphiphilic coating.The term "amphiphobic" used in this article refers to a compound or coating that repels both water-based substances and oil-based substances.The term "water-based substance" can refer to a liquid with water as the main phase.For example, the water content in the water-based substance can be at least 50wt% of the substance, such as at least 60wt%, at least 65wt%, at least 70wt%, at least 75wt%, at least 80wt%, at least 85wt%, at least 90wt%, or at least 95wt%.Similarly, the term "oil-based" can refer to a liquid with oil as the main phase.For example, the oil content in the oil-based substance can be at least 50wt% of the substance, such as at least 60wt%, at least 65wt%, at least 70wt%, at least 75wt%, at least 80wt%, at least 85wt%, at least 90wt%, or at least 95wt%.Oil can be in the form of an optionally substituted hydrocarbon, and examples of oil-based substances can include sebum and oil from the skin.

[0057] Therefore, the amphiphobic coating disclosed herein can be hydrophobic and oleophobic, because the water contact angle and oil contact angle of the amphiphobic coating can be equal to or greater than 90°, respectively. In various embodiments, the amphiphobic coating disclosed herein is superhydrophobic, which means that the contact angle between a water droplet and the surface formed by the amphiphobic coating is greater than 150°. In various embodiments, the amphiphobic coating disclosed herein has high oleophobicity, which means that the contact angle between an oil droplet (for example, diiodomethane) and the surface formed by the amphiphobic coating is greater than 130°.

[0058] Advantageously, the coatings according to the embodiments disclosed herein can exhibit self-cleaning properties, which refers to the inherent ability of a surface to remain clean over time without or with reduced need to apply mechanical forces or chemicals (e.g., detergents) to the surface to remove foreign matter (e.g., dirt). Since the coatings have amphiphilicity, they are able to repel both water-based and oil-based substances. Therefore, the coatings disclosed herein can keep the surface cleaner for a longer period of time. In addition, contaminants such as fingerprints, skin oil residues, and dust particles may not adhere to the surface of the coating. Therefore, the coating can be anti-fingerprint.

[0059] In addition to self-cleaning and anti-fingerprint properties, the coating disclosed herein can also provide good light transmittance and anti-reflection properties. As demonstrated by the experiments conducted, the amphiphobic coating disclosed herein can exhibit a transmittance of at least 84% in the wavelength range of 400nm to 700nm. The coating disclosed herein can also adhere well to the polymer substrate, thereby providing mechanical strength and durability for long-term use. The method for preparing the amphiphobic coating can be carried out under ambient conditions or at room temperature, which makes the method particularly suitable for preparing amphiphobic coatings on heat-sensitive or low-melting polymer substrates to achieve a wider range of functional surface applications.

[0060] In view of the above, an amphiphobic coating according to various embodiments includes: a polymer substrate having a surface treated with oxygen plasma; a silicon dioxide layer containing silicon dioxide nanoparticles directly disposed on the surface treated with oxygen plasma; and a fluoroalkylsilane layer directly disposed on the silicon dioxide layer.

[0061] The polymer substrate can be any suitable polymer material. For example, the material of the polymer substrate can be selected from polycarbonate, poly(methyl methacrylate), polyester, polyethylene terephthalate, polyimide, polytetrafluoroethylene, polypropylene, polyolefin, nylon, silicone, polyvinyl chloride, polystyrene and polyphenylene sulfide. Composite materials of these materials can also be used as substrates.

[0062] In a specific embodiment, the material of the polymer substrate is polycarbonate.

[0063] The shape and structure of the polymer substrate can be selected arbitrarily and is not limited to a plane. For example, the polymer substrate can have a non-planar shape or other complex shape, or be in the form of a product or article having a surface to which a coating is applied.

[0064] In various embodiments, the polymer substrate has a surface treated with oxygen plasma. Advantageously, the effect of oxygen plasma on the polymer substrate may result in an increase in surface roughness. A surface structure with a concave morphology may be formed. The term "concave" is used to describe the morphology of a structure formed below the substrate surface and having an opening on the substrate surface, wherein the width of the cross section of the structure increases as the distance from the opening increases. The formation of a surface structure with a concave morphology may advantageously result in an increase in the contact angle with water-based and oil-based substances. In addition, the surface chemistry may change, resulting in more oxygen bonding on the surface. This increases the surface energy of the polymer substrate and can be used to enhance the stability and adhesion of a coating subsequently deposited.

[0065] In various embodiments, the silicon dioxide layer containing silicon dioxide nanoparticles is directly disposed on the surface of the polymer substrate treated with oxygen plasma. The term "directly" refers to the silicon dioxide layer in contact with the surface of the polymer substrate treated with oxygen plasma. In other words, there may be no intermediate layer between the silicon dioxide layer and the surface of the polymer substrate treated with oxygen plasma.

[0066] In various embodiments, silicon dioxide is directly disposed on the surface of the polymer substrate through oxygen plasma treatment in the form of nanoparticles. The silicon dioxide layer may comprise silicon dioxide nanoparticles or be composed of silicon dioxide nanoparticles. The average size of the silicon dioxide nanoparticles may be in the range of 25nm to 50nm, for example, in the range of 30nm to 50nm, 40nm to 50nm, 25nm to 40nm, 25nm to 30nm or 30nm to 40nm.

[0067] The silica nanoparticles can be evenly distributed or dispersed on the surface of the polymer substrate treated with oxygen plasma. In various embodiments, the silica nanoparticles form clusters having a size range of 150nm to 250nm, such as 160nm to 250nm, 170nm to 250nm, 180nm to 250nm, 190nm to 250nm, 200nm to 250nm, 150nm to 240nm, 150nm to 230nm, 150nm to 220nm, 150nm to 200nm, or 180nm to 200nm.

[0068] Silica nanoparticles can coalesce to form a porous layer. In various embodiments, the silica layer is nanoporous. The porosity of the silica layer can result in an amphiphobic coating having a certain surface roughness factor.

[0069] Roughness factor R of amphiphobic coating f In various embodiments, the roughness factor R of the amphiphobic coating may be in the range of 0.1 to 0.5, for example, 0.15 to 0.5, 0.2 to 0.5, 0.25 to 0.5, 0.3 to 0.5, 0.1 to 0.45, 0.1 to 0.4, 0.1 to 0.35, 0.1 to 0.3, 0.15 to 0.45, 0.15 to 0.4, 0.2 to 0.3, 0.22 to 0.26, or 0.24 to 0.25. f 0.2451 or less, for example 0.24 or less, 0.23 or less, 0.22 or less, 0.21 or less, or 0.2 or less. Advantageously, this can impart amphiphobicity to the amphiphobic coating or result in the amphiphobic coating having good amphiphobicity.

[0070] The thickness of the silicon dioxide layer can be 10nm to 500nm, for example, 20nm to 500nm, 30nm to 500nm, 50nm to 500nm, 75nm to 500nm, 100nm to 500nm, 200nm to 500nm, 300nm to 500nm, 400nm to 500nm, 10nm to 400nm, 10nm to 300nm, 10nm to 200nm, 10nm to 100nm, 20nm to 400nm, 30nm to 300nm, 10nm to 150nm or 50nm to 100nm.

[0071] The silicon dioxide layer may be crystalline, amorphous, or a mixed phase of crystalline and amorphous. In various embodiments, the silicon dioxide layer is amorphous.

[0072] In various embodiments, the fluoroalkylsilane layer is directly disposed on the silicon dioxide layer. The term "directly" means that the silicon dioxide layer is in contact with the fluoroalkylsilane layer. In other words, there may be no intermediate layer between the silicon dioxide layer and the fluoroalkylsilane layer. In general, fluoroalkylsilanes that can provide fluorocarbon molecules on the surface, thereby reducing the surface energy to produce amphiphobicity, can be used. In this way, an amphiphobic coating with excellent anti-reflection, anti-fingerprint and self-cleaning properties can be obtained.

[0073] For example, the fluoroalkylsilane layer can be formed from a fluoroalkylsilane selected from trichloro(1H,1H,2H,2H-perfluorooctyl)silane, 1H,1H,2H,2H-perfluorodecyltriethoxysilane, and combinations thereof. In some embodiments, the fluoroalkylsilane layer is formed from trichloro(1H,1H,2H,2H-perfluorooctyl)silane.

[0074] In various embodiments, the surface of the silicon dioxide layer comprises hydroxyl groups. The hydroxyl groups on the silicon dioxide layer can be obtained by the method used to deposit the silicon dioxide layer. For example, the silicon dioxide layer can be deposited using pulsed laser deposition, which produces hydroxyl groups on the surface. The fluoroalkylsilane layer disposed directly on the silicon dioxide layer can be covalently bonded to the silicon dioxide layer via the hydroxyl groups.

[0075] In various embodiments, the fluoroalkylsilane layer is a self-assembled layer. As used herein, the term "self-assembled" or "self-assembly" refers to the spontaneous organization or arrangement of compounds on a surface, which may be affected by the affinity between the compound and moieties that may be present on the underlying surface. In embodiments where the surface of the silica layer comprises hydroxyl groups, for example, the fluoroalkylsilane molecules may self-assemble on the silica layer and covalently bond to the hydroxyl groups present on the silica layer.

[0076] The coating disclosed herein can be formed by a monolayer silica layer containing silica nanoparticles and a monolayer fluoroalkyl silane layer. The monolayer silica layer can be formed by a monolayer silica nanoparticle. Therefore, in some embodiments, the coating disclosed herein consists of only two layers on a polymer substrate. It may be advantageous to use only two layers to improve processing efficiency and reduce costs in forming a double-phobic coating. In some embodiments, the silica layer containing silica nanoparticles can have a multilayer structure containing multilayer silica nanoparticles or consisting of multilayer silica nanoparticles. Multilayer silica nanoparticles can be used, such as two layers, three layers, four layers, five layers, six layers, seven layers or more layers. For example, the coating disclosed herein can include a monolayer fluoroalkyl silane layer and a silica layer containing two or more layers of silica nanoparticles. In embodiments using multiple layers of silica nanoparticles, the uppermost surface of the silica layer may have a surface roughness and surface features as disclosed herein, and / or it may be the same or similar to the surface roughness and surface features formed by a silica layer comprising a single layer of silica nanoparticles, such that when the fluoroalkylsilane layer is disposed directly thereon, an amphiphobic coating as disclosed herein may be obtained.

[0077] The amphiphobic coating disclosed herein may exhibit a transmittance of at least 84% in the wavelength range of 400nm to 700nm. For example, the transmittance of the amphiphobic coating in the wavelength range of 400nm to 700nm may be at least 85%, at least 86%, at least 87%, at least 88%, at least 89%, or at least 90%. In some embodiments, the transmittance of the amphiphobic coating may be as high as 92%. Therefore, the transmittance of the amphiphobic coating may be in the range of 85% to 92%, 87% to 92%, 89% to 92%, 85% to 90%, 85% to 88%, or 86% to 90%.

[0078] As described above, the amphiphobic coating disclosed herein can be super hydrophobic and highly oleophobic. The contact angle of water on the amphiphobic coating can be greater than 150°, such as greater than 151°, greater than 152°, greater than 153°, greater than 154°, or greater than 155°. In various embodiments, the contact angle of diiodomethane on the amphiphobic coating is greater than 130°, such as greater than 131°, greater than 132°, greater than 133°, greater than 134°, or greater than 135°. It will be appreciated by those skilled in the art that if another oil or oil-based fluid is used for contact angle measurement, the amphiphobic coating may establish a different contact angle range.

[0079] In a second aspect, various embodiments are directed to a method of preparing an amphiphobic coating.

[0080] The method may include providing a polymer substrate having a surface treated with oxygen plasma. As described above, the action of the oxygen plasma on the polymer substrate may result in increased surface roughness and oxygen bonding of the surface. This increases the surface energy of the polymer substrate and can be used to enhance adhesion to a subsequently deposited coating.

[0081] In various embodiments, providing a polymer substrate having an oxygen plasma treated surface includes treating the surface of the polymer substrate with an oxygen containing plasma.

[0082] The surface of the polymer substrate is treated with oxygen-containing plasma for any suitable time, depending on, for example, the flow rate and / or type of oxygen-containing plasma used, and the area to be treated. In various embodiments, the surface of the polymer substrate is treated with oxygen-containing plasma for a time period in the range of 10 minutes to 20 minutes, such as 12 minutes to 20 minutes, 14 minutes to 20 minutes, 15 minutes to 20 minutes, 10 minutes to 18 minutes, 10 minutes to 15 minutes, 12 minutes to 18 minutes, or 14 minutes to 16 minutes.

[0083] The surface of the polymer substrate can be treated with oxygen-containing plasma in 10 -3 mbar to 10 -1 mbar pressure range, for example 10 -3 mbar to 10 -2 mbar or 10 -2 mbar to 10 -1 In some embodiments, the surface of the polymer substrate is treated with oxygen-containing plasma at a pressure of 10 -3 mbar to 10 -2 The pressure is carried out in the mbar range.

[0084] In various embodiments, treating the surface of the polymer substrate with an oxygen-containing plasma further comprises cleaning the surface of the polymer substrate with alcohol and deionized water prior to treating the surface with the oxygen-containing plasma. Advantageously, this helps ensure that contaminants that may be present on the surface of the polymer substrate are removed prior to the oxygen plasma treatment, thereby enhancing the adhesion of the coating on the polymer substrate.

[0085] The method disclosed herein may include: directly depositing silicon dioxide on the surface of the polymer substrate treated with oxygen plasma by pulsed laser deposition to form a silicon dioxide layer containing silicon dioxide nanoparticles; and directly depositing a fluoroalkyl silane on the silicon dioxide layer to form a fluoroalkyl silane layer on the silicon dioxide layer. The term "directly" means that the silicon dioxide layer is in contact with the surface of the polymer substrate treated with oxygen plasma, and the fluoroalkyl silane layer is in contact with the silicon dioxide layer.

[0086] To deposit silicon dioxide directly on the oxygen plasma treated surface of a polymer substrate, a target containing silicon or silicon dioxide may be used.

[0087] In some embodiments, a silicon target is used. Thus, directly depositing silicon dioxide on the oxygen plasma treated surface of a polymer substrate may include providing a silicon target, and directing a pulsed laser beam at the silicon target in the presence of oxygen to generate a silicon plasma that interacts with a background oxygen plasma to form a silicon dioxide layer on the oxygen plasma treated surface of the polymer substrate. The background oxygen plasma may be an oxygen plasma generated due to the action of the pulsed laser beam on the oxygen present, and / or an oxygen plasma generated due to the interaction of the ablated silicon plasma with the oxygen present. With respect to the interaction of the ablated silicon plasma with the oxygen present, collisions and charge exchange between the ablated high energy silicon plasma species and the background oxygen may generate oxygen plasma and reactive oxygen species that interact with the silicon plasma to form oxides of silicon.

[0088] In some embodiments, a silicon dioxide target is used. Thus, directly depositing silicon dioxide on the oxygen plasma treated surface of the polymer substrate may include providing a silicon dioxide target, and directing a pulsed laser beam toward the silicon dioxide target to form a silicon dioxide layer on the oxygen plasma treated surface of the polymer substrate.

[0089] Oxygen may not be required when using a silicon dioxide target, since pulsed laser deposition can reproduce the stoichiometry of the target on the polymer substrate. However, the corresponding process can still be carried out in the presence of oxygen to prevent or avoid oxygen defects in the silicon dioxide layer being formed. Therefore, in various embodiments, whether silicon or silicon dioxide is used as a target to form the silicon dioxide layer, silicon dioxide can be directly deposited on the oxygen plasma treated surface of the polymer substrate in the presence of oxygen.

[0090] In some embodiments, the deposition of silicon dioxide can be performed in the presence of oxygen in the chamber, and the oxygen can be introduced into the chamber at a flow rate in the range of 100 sccm to 300 sccm, 120 sccm to 300 sccm, 150 sccm to 300 sccm, 200 sccm to 300 sccm, 250 sccm to 300 sccm, 100 sccm to 250 sccm, 100 sccm to 200 sccm, 150 sccm to 250 sccm, or 180 sccm to 220 sccm.

[0091] The respective targets of silicon and silicon dioxide can be independently spaced apart from the polymer substrate at a distance ranging from 3 cm to 8 cm, such as 5 cm to 8 cm, 6 cm to 8 cm, 3 cm to 7 cm, 3 cm to 5 cm, 4 cm to 7 cm, or 4 cm to 6 cm. The term "independently spaced apart" means that each target can be spaced apart from the polymer substrate at the same or different distances.

[0092] In some embodiments, a silicon target is used to form the silicon dioxide layer. The silicon target may be spaced apart from the polymer substrate by a distance of 4 cm to 6 cm, such as about 5 cm.

[0093] When pulsed laser is applied to silicon or silicon dioxide target to deposit silicon dioxide layer, high energy hydroxyl group can be imparted to the formed layer. Silicon dioxide can be deposited in the form of nanoparticles. A single layer or multiple layers of silicon dioxide nanoparticles can be formed. In some embodiments, the nanoparticles can be agglomerated when pulsed laser is further applied to form a porous layer.

[0094] The pulsed laser beam can form 3×10 -4 cm 2 Up to 7×10 -4 cm 2 In various embodiments, the pulsed laser beam can form a spot size of 4×10 -4 cm 2 Up to 7×10 -4 cm 2 , 5×10 - 4 cm 2 Up to 7×10 -4 cm 2 , 6×10 -4 cm 2 Up to 7×10 -4 cm 2 , 4×10 -4 cm 2 Up to 6×10 -4 cm 2 , or 5×10 -4 cm 2 Up to 6×10 - 4 cm 2 In a specific embodiment, the pulsed laser beam can form a spot size of 4×10 -4 cm 2 Up to 6×10 -4 cm 2 spot size.

[0095] In various embodiments, the pulsed laser beam has a wavelength of about 532 nm.

[0096] In various embodiments, the frequency of the pulsed laser beam is in the range of 8 Hz to 12 Hz, such as 9 Hz to 12 Hz, 10 Hz to 12 Hz, 8 Hz to 11 Hz, 8 Hz to 10 Hz, or 9 Hz to 11 Hz. In some embodiments, the frequency of the pulsed laser beam is in the range of 9 Hz to 11 Hz.

[0097] The pulsed laser beam can have a flux of 1 Jcm -2 Up to 10Jcm -2 For example, the flux of a pulsed laser beam can be within the range of 2 J cm -2 Up to 10Jcm -2 、3Jcm -2 Up to 10Jcm -2 、4Jcm -2 Up to 10Jcm -2 ,2Jcm -2 Up to 8Jcm -2 ,2Jcm -2 Up to 6Jcm -2 ,2Jcm -2 Up to 5Jcm -2 、3Jcm -2 Up to 8Jcm -2 , or 4Jcm -2 Up to 5Jcm -2 In some embodiments, the flux of the pulsed laser beam is within the range of 4 Jcm -2 Up to 5Jcm -2 within the range.

[0098] The time period for depositing silicon dioxide can depend on the thickness of the silicon dioxide layer to be formed. In various embodiments, the time period for depositing silicon dioxide is in the range of 30 minutes to 90 minutes, such as 40 minutes to 90 minutes, 50 minutes to 90 minutes, 60 minutes to 90 minutes, 70 minutes to 90 minutes, 30 minutes to 80 minutes, 30 minutes to 70 minutes, 30 minutes to 60 minutes, 30 minutes to 50 minutes, 40 minutes to 80 minutes, 50 minutes to 70 minutes, or 60 minutes.

[0099] As mentioned above, the polymer substrate can be any suitable polymer material. For example, the material of the polymer substrate can be selected from polycarbonate, poly(methyl methacrylate), polyester, polyethylene terephthalate, polyimide, polytetrafluoroethylene, polypropylene, polyolefin, nylon, silicone, polyvinyl chloride, polystyrene and polyphenylene sulfide. The composite material of these materials can also be used as substrate.

[0100] In various embodiments, the polymer substrate is polycarbonate.

[0101] The shape and structure of the polymer substrate can be arbitrarily selected and is not limited to a plane. For example, the polymer substrate can have a non-planar shape or any complex shape, or be in the form of a product or article having a surface to which a coating is to be applied.

[0102] As described above, any fluoroalkylsilane that can provide fluorocarbon molecules on the surface, thereby reducing the surface energy to produce amphiphobicity, can be used. In various embodiments, the fluoroalkylsilane layer is formed by a fluoroalkylsilane selected from trichloro(1H,1H,2H,2H-perfluorooctyl)silane, 1H,1H,2H,2H-perfluorodecyltriethoxysilane, and combinations thereof.

[0103] In various embodiments, depositing the fluoroalkylsilane directly on the silicon dioxide layer comprises contacting the silicon dioxide layer with a solution comprising the fluoroalkylsilane and a liquid reagent. The liquid reagent may serve as a solvent and may be selected from hexane and methanol.

[0104] The concentration of the fluoroalkylsilane in the solution can be in the range of 0.05 vol% to 0.15 vol%, for example, 0.06 vol% to 0.15 vol%, 0.07 vol% to 0.15 vol%, 0.08 vol% to 0.15 vol%, 0.09 vol% to 0.15 vol%, 0.1 vol% to 0.15 vol%, 0.05 vol% to 0.14 vol%, 0.05 vol% to 0.13 vol%, 0.05 vol% to 0.12 vol%, 0.05 vol% to 0.11 vol%, 0.05 vol% to 0.1 vol%, or 0.08 vol% to 0.12 vol%.

[0105] Contacting the silica layer with the solution can be for any suitable period of time, for example, a period of time in the range of 5 minutes to 20 minutes, 8 minutes to 20 minutes, 10 minutes to 20 minutes, 12 minutes to 20 minutes, 5 minutes to 18 minutes, 5 minutes to 15 minutes, or 8 minutes to 15 minutes.

[0106] In various embodiments, the methods disclosed herein can be performed without heating. For example, the deposition of the silicon dioxide layer and the fluoroalkylsilane can be performed without heating. In some embodiments, the method is performed at ambient conditions or room temperature, such as a temperature in the range of about 20°C to 45°C or about 25°C to 35°C.

[0107] In various embodiments, depositing the fluoroalkylsilane directly on the silicon dioxide layer further comprises drying the silicon dioxide layer after contacting the silicon dioxide layer with the solution.

[0108] Although the silicon dioxide layer can be dried without heating, heating can be applied to accelerate drying. In various embodiments, drying is performed at a temperature in the range of 70°C to 90°C, such as 75°C to 90°C, 80°C to 90°C, 85°C to 90°C, 70°C to 85°C, 70°C to 80°C, 70°C to 75°C, or 75°C to 85°C.

[0109] Drying can be performed for any suitable period of time. When heat is applied, drying can be performed for a period of time in the following ranges: 1 hour to 3 hours, 1.5 hours to 3 hours, 2 hours to 3 hours, 1 hour to 2.5 hours, 1 hour to 2 hours, or 1.5 hours to 2.5 hours.

[0110] In a third aspect, various embodiments relate to an amphiphobic coating prepared by the method of the second aspect.

[0111] As described above, the method disclosed herein can be advantageously used to prepare a double-repellent coating that can be self-cleaned and has anti-fingerprint and anti-reflection properties. By applying oxygen plasma on the surface of a polymer substrate, the surface roughness can be increased and a structure with a concave morphology can be formed. As a result, the contact angle with water-based substances and oil-based substances can be increased. In addition, the surface energy of the polymer substrate can be increased to enhance the adhesion of the silicon dioxide layer deposited thereon. By depositing the silicon dioxide layer using pulsed laser deposition, hydroxyl groups can be generated on the silicon dioxide layer. Treating the silicon dioxide layer with a fluoroalkyl silane can result in the fluoroalkyl silane being covalently bonded to the silicon dioxide layer. Fluoroalkyl silane can form a fluoroalkyl silane layer on the silicon dioxide layer. This may mean that the resulting coating has a lower surface energy, thereby having double repellency. A double-repellent coating with excellent anti-reflection, anti-fingerprint and self-cleaning properties can be obtained.

[0112] In a fourth aspect, various embodiments relate to the use of the amphiphobic coating according to the first aspect or the amphiphobic coating prepared by the method according to the second aspect in an anti-reflective coating, an anti-fingerprint coating, an anti-fouling coating, a self-cleaning surface, a surface primer layer, an optical element, a sensor, a lens, a goggles, a mirror, a windshield, a mask, a display, a window or a cooker cover.

[0113] As described above, the amphiphobic coatings disclosed herein can be hydrophobic and oleophobic. Coatings according to embodiments disclosed herein can exhibit self-cleaning, anti-fingerprint and / or anti-reflective properties. Since the methods for preparing the coatings can be performed under ambient conditions, they are particularly suitable for preparing amphiphobic coatings on heat-sensitive or low-melting polymer substrates.

[0114] In a fifth aspect, various embodiments relate to an article comprising an amphiphobic coating according to the first aspect or an amphiphobic coating prepared by the method according to the second aspect, wherein the article is an optical element, a sensor, a lens, a goggles, a mirror, a windshield, a mask, a display, a window or a cooker cover.

[0115] In order that the present invention can be readily understood and put into practice, specific embodiments will now be described by way of the following non-limiting examples.

[0116] Example

[0117] According to the embodiments disclosed herein, a simple and effective manufacturing method is provided for preparing a highly transparent amphiphobic coating having super hydrophobicity and high oleophobicity on polycarbonate (PC).

[0118] In the experiments conducted, nanoporous films containing silica (SiO2) nanoparticles were deposited on polycarbonate (PC) pretreated with oxygen plasma by pulsed laser deposition. The deposition can be performed at ambient temperature and pressure. After film deposition, trichloro(1H,1H,2H,2H-perfluorooctyl)silane (PFTS) was assembled on the silica surface. The prepared PFTS-treated silica coating exhibited amphiphobicity, i.e., it was superhydrophobic, with a contact angle of 155.2±1.8° with water, and highly oleophobic, with a contact angle of 133.6±3.3° with diiodomethane. The coating also exhibited excellent adhesion to the PC substrate. The developed room temperature deposition process makes it possible to apply it to the modification of temperature-sensitive and other low-melting-point polymer substrates for a wider range of functional surface applications. The surface of the prepared coating, after modification with fluorocarbon compounds, exhibited excellent anti-reflective, anti-fingerprint and self-cleaning properties. From a mechanical point of view, the coating exhibited good stability and strong adhesion to the polymer substrate due to the pre-deposition plasma treatment.

[0119] Example 1: Sample preparation

[0120] Example 1.1: Coating of Silica Nanoparticle Film

[0121] The coating of silica nanoparticle film was performed in a two-step process. Prior to coating, polycarbonate (PC) substrates (1.5 cm × 1.5 cm in size) were cleaned with several rounds of ethanol and deionized water. Surface oxygen plasma treatment was performed before deposition of silica nanoparticle film. The solution-cleaned PC substrate was placed in a radio frequency (RF) plasma tube chamber that was capacitively coupled to two annular electrodes mounted outside the tube. The chamber was evacuated to a base pressure of 10 by a vacuum pump. -3 mbar, and then oxygen was introduced into the chamber at a flow rate of 2 sccm to stabilize the pressure at 10 -2mbar. The oxygen plasma was activated by a 13.56 MHz caeser136 RF generator with an automatic impedance matching device providing 250 W RF power. The oxygen plasma surface treatment was carried out for 15 minutes.

[0122] In the second step, a silicon dioxide nanoparticle film was deposited by a pulsed laser deposition (PLD) system. A silicon target (purchased from S1-Lab Pte Ltd, 99.99%) and a plasma-treated PC substrate were placed in the deposition chamber, 5 cm apart and facing each other. The system was evacuated to 10 -5 mbar, and then oxygen was introduced into the chamber at a flow rate of 200 sccm to stabilize the chamber pressure at 10 -2 mbar. The Nd:YAG 532nm laser was operated at a frequency of 10Hz and the laser pulse flux was F = 4.74Jcm -2 , focused on the silicon target, with a spot size of about 5.0×10 -4 cm 2 The deposition process was performed for 4 different deposition times: 10 min, 30 min, 60 min, and 90 min.

[0123] Example 1.2: Modification of trichloro(1H,1H,2H,2H-perfluorooctyl)silane

[0124] Trichloro(1H,1H,2H,2H-perfluorooctyl)silane (PFTS) (CF3(CF2)5CH2CH2SiCl3) was purchased from SigmaAldrich. The prepared silica nanoparticle film was immersed in a 0.1 vol% hexane solution of PFTS for 10 minutes. The sample was then placed in a drying oven at 80°C for 2 hours.

[0125] Example 2: Material Characterization

[0126] The surface morphology was observed using a JEOL 7600 field emission scanning electron microscope (SEM) operated at 2.0 kV. The surface topology was examined and the surface roughness parameters were measured using an NX10 Park system atomic force microscope (AFM). The surface chemical composition analysis was performed using a Kratos AXIS Supra X-ray photoelectron spectrometer (XPS). As a reference, the binding energy of the C1s peak of sp2-bonded carbon, 284.8 eV, was used. Additional surface chemical molecular bonding analysis was performed using a Fourier transform infrared (FTIR) spectrometer (Perkin Elmer Frontier). The static water contact angle (WCA) and oil (using diiodomethane as an example) contact angle (OCA) of a 5 μL DI water droplet and a 3 μL oil droplet were recorded using a contact angle goniometer (OCA 20 Dataphysic), respectively. The transmittance in the visible wavelength range was measured using a Perkin Elmer Lambda 950 UV-VIS-NIR spectrometer.

[0127] Example 3: Mechanical durability

[0128] Example 3.1: Wear test (MIL-C-48497 standard)

[0129] The surface was rubbed with a cheesecloth pad at a constant force (400 grams of weight evenly distributed on a 1.5 cm x 1.5 cm substrate, equivalent to 26.7 kPa pressure). Twenty rubbing actions were performed for each test. The surface condition was monitored by SEM and visual observation after the test.

[0130] Example 3.2: Adhesion Test (MIL-C-48497 Standard)

[0131] First, the transparent tape was pressed on the coating surface and then torn off very slowly at an angle of 45°. After the test, SEM and visual observation were performed.

[0132] Example 3.3: Adhesion test (ASTM-3359 standard)

[0133] Use a sharp steel knife to crosscut the coating surface. Press the transparent tape onto the surface and then slowly peel it off the surface. After testing, evaluate the coating performance by SEM and visual observation.

[0134] Example 4: Results and Discussion

[0135] Figure 1 The schematic diagram shows the process of preparing a silica nanoparticle film with a PFTS coating on a PC surface according to one embodiment. The whole process is relatively fast and does not require substrate heating.

[0136] Example 4.1: Effect of surface morphology and thickness on wetting behavior and mechanical durability

[0137] Pulsed laser deposition of SiO2 films was performed with four different deposition times of 10 min, 30 min, 60 min, and 90 min to investigate the effects of surface morphology and thickness on the wetting behavior and mechanical durability.

[0138] The surface morphology of PFTS-coated silica nanoparticle films deposited at different times was investigated by SEM and AFM. Figures 2A to 2L As shown in the SEM images in , similar morphologies were observed for the four coating times, except that the cluster size became larger at longer coating times. As shown in Table 1, the film thickness increased with increasing deposition time.

[0139] Table 1: Surface roughness parameter measurements and film thickness measurements at different silica nanoparticle film deposition times

[0140] Deposition time <![CDATA[R q (nm)]]> <![CDATA[R v (nm)]]> <![CDATA[R a (nm)]]> <![CDATA[R f (R a / R v )]]> Thickness(nm) 10 minutes 50.9 144.5 42.9 0.296 17.9±4.4 30 minutes 48.9 169 38.4 0.227 42.3±5.9 60 minutes 55 165.1 40 0.242 97.1±4.5 90 minutes 48.6 130.9 39 0.297 142.3±3.7

[0141] Surface roughness may play an important role in surface wetting behavior. AFM is used to study and measure surface morphology and roughness parameters such as Figure 2C , Figure 2F , Fig.2I and Figure 2L As shown in Table 1, similar arithmetic mean roughness R a and root mean square roughness R q However, higher R was observed at deposition times of 30 and 60 min. v , which is associated with the higher water and oil contact angles listed in Table 2.

[0142] Table 2: Water contact angle and oil (diiodomethane) contact angle measurements before and after wear testing at different deposition times.

[0143] Deposition time Water contact angle (°) Water contact angle after wear (°) Oil contact angle (°) Oil contact angle after wear (°) 10 minutes 150.2±4.1 94.5±3.8 133±1 71.6±4.1 30 minutes 158.2±2.3 106.5±7.5 128.2±3.7 79±3.6 60 minutes 155.2±1.8 129.2±4.4 133.6±3.3 98±2.6 90 minutes 150.4±4.0 137.2±4.2 118.7±8.4 82±7.0

[0144] As described in this article, a larger R v It is beneficial for anti-fingerprint amphiphobicity. Therefore, relatively good performance is expected in terms of water contact angle and oil contact angle. A decrease in water contact angle and oil contact angle was observed at a longer deposition time (90 min), which is due to the decrease in peaks and valleys caused by larger cluster growth.

[0145] The inventors have found that the thickness of the silica nanoparticle film has a great influence on the wear resistance. Figure 3A and Figure 3BAs shown, at longer deposition times, a less pronounced decrease in the water or oil contact angle can be observed. For the deposition completed at 60 minutes, the water contact angle after wear remains around 130°, while the oil contact angle is still above 90°. Therefore, this film has a higher mechanical wear resistance and was chosen as the condition to be studied in detail in this study.

[0146] In conclusion, combined with the obtained results, the silica nanoparticle film deposited for 60 min before PFTS coating showed the best performance in terms of transparency, surface wetting behavior, and mechanical wear resistance.

[0147] The silica nanoparticle film deposited for 60 minutes followed by PFTS coating showed the best results in terms of surface wetting behavior, transparency and mechanical wear resistance. Therefore, unless otherwise stated, the results disclosed herein are based on the silica nanoparticle film deposited for 60 minutes with PFTS coating.

[0148] Example 4.2: Surface wettability

[0149] Figure 4 Static contact angle profiles of silica nanoparticle films with or without PFTS coatings with water and oil are shown. The water contact angle (WCA) changes from complete wetting (401) on the silica nanoparticle film deposited by PLD to 155.2 ± 1.8 ° (403) after PFTS modification. The oil (diiodomethane) contact angle changes from complete wetting to 133.6 ± 3.3 ° (references 405 and 407). The sliding behavior of water and diiodomethane droplets of silica nanoparticle films with PFTS coatings was also tested. It was observed that the sliding angle of water was significantly lower (about 4 °), while the sliding angle of diiodomethane was about 23 °. Therefore, the coating is super hydrophobic and highly oleophobic.

[0150] Example 4.3: Surface physical microstructure and chemical structure

[0151] The change of surface properties is caused by the modification of its physical microstructure and surface chemical properties. In this study, SEM and AFM were used to characterize the surface physical structure. XPS was used to detect the surface chemical composition. Figure 5A and Figure 5B SEM and AFM images of the prepared silica nanoparticle films with and without PFTS coating are shown, respectively. The surface morphology of the silica nanoparticles prepared by PLD deposition is well preserved after PFTS coating, as similar nanostructures are observed (compare Figure 5A and Figure 5B ) and surface roughness (listed in Table 3).

[0152] Table 3: Comparison of roughness measurements of nanoparticle films with and without PFTS coating.

[0153]

[0154] As mentioned above, fabricating anti-fingerprint surfaces with high optical transmittance is a great challenge because surface roughness is essential for superamphiphobicity. However, high surface roughness may induce light scattering, leading to transmittance loss and even appearance loss (e.g., the surface may become milky). A new roughness factor R is proposed f , which is used to theoretically predict the anti-fingerprint performance of surface coatings. The roughness factor is defined as the arithmetic mean roughness (R a ) and the maximum height (R v ) ratio, namely R f =R a / R v For surfaces with low average roughness (R a <1μm) surface, relatively deep valleys (higher R v ) is conducive to better hydrophobic and oleophobic properties. For anti-fingerprint surfaces, R f It should be no greater than 0.2451, which provides a standard for the surface structure to enhance anti-fingerprint performance while maintaining high optical transmittance. The surface of the original PC is carefully modified by oxygen plasma treatment and deposition of silica nanoparticles.

[0155] like Fig. 6A and Figure 6B As shown, oxygen plasma treatment significantly increased the surface roughness and produced peaks and valleys. XPS spectra ( Figure 6C ) showed that the large amount of oxygen bonding generated by oxygen plasma also helps to promote the nucleation and growth of oxide nanoparticles. Figure 5A As shown, the silica nanoparticles with an average size of 37.4 ± 10.7 nm form clusters with a size of 188.5 ± 36.5 nm and are evenly distributed on the surface without large aggregates. f Control below the recommended value of 0.2451.

[0156] Regarding surface chemical transformation, XPS spectra such as 7A to 7E shown. Fig. 7A The XPS survey spectra of pristine PC, silica film, and PFTS-coated silica film are shown. After PLD deposition, there is a significant increase in the surface oxygen peak and the presence of a silicon peak (located at 103.4 eV, as shown in Figure 2). Fig.7DThe Si 2p high-resolution spectrum in Figure 1 shows that the silica film has been coated on the PC. It is well known that the surface of silica is hydrophilic in nature due to the presence of silanol (Si-OH) groups. The silanol groups have a strong affinity with water by forming hydrogen bonds, thus forming a hydrophilic nanoparticle film on the surface. The large number of hydroxyl (-OH) groups also provide sites for chemical reactions with PFTS. High-resolution spectrum Figure 7B and Fig. 7E The C1s doublet at 291.1 eV and 293.4 eV and the F1s peak at 688.2 eV shown in the figure are characterized by -CF2 and -CF3 bonds, which clearly indicate that PFTS has been successfully deposited on the silicon dioxide film. The modification of fluorocarbon molecules results in a lower surface energy required for amphiphobicity.

[0157] Example 4.4: Surface transparency, self-cleaning and anti-fingerprint performance

[0158] Fig. 8A The digital image of the prepared transparent PC substrate with PTFS coated silica film is shown, where water droplets and oil droplets are stably staying on the surface. The transmittance measured in the visible wavelength range of 400nm to 700nm clearly shows a slight increase in transmittance (as shown in Figure 2). Figure 8B As shown). The average transmittance between wavelengths of 400nm and 700nm increased from 84.9% to 87.8%. Despite the slight increase in surface roughness, the scattering of light did not increase because the surface features are well below the wavelength of visible light. On the contrary, the transmittance increased with the addition of the silica nanoparticle coating, indicating anti-reflection characteristics. This can be explained by a single-layer anti-reflection film system, in which a coating material with a lower refractive index than the substrate is preferred. In the current study, the silica film used was porous and can be regarded as a composite of silica and air. This composite would result in a much lower refractive index than a dense silica film. Therefore, the prepared silica nanoparticle film exhibits anti-reflection properties.

[0159] Example 4.5: Effect of deposition time on transmittance in the visible light range

[0160] This paper reports the effect of deposition time on light transmittance.

[0161] Fig. 9 The average transmittance measurements in the visible range between 400 nm and 700 nm are shown for each deposition time. The coating with a deposition time of 10 minutes exhibited an average transmittance almost identical to that of the original PC substrate (T for deposition of 10 minutes). ave =84.95%; T of original PC ave =84.91%). The highest average transmittance (88.94%) was observed at a deposition time of 30 minutes. A decreasing trend was observed at longer deposition times (T = 84.91%).ave = 87.8%, T after 90 minutes of deposition ave =85.81%). The increase in transmittance observed at 30 and 60 minutes of deposition can be explained by the anti-reflection features described herein. The decrease in transmittance at longer deposition times is due to light absorption by the thicker film.

[0162] Figure 8C and Fig.8D Demonstrated anti-fingerprint performance. A thumb is placed on the surface for 2 seconds to form a fingerprint. Comparison of digital and microscopic images clearly shows that the fingerprint sticks to the original PC surface but not to the coated PC surface.

[0163] Self-cleaning properties have been used to remove contaminants such as dust, dirt, and grease from solid surfaces. In this study, titanium oxide powder was used as a model contaminant dust particle to investigate the self-cleaning properties of the samples. Fig. 8E As shown, titanium oxide powder is evenly distributed on the inclined PC surface. After a water droplet is dropped, the silica nanoparticle film with PFTS coating shows a strong self-cleaning ability. The water droplet rolls off the superhydrophobic surface and immediately takes the powder along the path. In comparison, the powder remains on the original PC surface.

[0164] Example 4.6: Mechanical strength and durability of PFTS-coated silica coatings

[0165] The main issues in the practical use of such coatings are mechanical toughness and durability. The mechanical robustness of the coatings is analyzed using the US military standard (MIL-C-48497) to measure coating adhesion and abrasion resistance. This specification is most suitable for optical coatings. Due to the superhydrophobic nature of the coating, the tape exhibits very weak or no adhesion to the substrate. Therefore, a cross-hatch test according to the ASTM standard was performed instead to evaluate the adhesion quality. Fig. 10A No delamination of the coating was shown along the cross-hatched lines, indicating strong adhesion of the coating to the substrate.

[0166] The coating durability was further evaluated by rubbing the surface with a cheesecloth pad as described previously. The surface topography was altered by the applied friction ( Fig. 10B ).like Fig. 10C As shown in Figure 2, the surface roughness is reduced due to the damage of the peaks and valleys by the shear forces applied during the wear process. As a result, the surface wettability is affected, showing a decrease in WCA to 129.2 ± 4.4° and OCA (diiodomethane) to 98 ± 2.6°, as shown in Figure 2. Fig. 10D As shown. Fig.10E As shown in the transmittance measurements in , although a slight decrease in average transmittance was observed, a higher average transmittance than pristine PC was still achieved. Despite the decrease in water and oil contact angles, the anti-fingerprint performance was still maintained, as shown in the microscopic images Fig.10F As shown, fingerprints are greatly reduced compared to the original PC substrate.

[0167] Example 5: Conclusion

[0168] As disclosed herein, a simple method for preparing a highly transparent, amphiphobic coating with self-cleaning and anti-fingerprint properties has been developed. In an exemplary embodiment, a nanoporous silica film is deposited at room temperature by pulsed laser deposition, resulting in a desired surface morphology. XPS analysis showed the presence of CF bonds, confirming the functionalization of silica nanoparticles by low surface energy PFTS molecules. Treatment of the PC substrate with oxygen plasma not only helps promote the nucleation and growth of silica nanoparticles into the desired morphology, but also enhances the adhesion strength between the coating and the substrate. The combination of enhanced transparency, superhydrophobic / oleophobic properties, excellent mechanical durability and adhesion makes this coating have great potential in optical and display applications that are sensitive to pollution.

[0169] The term "comprising" means including, but not limited to, the contents following the word "comprising". Thus, the use of the term "comprising" indicates that the listed elements are required or mandatory, but other elements are optional and may or may not be present.

[0170] The meaning of “consisting of” includes and is limited to the contents in “consisting of.” Thus, the phrase “consisting of” means that the listed elements are required or mandatory, and no other elements may be present.

[0171] The invention exemplarily described herein can be appropriately practiced in the absence of any element or elements, limitations or limitations not specifically disclosed herein. Therefore, for example, terms such as "including", "comprising", "containing" and the like should be understood broadly without limitation. In addition, the terms and expressions used herein are used as descriptive terms rather than restrictive terms, and the use of these terms and expressions is not intended to exclude any equivalents of the features shown and described or parts thereof, but it should be recognized that various modifications can be made within the scope of the invention claimed. Therefore, it should be understood that although the present invention has been specifically disclosed by preferred embodiments and optional features, those skilled in the art may modify and change the invention embodied in the contents disclosed herein, and such modifications and changes are considered to be within the scope of the present invention.

[0172] With respect to given values ​​(eg, temperature and time period), "about" is intended to include values ​​within 10% of the specified value.

[0173] The invention has been described broadly and generically herein. Each of the narrower species and sub-generic groupings falling within the generic disclosure also form part of the invention. This includes the generic description of the invention, but with any subject matter proviso or negative limitation deleted from that genus, regardless of whether the deleted material is specifically recited herein.

[0174] Other embodiments are within the scope of the following claims and non-limiting examples. In addition, where features or aspects of the invention are described in terms of Markush groups, those skilled in the art will recognize that the invention is also thereby described in terms of any individual member or subgroup of members of the Markush group.

Claims

1. An amphiphobic coating, comprising: a polymer substrate having an oxygen plasma treated surface; a silicon dioxide layer comprising silicon dioxide nanoparticles disposed directly on the oxygen plasma treated surface; as well as A fluoroalkylsilane layer is disposed directly on the silicon dioxide layer.

2. The amphiphobic coating of claim 1, wherein the material of the polymer substrate is selected from the group consisting of polycarbonate, poly(methyl methacrylate), polyester, polyethylene terephthalate, polyimide, polytetrafluoroethylene, polypropylene, polyolefin, nylon, silicone, polyvinyl chloride, polystyrene and polyphenylene sulfide.

3. An amphiphobic coating according to claim 1 or 2, wherein the silicon dioxide layer is nanoporous.

4. The amphiphobic coating according to any one of claims 1 to 3, wherein the average size of the silica nanoparticles is in the range of 25 nm to 50 nm.

5. The amphiphobic coating according to any one of claims 1 to 4, wherein the silica nanoparticles form clusters having a size ranging from 150 nm to 250 nm.

6. The amphiphobic coating according to any one of claims 1 to 5, wherein the thickness of the silicon dioxide layer is in the range of 10 nm to 500 nm. 7 . The amphiphobic coating according to claim 1 , wherein the fluoroalkylsilane layer is a self-assembled layer.

8. The amphiphobic coating according to any one of claims 1 to 7, wherein the surface of the silicon dioxide layer comprises hydroxyl groups. 9 . The amphiphobic coating according to claim 8 , wherein the fluoroalkylsilane layer directly disposed on the silicon dioxide layer is covalently bonded to the silicon dioxide layer via the hydroxyl group.

10. The amphiphobic coating according to any one of claims 1 to 9, wherein the fluoroalkylsilane layer is formed of a fluoroalkylsilane selected from trichloro(1H,1H,2H,2H-perfluorooctyl)silane, 1H,1H,2H,2H-perfluorodecyltriethoxysilane, and a combination thereof.

11. The amphiphobic coating according to any one of claims 1 to 10, wherein the roughness factor R of the amphiphobic coating is f 0.2451 or less.

12. The amphiphobic coating according to any one of claims 1 to 11, wherein the amphiphobic coating exhibits a transmittance of at least 84% in the wavelength range of 400 nm to 700 nm.

13. The amphiphobic coating according to any one of claims 1 to 12, wherein the contact angle of water on the amphiphobic coating is greater than 150°.

14. The amphiphobic coating according to any one of claims 1 to 13, wherein the contact angle of diiodomethane on the amphiphobic coating is greater than 130°.

15. A method for preparing an amphiphobic coating, the method comprising: providing a polymer substrate having an oxygen plasma treated surface; directly depositing silicon dioxide on the oxygen plasma treated surface by pulsed laser deposition to form a silicon dioxide layer containing silicon dioxide nanoparticles; and A fluoroalkylsilane is deposited directly on the silicon dioxide layer to form a fluoroalkylsilane layer on the silicon dioxide layer.

16. The method according to claim 15, wherein the fluoroalkylsilane is selected from trichloro(1H,1H,2H,2H-perfluorooctyl)silane, 1H,1H,2H,2H-perfluorodecyltriethoxysilane, and combinations thereof.

17. The method of claim 15 or 16, wherein depositing the fluoroalkylsilane directly on the silicon dioxide layer comprises contacting the silicon dioxide layer with a solution comprising the fluoroalkylsilane and a liquid reagent.

18. The method of claim 17, wherein the liquid reagent is selected from the group consisting of hexane and methanol.

19. The method according to claim 17 or 18, wherein the concentration of the fluoroalkylsilane in the solution is in the range of 0.05 vol% to 0.15 vol%.

20. The method of any one of claims 17 to 19, wherein the silicon dioxide layer is contacted with the solution for a period of time in the range of 5 minutes to 20 minutes.

21. The method of any one of claims 17 to 20, wherein depositing the fluoroalkylsilane directly on the silicon dioxide layer further comprises drying the silicon dioxide layer after contacting the silicon dioxide layer with the solution.

22. The method of claim 21, wherein the drying is performed for a period of time ranging from 1 hour to 3 hours.

23. The method according to claim 21 or 22, wherein the drying is carried out at a temperature in the range of 70°C to 90°C.

24. The method of any one of claims 15 to 22, wherein the method is performed without heating.

25. An amphiphobic coating prepared according to the method of any one of claims 15 to 24.

26. Use of the amphiphobic coating according to any one of claims 1 to 14, or the amphiphobic coating prepared by the method according to any one of claims 15 to 24, in an anti-reflective coating, an anti-fingerprint coating, an anti-fouling coating, a self-cleaning surface, a surface primer layer, an optical element, a sensor, a lens, a goggles, a mirror, a windshield, a mask, a display, a window or a cooker cover.

27. An article comprising the amphiphobic coating according to any one of claims 1 to 14, or the amphiphobic coating prepared by the method according to any one of claims 15 to 24, wherein the article is an optical element, a sensor, a lens, a goggles, a mirror, a windshield, a mask, a display, a window or a cooker cover.

Citation Information

Patent Citations

  • Amphiphobic surface with layered structure and manufacturing method and application thereof

    CN114555245A

  • Super non-wetting, Anti-fingerprinting coatings for glass

    US20100304086A1

  • Manufacture of hydrophobic surfaces

    US20140147631A1

  • Water and oil repelling film having surface irregularities and method of manufacturing the same

    US5324566A

  • Improving the adhesion of hydrophobic coatings on eyeglass lenses

    WO2006056274A1